A water hyacinth-derived N and P-rich biomass hierarchical charcoal and its preparation method and application
N- and P-rich biomass hierarchical porous carbon was prepared through water hyacinth-derived co-hydrothermal carbonization and oxygen-limited pyrolysis methods, which solved the problem of insufficient performance of activated carbon in VOCs adsorption and achieved efficient VOCs adsorption effect, especially in It exhibits excellent performance in toluene adsorption.
Patent Information
- Application Number
- CN202311009859.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-08-11
AI Technical Summary
Existing activated carbon has poor performance in the adsorption of volatile organic compounds (VOCs), and its thermal stability and preparation cost are high, making it unable to meet the needs of practical applications.
Using water hyacinth as a precursor, N- and P-rich biomass hierarchical porous carbon was prepared through co-hydrothermal carbonization and oxygen-limited pyrolysis methods to improve its surface polarity and pore structure, increase specific surface area and pore volume, and improve adsorption. performance.
The prepared water hyacinth-derived N- and P-rich biomass hierarchical porous carbon showed excellent adsorption performance, with an adsorption capacity of toluene reaching 624.7mg/g. It has high thermal stability and large pore volume, significantly increasing VOCs. adsorption efficiency.
Smart Images

Figure CN117105223B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmental protection and environmental pollution control, and in particular to a water hyacinth-derived N and P-rich biomass multi-level porous carbon and a preparation method and application thereof. Background Art
[0002] Volatile organic compounds (VOCs) are important precursors to complex atmospheric pollution such as urban haze and photochemical pollution. They have a significant impact on human health and the ecological environment, and have attracted widespread attention from the government and the public. Therefore, VOCs control is the key to winning the battle to protect blue skies. Common methods for VOCs control include condensation recovery, absorption, adsorption, direct combustion, catalytic combustion, and low-temperature plasma purification. Among them, the adsorption method has been widely used in VOCs waste gas treatment due to its low cost, simple operation, and no secondary pollutants. The core of adsorption technology is adsorbent.
[0003] At present, activated carbon is the most widely used VOCs adsorption material. Taking toluene as an example, the adsorption performance of conventional activated carbon for VOCs is about 50-200 mg / g, which is poor. In addition, activated carbon still faces some serious defects and deficiencies in practical applications, including poor thermal stability, large mass transfer resistance, and relatively high preparation cost, which have gradually failed to meet the needs of practical applications. In comparison, biomass hierarchical porous carbon has good economic benefits due to its large specific surface area, developed pore structure, low cost and easy availability, and directional design and preparation. At present, the application of water hyacinth-derived biomass hierarchical porous carbon in VOCs adsorbents has not been reported. Summary of the invention
[0004] In view of the shortcomings of the prior art, the first object of the present invention is to provide a method for preparing N and P-rich biomass multi-porous carbon derived from water hyacinth.
[0005] The second object of the present invention is to provide water hyacinth-derived N and P-rich biomass hierarchical porous carbon prepared by the above method.
[0006] The third object of the present invention is to provide the use of the above-mentioned water hyacinth-derived N and P-rich biomass multi-porous carbon in the adsorption of volatile organic compounds.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The first object of the present application is to provide a method for preparing N and P-rich biomass hierarchical charcoal derived from water hyacinth, comprising the following steps:
[0009] (1) Pretreatment of raw water hyacinth: washing the collected water hyacinth, drying it in the sun to remove moisture and crushing it into powder, and then drying it in an oven to obtain pretreated water hyacinth powder;
[0010] (2) Co-hydrothermal carbonization: KOH, water hyacinth powder and water are mixed evenly and placed in a hydrothermal reactor for hydrothermal carbonization reaction. After the hydrothermal reaction is completed, the mixture is filtered out and placed in an oven for drying to obtain hydrothermally carbonized water hyacinth hydrogen carbon;
[0011] (3) Oxygen-limited pyrolysis: calcine the water hyacinth hydrogen charcoal at 500°C to 900°C for 1 to 5 hours under a protective atmosphere, wash it to neutrality after cooling, and dry it to obtain the water hyacinth derived N and P-rich biomass hierarchical charcoal.
[0012] The present invention utilizes the characteristics of natural source N and P of water hyacinth to improve the non-polar characteristics of the porous carbon surface, and then through co-hydrothermal carbonization, the activator KOH is better dispersed. In addition, the co-hydrothermal carbonization can also retain N and P on the porous carbon, thereby improving the adsorption of VOCs molecules by the adsorbent. The subsequent KOH activation greatly improves the specific surface area and pore volume of the adsorbent.
[0013] Furthermore, in step (1), the oven temperature is 60 to 120° C., and the drying time is 12 to 72 hours;
[0014] Preferably, the oven temperature is 105° C. and the drying time is 24 hours.
[0015] Furthermore, in step (2), the weight ratio of the water hyacinth powder to deionized water is 1:(20-80);
[0016] Preferably, the weight ratio of water hyacinth powder to deionized water is 1:30.
[0017] Furthermore, the specification of the hydrothermal reaction kettle in step (2) is 100 ml, the hydrothermal temperature is 100-260° C., the hydrothermal time is 1-20 hours, and the mass ratio of KOH to water hyacinth powder is 1:(1-10).
[0018] Preferably, the hydrothermal temperature is 230° C., the hydrothermal time is 10 hours, and the mass ratio of KOH to water hyacinth powder is 1:4.
[0019] Furthermore, the drying in steps (2) and (3) is carried out in a drying oven, the drying temperature is 60 to 120° C., and the drying time is 12 to 72 hours;
[0020] Preferably, the drying temperature is 105° C. and the drying time is 24 hours.
[0021] Furthermore, the heating rate in step (3) is 1 to 20°C / min;
[0022] Preferably, the calcination temperature is 800° C., the heating rate is 10° C. / min, and the holding time is 90 min.
[0023] Furthermore, the concentration of HCl in step (3) is 0.1 to 2.0 mol / L;
[0024] Preferably, the HCl concentration is 0.5 mol / L.
[0025] The second objective of the present application is to provide a water hyacinth-derived N and P-rich biomass multi-porous carbon prepared according to the above method.
[0026] The third objective of the present application is to provide the role of water hyacinth-derived N and P-rich biomass multi-porous carbon in the adsorption of volatile organic compounds.
[0027] Furthermore, the volatile organic compound is toluene.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The present invention uses water hyacinth as a precursor raw material. Water hyacinth has abundant natural nutrient elements N and P, which significantly improves the surface polarity and loose porous structure. The preparation method is introduced by co-hydrothermal carbonization + oxygen-limited pyrolysis. Co-hydrothermal carbonization is a mild and simple method. While fixing N and P in the multi-level porous carbon, it is conducive to the high dispersion of the activator KOH, which helps to improve the surface polarity of the multi-level porous carbon; oxygen-limited pyrolysis significantly increases the specific surface area and pore volume of the multi-level porous carbon, and improves the adsorption performance.
[0030] (2) The present invention uses water hyacinth as a precursor raw material, thereby solving the problem of the difficulty in disposing of solid waste of water hyacinth.
[0031] (3) The water hyacinth-derived N and P-rich biomass multi-porous carbon provided in the present application has the characteristics of well-developed pores, large specific surface area, strong adsorption performance, higher thermal stability, large pore volume, pore structure with a specific micro / mesopore ratio and abundant surface functional groups. In the dynamic adsorption experiment with toluene as a typical VOC, it showed excellent adsorption performance (toluene: 624.7 mg / g). BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The scanning electron microscope image and element surface scanning result of the water hyacinth-derived N and P-rich biomass multi-level porous carbon of the present invention;
[0033] Figure 2 The Fourier transform infrared spectrum of the water hyacinth-derived N and P-rich biomass hierarchical porous carbon of the present invention;
[0034] Figure 3This is a pore size distribution diagram of the water hyacinth-derived N and P-rich biomass multi-porous carbon of the present invention.
[0035] Figure 4 The adsorption penetration curve of toluene by the water hyacinth-derived N and P-rich biomass hierarchical pore carbon of the present invention;
[0036] The present invention is further described below in conjunction with the accompanying drawings and embodiments. DETAILED DESCRIPTION
[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The water hyacinth variety described in the present application is Eichhornia crassipes of the genus Eichhornia crassipes of the family Pontederiaceae. The parts collected in the experiment were the stems and leaves of the water hyacinth, and the roots were not collected.
[0039] The methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified.
[0040] Example 1
[0041] (1) Pretreatment of raw water hyacinth: The collected water hyacinth was washed and dried in the sun to remove moisture and crushed into powder, and then placed in an oven and dried at 105° C. for 24 h to obtain pretreated water hyacinth powder;
[0042] (2) Preparation of co-hydrothermal carbonization hydrogen carbon: 2 g of dried water hyacinth powder and 0.25 g of KOH were added to 60 ml of deionized water, mixed evenly and placed in a 100 ml hydrothermal reactor, hydrothermally carbonized at 230 °C for 10 h, cooled naturally to room temperature and then taken out, the obtained mixture was filtered and then placed in an oven at 105 °C for 24 h to obtain water hyacinth carbonization hydrogen carbon; the mass ratio of the raw water hyacinth to KOH was 8:1.
[0043] (3) Oxygen-limited pyrolysis: Weigh 1g of the dried water hyacinth hydrogen carbon and place it evenly in a quartz ark, then roast it at 800℃ in a tube furnace under N2 atmosphere (heating rate 10℃ / min, holding time 90min), cool it naturally to room temperature, wash it repeatedly with 0.5mol / L HCl solution and deionized water until the filtrate is neutral, and dry it in an oven to obtain 8:1 water hyacinth derived N, P-rich biomass multi-level porous carbon. (Recorded as HWK-H-8, where the mass ratio of water hyacinth hydrogen carbon and KOH is 8:1, and the roasting temperature is 800℃)
[0044] Example 2
[0045] (1) Pretreatment of raw water hyacinth: The collected water hyacinth was washed and dried in the sun to remove moisture and crushed into powder, and then placed in an oven and dried at 105° C. for 24 h to obtain pretreated water hyacinth powder;
[0046] (2) Preparation of co-hydrothermal carbonization: 2 g of dried water hyacinth powder and 0.5 g of KOH were added to 60 ml of deionized water, mixed evenly and placed in a 100 ml hydrothermal reactor, hydrothermally carbonized at 230 °C for 10 h, cooled naturally to room temperature and then taken out, the obtained mixture was filtered and then placed in an oven at 105 °C for 24 h to obtain water hyacinth carbonization after co-hydrothermal carbonization; the mass ratio of the raw water hyacinth to KOH was 4:1.
[0047] (3) Oxygen-limited pyrolysis: Weigh 1.5 g of the dried water hyacinth hydrogen carbon and place it evenly in a quartz ark, then roast it at 800 °C in a tube furnace under N2 atmosphere (heating rate 10 °C / min, holding time 90 min), cool it naturally to room temperature, wash it repeatedly with 0.5 mol / L HCl solution and deionized water until the filtrate is neutral, and dry it in an oven to obtain a 4:1 water hyacinth-derived N and P-rich biomass multi-level porous carbon. (Recorded as HWK-H, where the mass ratio of water hyacinth hydrogen carbon and KOH is 4:1, and the roasting temperature is 800 °C)
[0048] Example 3
[0049] (1) Pretreatment of raw water hyacinth: The collected water hyacinth was washed and dried in the sun to remove moisture and crushed into powder, and then placed in an oven and dried at 105° C. for 24 h to obtain pretreated water hyacinth powder;
[0050] (2) Preparation of co-hydrothermal carbonization: 2 g of dried water hyacinth powder and 1 g of KOH were added to 60 ml of deionized water, mixed evenly and placed in a 100 ml hydrothermal reactor for hydrothermal carbonization at 230 °C for 10 h. The mixture was naturally cooled to room temperature and then taken out. The obtained mixture was filtered and then placed in an oven at 105 °C for drying for 24 h to obtain water hyacinth carbonization after co-hydrothermal carbonization. The mass ratio of the raw water hyacinth to KOH was 2:1.
[0051] (3) Oxygen-limited pyrolysis: Weigh 2 g of the dried water hyacinth hydrogen carbon and place it evenly in a quartz ark, then roast it at 800°C in a tube furnace under N2 atmosphere (heating rate 10°C / min, holding time 90 min), cool it naturally to room temperature, wash it repeatedly with 0.5 mol / L HCl solution and deionized water until the filtrate is neutral, and dry it in an oven to obtain 2:1 water hyacinth-derived N and P-rich biomass multi-level porous carbon. (Recorded as HWK-H-2, where the mass ratio of water hyacinth hydrogen carbon and KOH is 2:1, and the roasting temperature is 800°C)
[0052] Comparative Example 1
[0053] (1) Pretreatment of raw water hyacinth: The collected water hyacinth was washed and dried in the sun to remove moisture and crushed into powder, and then placed in an oven and dried at 105° C. for 24 h to obtain pretreated water hyacinth powder;
[0054] (2) Direct pyrolysis: Weigh 2g of dried water hyacinth powder and 0.5g of KOH, grind them evenly in an agate mortar, place them in a quartz ark, and roast them at 800℃ in a tube furnace under N2 atmosphere (heating rate 10℃ / min, holding time 90min), cool them naturally to room temperature, wash them repeatedly with 0.5mol / L HCl solution and deionized water until the filtrate is neutral, and dry them in an oven to obtain multi-level porous carbon from water hyacinth biomass directly pyrolyzed (denoted as WK-G, where the mass ratio of water hyacinth powder to KOH is 4:1, and the roasting temperature is 800℃)
[0055] Comparative Example 2
[0056] (1) Pretreatment of raw water hyacinth: The collected water hyacinth was washed and dried in the sun to remove moisture and crushed into powder, and then placed in an oven and dried at 105° C. for 24 h to obtain pretreated water hyacinth powder;
[0057] (2) Hydrothermal carbonization: 2 g of dried water hyacinth powder was added to 60 ml of deionized water, mixed evenly, and placed in a 100 ml hydrothermal reactor for hydrothermal carbonization at 230°C for 10 h. The mixture was naturally cooled to room temperature and then taken out. The obtained mixture was filtered and then placed in an oven at 105°C for drying for 24 h to obtain water hyacinth hydrogen carbon after hydrothermal carbonization. Only the raw material water hyacinth was added, and no activator KOH was added.
[0058] (3) Oxygen-limited pyrolysis: Weigh 1 g of the dried water hyacinth hydrogen charcoal and place it evenly in a quartz ark, then roast it at 800°C in a tube furnace under N2 atmosphere (heating rate 10°C / min, holding time 90 min), cool it naturally to room temperature, wash it repeatedly with 0.5 mol / L HCl solution and deionized water until the filtrate is neutral, and dry it in an oven to obtain water hyacinth-derived N and P-rich biomass hierarchical charcoal (denoted as HW, where no KOH is added and the roasting temperature is 800°C)
[0059] Test example
[0060] The pore characteristics of the porous carbon obtained in Examples 1-3 and Comparative Examples 1-2 were tested. The pore structure characteristics of the materials were determined using the N2 adsorption isotherm at 77K (ASAP2020, Micromeritic). The pore characteristics of the porous carbon obtained are shown in Table 1 below:
[0061] Table 1: Pore characteristics of water hyacinth derived N, P-rich biomass hierarchical pore carbons prepared in Examples 1-3 and Comparative Examples 1-2
[0062]
[0063] It can be seen from Table 1 that the water hyacinth-derived N and P-rich biomass multi-level porous carbon HWK-H of Example 2 of the present invention has the highest specific surface area of 2199.9 m 2 / g, and the mesopore volume is 0.70cm 3 / g, micropore volume is 0.54cm 3 / g.
[0064] The morphology of the porous carbon HWK-H obtained in Example 2 was collected using a S-4800 field emission scanning electron microscope (SEM, Hitachi, Japan) at an accelerating voltage of 15 kV, and the 400 to 4000 cm-1 infrared spectrometer (Nicolet iS50, ThermoFisher, USA) was used to obtain the -1 Fourier transform infrared spectroscopy.
[0065] The scanning electron microscope image and element surface scanning results of the water hyacinth-derived N and P-rich biomass multi-porous carbon obtained in Example 2 are as follows: Figure 1 As shown, from Figure 1 It can be seen that the water hyacinth-derived N and P-rich biomass hierarchical pore carbon of the present invention exhibits obvious hierarchical pores and porous honeycomb pore structures. The Fourier transform infrared spectrum of the water hyacinth-derived N and P-rich biomass hierarchical pore carbon is shown in FIG. Figure 2As shown in the figure, it can be seen that the water hyacinth-derived N and P-rich biomass hierarchical carbon of the present invention presents abundant surface functional groups. The pore size distribution diagram of the water hyacinth-derived N and P-rich biomass hierarchical carbon is shown in the figure. Figure 3 As shown in the figure, it can be seen that the water hyacinth-derived N and P-rich biomass multi-level porous carbon of the present invention has a rich pore structure, and the pore size distribution is in the range of 0.5-10nm.
[0066] The water hyacinth-derived N and P-rich biomass multi-level porous carbon adsorbent prepared in Examples 1-3 and Comparative Examples 1-2 was placed in a quartz tube fixed adsorption bed for activity evaluation. The evaluation parameters were as follows: 0.05 g of the adsorbent was weighed and placed in a quartz tube of the adsorption bed. Toluene gas with a flow rate of 100 ml / min and an initial concentration of 300 ppm was introduced into the quartz tube. The concentration and adsorption time of the tail gas were measured by a GC (GC-9790, Fuli) gas chromatograph to evaluate the adsorption capacity of the adsorbent for toluene. The test results are shown in Table 2:
[0067] Table 2: Adsorption capacity of water hyacinth-derived N and P-rich biomass hierarchical charcoal prepared in Examples 1-3 and Comparative Examples 1-2
[0068]
[0069] As can be seen from Table 2, the porous carbon prepared in Examples 1-3 has a good VOCs adsorption capacity within 60-420 min, and under the same preparation conditions, the VOCs adsorption capacity of HWK-H prepared in Example 2 within 420 min is about 40-70% higher than that of Examples 1 and 3. It should be that in the process of co-hydrothermal carbonization, too much activator KOH may cause too many carbon atoms and functional groups to escape, and too little will make it difficult to achieve efficient activation, resulting in a decrease in adsorption capacity. In particular, the effect of the porous carbon HWK-H prepared in Example 2 is much better than the adsorption capacity of Comparative Examples 1 and 2, and plays a key role in improving the adsorption performance of VOCs. It shows that the VOCs adsorption performance of the porous carbon obtained by the preparation method of co-hydrothermal carbonization coupled with oxygen-limited pyrolysis is more superior.
[0070] The adsorption penetration curves and adsorption amounts of toluene by the water hyacinth-derived N and P-rich biomass hierarchical pore carbons of Examples 1-3 and Comparative Examples 1-2 are shown in Table 1. Figure 4 As shown and Table 3.
[0071] Table 3: Penetration adsorption and saturation adsorption of water hyacinth-derived N and P-rich biomass multi-level porous carbon prepared in Examples 1-3 and Comparative Examples 1-2
[0072] sample Penetration adsorption capacity (mg / g) Saturated adsorption capacity (mg / g) HWK-H-8 313.8 426.9 HWK-H 425.2 624.7 HWK-H-2 208.4 385.1 WK-G 224.1 404.2 HW 84.1 209.1
[0073] Depend on Figure 4It can be seen that the penetration time (time required when the outlet concentration / inlet concentration reaches 5%) and saturation time (time required when the outlet concentration / inlet concentration = 100%) of the water hyacinth-derived N and P-rich biomass multi-porous carbon HWK-H in Example 2 for toluene are both improved compared to Examples 1 and 3. As shown in Table 3, the penetration adsorption amount and saturation adsorption amount of HWK-H in Example 2 are the largest, which are 425.2 mg / g and 624.7 mg / g, respectively. The penetration adsorption amount and saturation adsorption amount of Comparative Examples 1 and 2 are 224.1 mg / g, 404.2 mg / g and 84.1 mg / g, 209.1 mg / g, respectively. The saturation adsorption amount of HWK-H in Example 2 for toluene is increased by 1-3 times compared to Comparative Examples 1 and 2.
[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application and not to limit it. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present application can still be modified or some technical features can be replaced by equivalents, which should all be included in the scope of the technical solution requested for protection in this application.
Claims
1. Application of water hyacinth-derived N and P-rich biomass hierarchical carbon in the adsorption of volatile organic compounds, characterized in that: The volatile organic compound is toluene, and its preparation method comprises the following steps: (1) Pretreatment of raw water hyacinth: washing the collected water hyacinth, drying it in the sun to remove moisture, crushing it into powder, and then drying it in an oven to obtain pretreated water hyacinth powder; (2) Co-hydrothermal carbonization: KOH, water hyacinth powder and water are mixed evenly and placed in a hydrothermal reactor for hydrothermal carbonization reaction. After the hydrothermal reaction is completed, the mixture is filtered out and placed in an oven for drying to obtain hydrothermally carbonized water hyacinth hydrogen carbon; the hydrothermal temperature is 230 °C, the hydrothermal time is 10 hours, and the mass ratio of KOH to water hyacinth is 1:4; (3) Oxygen-limited pyrolysis: The water hyacinth hydrogen charcoal was calcined at 800 °C for 90 min under a protective atmosphere, washed to neutrality after cooling, and dried to obtain water hyacinth-derived N and P-rich biomass hierarchical charcoal.
2. The use of a water hyacinth-derived N and P-rich biomass multi-porous carbon in the adsorption of volatile organic compounds according to claim 1, characterized in that: The oven temperature in step (1) is 60 to 120° C., and the drying time is 12 to 72 hours.
3. The use of a water hyacinth-derived N and P-rich biomass multi-porous carbon in the adsorption of volatile organic compounds according to claim 1, characterized in that: The weight ratio of the water hyacinth powder to deionized water in step (2) is 1:(20-80).
4. The use of a water hyacinth-derived N and P-rich biomass multi-porous carbon in the adsorption of volatile organic compounds according to claim 1, characterized in that: The specification of the hydrothermal reactor in step (2) is 100 ml.
5. The use of a water hyacinth-derived N and P-rich biomass multi-porous carbon in adsorbing volatile organic compounds according to claim 1, characterized in that: The drying in steps (2) and (3) is carried out in a drying oven at a drying temperature of 60 to 120° C. and a drying time of 12 to 72 hours.
6. The use of a water hyacinth-derived N and P-rich biomass multi-porous carbon in adsorbing volatile organic compounds according to claim 1, characterized in that: The heating rate in step (3) is 1 to 20°C / min.