Treatment of alkaline copper etching waste liquid by copper leaching method
The alkaline copper corrosion waste liquid is stirred and filtered in the copper depositing reaction tank by breaking the copper depositing method to generate alkaline salt precipitation that is insoluble in water, which solves the problem of incomplete treatment of alkaline copper corrosion waste liquid in the prior art. It realizes efficient waste liquid recycling and environmentally friendly utilization.
Patent Information
- Application Number
- CN202311071426.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-08-23
AI Technical Summary
When processing alkaline copper corrosion waste liquid, the prior art cannot fully generate water-insoluble alkali salt precipitation, resulting in the failure to completely solve the environmental protection problems and the cost of increasing copper is high.
By using the method of breaking and copper depositing, the alkaline copper corrosion waste liquid is stirred in the copper depositing reaction tank, the cracking agent and alkali copper salt seed crystal are added, and the primary reaction product is generated and filtered and rinsed to obtain the alkaline salt precipitation. And the pH value and stirring conditions are controlled to promote the filling and analysis of basic salts.
The recycling efficiency and recycling rate of alkaline copper waste liquid is improved, the waste liquid is converted into environmentally friendly pure substances, the recycling of waste is realized, and environmental pollution and recycling costs are reduced.
Smart Images

Figure CN117105376B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of etching waste liquid treatment, and in particular to a process for treating alkaline copper etching waste liquid by a chelation breaking copper precipitation method. Background Art
[0002] In recent years, the electronics industry has developed rapidly. As a basic link in the electronics industry, the printed circuit board industry has also maintained a relatively fast growth rate in recent years. When making printed circuit boards, etching liquid is needed to corrode and remove the remaining copper foil outside the circuit to form the circuit, and a large amount of copper-containing etching waste liquid is also generated. Direct discharge of copper-containing waste liquid will cause serious environmental pollution. It is transferred to the human body through plants and water, and excessive copper will cause enzyme poisoning in the human body. Therefore, the copper-containing etching waste liquid in the printed circuit board industry needs to be cleaned up in a timely and effective manner.
[0003] In the prior art, when alkaline copper etching waste liquid is decomposed to generate water-insoluble basic salt precipitation, the basic salt precipitation cannot be fully generated and precipitated, and there are problems such as long process method and high copper extraction cost, and the environmental protection problem cannot be completely solved. Summary of the invention
[0004] Based on this, it is necessary to provide a process for treating alkaline copper etching waste liquid by a chelation breaking copper precipitation method.
[0005] The technical solution of the present invention to solve the above technical problems is as follows: A process for treating alkaline copper etching waste liquid by a chelation breaking copper precipitation method comprises the following steps:
[0006] Adding alkaline copper etching waste liquid into the copper precipitation reaction tank, and stirring the alkaline copper etching waste liquid;
[0007] Adding a complex-breaking agent to the copper precipitation reaction tank, and then adding basic copper salt seed crystals to react to obtain a primary reaction product;
[0008] filtering the primary reaction product to obtain a basic salt precipitate and an ammonium chloride mother liquor;
[0009] The basic salt precipitate is stirred, rinsed, dehydrated and dried to obtain the basic salt.
[0010] In one embodiment, the complex breaking agent is one of hydrochloric acid, carbonic acid and sulfuric acid.
[0011] In one embodiment, the basic copper salt seed crystal is one of basic copper chloride, basic copper carbonate and basic copper sulfate.
[0012] In one embodiment, when a complex breaking agent is added to the copper precipitation reaction tank and then basic copper salt seed crystals are added for reaction, the pH value of the alkaline copper etching waste liquid is controlled to be 4-5.5.
[0013] In one embodiment, the process for treating alkaline copper etching waste liquid by the chelation breaking copper precipitation method also includes: adding the ammonium chloride mother liquor into a regeneration mixing tank, taking samples to test the chloride ion content while stirring, and introducing ammonia gas after balance to obtain an alkaline etching solution.
[0014] In one embodiment, when sampling and testing the chloride ion content, the chloride ion content is controlled to be 165-175 g / L.
[0015] In one embodiment, when ammonia gas is introduced into the reaction after the equilibrium, the reaction endpoint is controlled so that the ammonia concentration reaches 5.1-5.3 mol / L and the pH is 8.5-9.5.
[0016] In one embodiment, the copper plating reaction tank includes: a reaction tank body, a stirring paddle and a motor, a stirring chamber is opened in the reaction tank body, the stirring paddle is rotatably arranged in the stirring chamber, the motor is arranged on the first side of the reaction tank body, and the motor is drivingly connected to the stirring paddle, and a plurality of guide plates are obliquely arranged on the side wall of the stirring chamber, the first side of each of the guide plates is connected to the side wall of the stirring chamber, and the second side of each of the guide plates faces the central axis of the stirring chamber.
[0017] In one embodiment, an annular air pipe is disposed around the side wall of the stirring chamber, the annular air pipe is spaced apart from the guide plate in the upper and lower directions, and a plurality of aeration holes are opened on the annular air pipe, each of the aeration holes faces the bottom of the stirring chamber.
[0018] In one embodiment, the reaction tank is a tank with a flat top and a round bottom.
[0019] The beneficial effects of the present invention are as follows: the present invention provides a process for treating alkaline copper etching waste liquid by a chelation breaking copper precipitation method, wherein the alkaline copper etching waste liquid is added into a copper precipitation reaction tank, a chelation breaking agent is added while stirring, and then basic copper salt seeds are added to react to obtain a primary reaction product, and then the primary reaction product is filtered to obtain a basic salt precipitate and an ammonium chloride mother liquor, and the obtained basic salt precipitate is stirred, rinsed, dehydrated and dried to obtain a basic salt, so that when the alkaline copper etching waste liquid is chelated to generate a water-insoluble basic salt precipitate, under sufficient stirring of the copper precipitation reaction tank, the generated basic salt molecules continuously collide with the basic copper salt seeds to precipitate, can be well attached to the basic copper salt seeds, can promote the basic salt molecules to be fully precipitated from the reaction solution, can greatly improve the recovery efficiency and recovery rate of the alkaline copper etching waste liquid, so that the alkaline copper etching waste liquid is fully converted into an environmentally friendly and pure substance, and the recycling and utilization of waste is realized, which is green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 The schematic diagram of the process of treating alkaline copper etching waste liquid by the copper precipitation method of the present invention is shown in FIG.
[0022] Figure 2 It is a structural schematic diagram of the copper deposition reaction tank of the present invention;
[0023] Figure 3 It is a schematic cross-sectional structure diagram of the copper deposition reaction tank of the present invention;
[0024] Figure 4 It is a schematic structural diagram of a copper deposition reaction tank in one direction of the present invention.
[0025] In the attached drawings, 10, copper deposition reaction tank; 100, reaction tank body; 200, stirring paddle; 300, motor; 400, guide plate; 500, annular air pipe; 510, aeration hole. DETAILED DESCRIPTION
[0026] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0027] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0029] In one embodiment, Figure 1 As shown, a process for treating alkaline copper etching waste liquid by a chelation-breaking copper precipitation method comprises the following steps:
[0030] Step 110, adding alkaline copper etching waste liquid into the copper precipitation reaction tank, and stirring the alkaline copper etching waste liquid.
[0031] In this embodiment, the main components of the alkaline copper etching waste liquid are Cu(NH3)4Cl2 and NH4Cl. The collected alkaline copper etching waste liquid is placed in a copper precipitation reaction tank, and the stirring paddle is driven by a motor to rotate, so that the alkaline copper etching waste liquid can be fully stirred, which is convenient for subsequent contact with the decomplexing agent for reaction.
[0032] Step 120, adding a complex breaking agent to the copper precipitation reaction tank, and then adding basic copper salt seed crystals to react to obtain a primary reaction product.
[0033] In the present embodiment, under the condition of normal temperature and stirring speed of 160r / min, a chelating agent is added to the alkaline copper-etching waste liquid, and the alkaline copper-etching waste liquid and the chelating agent are fully mixed by stirring, and the pH value of the alkaline copper-etching waste liquid is equal to 7 under the monitoring of a pH meter or an ORP detector, and then the chelating agent is continuously added dropwise to make the pH value of the alkaline copper-etching waste liquid less than 7, and then basic copper salt seeds are added to induce crystallization, and the pH value of the alkaline copper-etching waste liquid is controlled to be 4-5.5, that is, the amount of chelating agent added is controlled, so that the pH value of the alkaline copper-etching waste liquid is maintained between 4-5.5, at this time, the color of the primary reaction product becomes dark green. If the pH value of the alkaline copper-etching waste liquid is lower than 4, the basic salt precipitate generated in the primary reaction product will dissolve again, which will reduce the recovery rate of the copper element and easily cause heavy metal pollution; if the pH value of the copper-etching waste liquid is higher than 5.5, it will cause insufficient dechelating force, and the basic salt precipitate cannot be completely generated, and it is impossible to ensure that the copper element is completely recovered, which will also cause environmental pollution. At the same time, the addition of basic copper salt seed crystals is beneficial to the growth of crystals, the particle size distribution of the crystals is more uniform, and a crystalline precipitate with good crystal shape is obtained.
[0034] In one embodiment, the complex breaking agent is hydrochloric acid, and the basic copper salt seed is basic copper chloride. Specifically, when Cu(NH3)4Cl2 encounters H+ in hydrochloric acid, the complex will be broken and Cu will be released. 2+ , and react to form basic copper chloride precipitate, and then H+ combines with NH3 in the ammonia complex to form NH 4+ , and finally NH 4+ With Cl - Combine to form NH4Cl. The reaction principle is as follows:
[0035] 2[Cu(NH3)4]Cl2+5HCl+8H2O→Cu2Cl(OH)3↓+8NH4Cl.
[0036] In one embodiment, the complex breaking agent is carbonic acid, and the basic copper salt seed is basic copper carbonate. Specifically, when Cu(NH3)4Cl2 encounters H+ in carbonic acid, it will break the complex and release Cu 2+ , and react to form basic copper carbonate precipitate, and then H+ combines with NH3 in the ammonia complex to form NH 4+ , and finally NH 4+ With Cl - Combine to form NH4Cl. The reaction principle is as follows:
[0037] Cu2(NH3)2Cl2+H2CO3+2OH 一 →Cu2(OH)2CO3↓+2NH4Cl.
[0038] In one embodiment, the complex breaking agent is sulfuric acid, and the basic copper salt seed is basic copper sulfate. Specifically, when Cu(NH3)4Cl2 encounters H+ in carbonic acid, it will break the complex and release Cu 2+ , and react to form basic copper carbonate precipitate, and then H+ combines with NH3 in the ammonia complex to form NH 4+ , and finally NH 4+ With Cl - Combine to form NH4Cl. The reaction principle is as follows:
[0039] Cu2(NH3)2Cl2+H2SO4+2OH 一 →Cu2(OH)2SO4↓+2NH4Cl.
[0040] Step 130, filtering the primary reaction product to obtain a basic salt precipitate and an ammonium chloride mother liquor.
[0041] In this embodiment, a corrosion-resistant pump is used to press the primary reaction product obtained by the reaction into a separation device for filtration, and the separation device is a flat automatic centrifuge to obtain a basic salt precipitate and an ammonium chloride mother liquor, and then the basic salt precipitate and the ammonium chloride mother liquor obtained by separation are treated differently. It should be understood that when separating the basic salt precipitate and the ammonium chloride mother liquor in the primary reaction product, other solid-liquid separation methods can also be used, including gravity filtration, pressure filtration and vacuum filtration, etc. The method for achieving solid-liquid separation is common knowledge known to those skilled in the art and will not be repeated here.
[0042] Step 140, stirring and rinsing the basic salt precipitate, and dehydrating and drying to obtain the basic salt.
[0043] In this embodiment, in addition to water, the basic salt precipitate also contains 1-2% of ammonium chloride mother liquor. Therefore, when preparing high-quality basic salt, it is necessary to further remove the ammonium chloride mother liquor attached to the surface. Specifically, the basic salt precipitate obtained by filtration is added to a rinsing tank, and purified water is added while stirring and rinsing is performed to remove the ammonium chloride mother liquor on the surface of the basic salt precipitate. At this time, the rotation speed of the stirrer is 160r / min. The rinsed basic salt precipitate is then dehydrated to obtain the rinsed basic salt precipitate, and the above operation is repeated until the component concentration of the ammonium chloride mother liquor in the rinsing liquid is lower than 30g / L, so that the basic salt precipitate can reach a certain purity. The rinsed basic salt precipitate is then dehydrated and pressed into a high-temperature air flow dryer. The rinsed basic salt precipitate contains 50%-60% of water. In the high-temperature air flow dryer, the basic salt precipitate is reversely contacted with high-temperature air, which can play a sufficient drying role. The drying temperature is controlled to be 150°C, and the water can be evaporated quickly, so that the water content of the basic salt precipitate is lower than 0.5%. The drying time is short, and the drying time is 1-2min. Finally, a high-quality basic salt precipitate is obtained.
[0044] The invention provides a process for treating alkaline copper etching waste liquid by a chelation breaking copper precipitation method. The process comprises the following steps: adding the alkaline copper etching waste liquid into a copper precipitation reaction tank, adding a chelation breaking agent while stirring, then adding basic copper salt seeds, reacting to obtain a primary reaction product, filtering the primary reaction product to obtain a basic salt precipitate and an ammonium chloride mother liquor, stirring and rinsing the obtained basic salt precipitate, and dehydrating and drying to obtain a basic salt. In this way, when the alkaline copper etching waste liquid is chelated to generate a water-insoluble basic salt precipitate, under sufficient stirring of the copper precipitation reaction tank, the generated basic salt molecules continuously collide with the basic copper salt seeds to precipitate, can be well attached to the basic copper salt seeds, can promote the basic salt molecules to be fully precipitated from the reaction solution, can greatly improve the recovery efficiency and recovery rate of the alkaline copper etching waste liquid, make the alkaline copper etching waste liquid fully converted into an environmentally friendly and pure substance, realize the recycling and utilization of waste materials, and be green and environmentally friendly.
[0045] In one embodiment, the process for treating alkaline copper etching waste liquid by the chelation breaking copper precipitation method also includes: adding the ammonium chloride mother liquor into a regeneration mixing tank, taking samples to test the chloride ion content while stirring, and introducing ammonia gas after balance to obtain an alkaline etching solution.
[0046] In the present embodiment, the main component in the ammonium chloride mother liquor is ammonium chloride, and the ammonium chloride solution is one of the main components of the alkaline etching solution. The ammonium chloride solution obtained by filtering the primary reaction product is placed in a regeneration mixing tank. Since the ammonium chloride solution and ammonia are mixed into an alkaline etching solution, the ratio of the amount of the two exists. Therefore, before the ammonia is introduced, it is necessary to sample and test the content of chloride ions under uniform stirring, and the speed of the mixer is 60r / min. If the ammonium chloride content obtained by the test is in accordance with the ratio of the two, it is not necessary to balance; if the ammonium chloride content obtained by the test is not in accordance with the ratio of the two, when the ammonium chloride content is higher than the formula ratio, water is added for dilution; when the ammonium chloride content is lower than the formula ratio, ammonium chloride is added to make the content of ammonium chloride meet the formula ratio, and the chloride ion content is finally controlled to be 165-175g / L.
[0047] In the present embodiment, after confirming the balance of the ratio of ammonium chloride solution and ammonia, ammonia is introduced into the regeneration blending tank, and the reaction end point is controlled to be 5.1-5.3 mol / L for the concentration of ammonia, and the solution pH value is 8.5-9.5, that is, an alkaline etching solution is obtained. If the solution pH value is too low, on the one hand, it is unfavorable for the metal anti-corrosion layer, and on the other hand, the copper in the etching solution cannot be completely complexed into copper ammonia complex ions, causing etching difficulties; if the solution pH value is too high, the ammonia in the etching solution is supersaturated, and free ammonia is released into the atmosphere, causing environmental pollution, and also increasing the degree of side etching, thereby affecting the accuracy of etching. After passing the inspection, it can be returned to the etching production line of the PCB factory for reuse, avoiding the environmental pollution caused by directly discharging the ammonium chloride solution, and reducing the recovery cost of the alkaline copper etching waste liquid, avoiding the waste of reagents, so that the ammonium chloride solution can be used cyclically, so that the components of the alkaline copper etching waste liquid can be fully recycled and recycled, without other pollutants.
[0048] In order to improve the crystallization efficiency of basic salt precipitation. In one embodiment, Figure 2 , Figure 3 and Figure 4As shown, the copper plating reaction tank 10 includes: a reaction tank body 100, a stirring paddle 200 and a motor 300. A stirring chamber is opened in the reaction tank body 100. The stirring paddle 200 is rotatably arranged in the stirring chamber. The motor 300 is arranged on a first side of the reaction tank body 100, and the motor 300 is drivingly connected to the stirring paddle 200. A plurality of guide plates 400 are obliquely arranged on the side wall of the stirring chamber. The first side of each of the guide plates 400 is connected to the side wall of the stirring chamber, and the second side of each of the guide plates 400 faces the central axis of the stirring chamber. Specifically, when the motor 300 drives the stirring paddle 200 to rotate, it can generate a strong radial force, driving the alkaline copper-etching waste liquid, the chelating agent and the basic copper salt crystal seeds to move radially. By arranging a plurality of guide plates 400 on the side wall of the stirring wall, the movement direction of the alkaline copper-etching waste liquid, the chelating agent and the basic copper salt crystal seeds can be changed, so that the alkaline copper-etching waste liquid, the chelating agent and the basic copper salt crystal seeds can move radially and axially. At the same time, the inclined guide plates 400 can guide the alkaline copper-etching waste liquid, the chelating agent and the basic copper salt crystal seeds to the central area of the stirring chamber, forming a mixed zone with strong collisions, and the generated basic salt molecules constantly collide with the basic copper salt crystal seeds and precipitate, and adhere to the basic copper salt crystal seeds, which is conducive to improving the crystallization efficiency of generating the basic salt precipitation, so that precipitation crystallization can occur better, the basic salt precipitation is fine and uniform, and the copper element can be fully recovered.
[0049] In one embodiment, Figure 3As shown, an annular air pipe 500 is disposed around the side wall of the stirring chamber, and the annular air pipe 500 is spaced apart from the guide plate 400. A plurality of aeration holes 510 are provided on the annular air pipe 500, and each of the aeration holes 510 faces the bottom of the stirring chamber. Specifically, the annular air pipe 500 is located below the guide plate 400, and the annular air pipe 500 is disposed around the side wall of the stirring chamber, and each of the aeration holes 510 faces the bottom of the stirring chamber. In this way, air is supplied to the annular air pipe 500 through an external air supply device, and is introduced into the stirring chamber through the aeration holes 510. For example, the number of aeration holes 510 is 80, and the injected air will form bubbles that move upward, thereby driving the alkaline copper etching waste liquid at the bottom of the stirring chamber to move from bottom to top, and the aeration holes 510 are evenly distributed around. On the side wall of the stirring chamber, the alkaline copper-etching waste liquid at the bottom of the stirring chamber can move from the bottom center of the stirring chamber to the top, so that the alkaline copper-etching waste liquid is directed to the central area of the stirring chamber, that is, the generated basic salt precipitate rolls, further forming a mixed zone with strong collisions, and the alkaline copper-etching waste liquid can more fully contact and react with the decomposing agent, and the generated basic salt molecules further collide with the basic copper salt seeds and precipitate, and adhere to the basic copper salt seeds to obtain uniform and fine basic salt precipitation particles, thereby improving the efficiency of generating basic salt precipitation. At the same time, the discharge is smooth, which can prevent the basic salt precipitate from adhering to the bottom side wall of the stirring chamber, and reduce the difficulty of cleaning the reaction tank body 100.
[0050] In one embodiment, Figure 3 As shown, the reaction tank body 100 is a flat-top round-bottom tank body. Specifically, by setting a round bottom at the bottom of the reaction tank body 100, when the external gas supply device supplies gas into the annular gas supply pipe 500 and passes the gas into the stirring chamber through the aeration hole 510, under the action of the airflow, the alkaline copper-etching waste liquid at the bottom of the stirring chamber is facilitated to move from the outer edge of the bottom to the center, and can move better from bottom to top, and can avoid residual basic salt precipitation at the bottom corners of the reaction tank body 100.
[0051] In one embodiment, a plurality of limit blocks are provided on the guide plate 400, and the limit blocks are distributed in a matrix shape along the central axis of the guide plate 400, and the height of the limit blocks gradually decreases in the direction from the first side of the guide plate 400 to the second side of the guide plate 400. In this way, when the motor 300 drives the stirring paddle 200 to stir and lift the alkaline copper etching waste liquid to flow, the guide plate 400 can play a role in guiding the flow, so that the alkaline copper etching waste liquid flows back from the outside of the stirring chamber to the central area, thereby improving the stirring and mixing effect of the alkaline copper etching waste liquid and the complex breaking agent, and is beneficial to the movement and collision between the molecular ions in the alkaline copper etching waste liquid and the complex breaking agent, thereby promoting the generation and polymerization precipitation of basic copper chloride crystals, and is beneficial to fully recovering the recovery rate of copper ions.
[0052] Furthermore, by arranging a plurality of limit blocks on the guide plate 400, the limit blocks are of an arc-shaped structure. When the alkaline copper-etching waste liquid is stirred by the stirring paddle 200, the basic cupric chloride crystals in the alkaline copper-etching waste liquid move along the guide plate 400 toward the central area of the stirring chamber. In this way, each limit block can increase the surface area of the guide plate 400, that is, increase the contact area between the basic cupric chloride crystals and the guide plate 400, and can better generate collision force on the basic cupric chloride crystals, thereby facilitating the contact and collision between the basic cupric chloride crystals, and further promoting the agglomeration speed of the basic cupric chloride crystals.
[0053] In addition, the height of the limit block gradually decreases from the first side of the guide plate 400 to the second side of the guide plate 400, so that the basic cupric chloride crystals can touch the limit block with a larger area during the initial reflux and be subjected to a larger collision force. As the reflux kinetic energy decreases, the height and area of the limit block decrease, so that the basic cupric chloride crystals are subjected to a smaller collision force, so that the collision effect of the basic cupric chloride crystals decreases from large to small, and the impact force is linearly distributed. In this way, in the initial stage, the basic cupric chloride crystals are subjected to a large collision force and the speed decreases rapidly, and the basic cupric chloride crystals can collide and contact better. As the reflux distance increases, the collision force gradually decreases and the speed is also slower, which can ensure that the basic cupric chloride crystals can smoothly pass through the limit protrusion and reflux to the central area of the stirring chamber. By stirring again to form a circulating reflux, the efficiency of the crystallization and precipitation of the basic cupric chloride crystals can be improved.
[0054] In one embodiment, the stirring paddle 200 includes: a stirring shaft and a stirring blade, the motor 300 is drivingly connected to the first end of the stirring shaft, the first side of the stirring blade is connected to the second end of the stirring shaft, and a plurality of conducting grooves are provided on the stirring blade, each of which is arranged to penetrate the second side of the stirring blade. In this way, when the motor 300 drives the stirring paddle 200 to rotate and stir, a part of the alkaline copper etching waste liquid rotates under the action of the stirring blade, and the other part of the alkaline copper etching waste liquid passes through the conducting groove and does not rotate synchronously with the stirring blade. In this way, a relative displacement is formed between the two parts of the alkaline copper etching waste liquid, which is conducive to the violent collision of the basic copper chloride crystals due to the displacement difference, and can better agglomerate and precipitate.
[0055] Furthermore, a countercurrent groove is provided on the side wall of the conducting groove, and the height of the first side of the countercurrent groove is less than the height of the second side of the countercurrent groove, that is, the countercurrent groove is an arc-shaped groove. In this way, when the alkaline copper-etching waste liquid flows from the first side of the countercurrent groove to the second side of the countercurrent groove, due to the height difference, the kinetic energy of part of the alkaline copper-etching waste liquid increases, and part of the alkaline copper-etching waste liquid can flow upward, which is beneficial to promote the contact and collision between the basic copper chloride crystals, and can better agglomerate and precipitate.
[0056] In one embodiment, a system for treating alkaline copper etching waste liquid by a chelating copper precipitation method comprises a chelating agent metering tank, a copper precipitation reaction tank, a flat automatic centrifuge, a regeneration mixing tank and a high-temperature airflow dryer which are arranged in sequence. When treating the alkaline copper etching waste liquid, the alkaline copper etching waste liquid is pumped into the copper precipitation reaction tank by a centrifugal pump to perform a chelating copper precipitation process. Under the condition of stirring at room temperature and monitoring by the chelating agent metering tank, a chelating agent is added to make the pH value of the alkaline copper etching waste liquid equal to 7, and then the chelating agent is continuously added dropwise to make the pH value of the alkaline copper etching waste liquid less than 7, and then basic copper salt seed crystals are added to induce crystallization, and the pH value of the alkaline copper etching waste liquid is reduced to 4-5.5, and the color of the primary reaction product becomes dark green. At this time, the primary reaction product contains basic salt precipitation and ammonium chloride mother liquor.
[0057] Then the primary reaction product is pumped into a flat plate automatic centrifuge through a mud pump for centrifugal separation. The flat plate automatic centrifuge is started to continuously dehydrate to obtain basic salt precipitate and ammonium chloride mother liquor. The basic salt precipitate is then sprayed with hot water and scraped off.
[0058] Furthermore, the basic salt precipitate is conveyed to the wet material tank of the drying process by belt conveyor for high-temperature drying process, and the high-temperature airflow dryer is started to make the basic salt precipitate contact with the high-temperature air in reverse direction, which can play a sufficient drying role, and the drying temperature is controlled to be 150°C, which can quickly evaporate the water, so that the water content of the basic salt precipitate is less than 0.5%, thereby obtaining high-quality basic salt.
[0059] Finally, the ammonium chloride mother liquor recovered in the centrifugal separation process is pumped into the regeneration mixing tank, and the chloride ion content is sampled and tested, and then ammonium chloride is added according to the industry standard, and ammonia gas is introduced into the regeneration mixing tank, and the reaction end point is controlled to be ammonia concentration of 5.1-5.3 mol / L, and the solution pH value is 8.5-9.5, to obtain an alkaline etching solution.
[0060] The present invention is further described below with specific examples.
[0061] Example 1
[0062] A process for treating alkaline copper etching waste liquid by a chelation-breaking copper precipitation method comprises the following steps:
[0063] 1.0m 3 The alkaline copper etching waste liquid is added to the copper precipitation reaction tank, the alkaline copper etching waste liquid is stirred at room temperature, and then a certain amount of complex breaking agent hydrochloric acid is added to the copper precipitation reaction tank, that is, 320Kg / m 330% HCl is added to make the pH value of the alkaline copper etching waste liquid equal to 7, and then the complex breaking agent is continued to be added to make the pH value of the alkaline copper etching waste liquid less than 7, and basic copper salt seed crystals and basic copper chloride are added to induce crystallization, that is, 60Kg of 30% HCl is continued to be added to make the pH value of the alkaline copper etching waste liquid drop to 4-5.5, and the color of the primary reaction product obtained by the reaction turns dark green. At this time, the primary reaction product contains basic copper chloride precipitate and ammonium chloride mother liquor.
[0064] Then, the primary reaction product is pumped into a flat plate automatic centrifuge through a mud pump for centrifugal separation. The flat plate automatic centrifuge is started to continuously dehydrate to obtain basic cupric chloride precipitate and ammonium chloride mother liquor. The basic cupric chloride precipitate is then sprayed with hot water and scraped off.
[0065] Furthermore, the basic cupric chloride precipitate is conveyed to the wet material tank of the drying process by belt conveyor for high-temperature drying process, and the high-temperature airflow dryer is started to make the basic cupric chloride precipitate contact with the high-temperature air in reverse direction, which can play a sufficient drying role, and the drying temperature is controlled to be 150° C., which can quickly evaporate the water content of the basic salt precipitate, so that the water content of the basic salt precipitate is less than 0.5%, thereby obtaining the basic cupric chloride as an additive for high-grade feed.
[0066] Finally, the obtained 0.8m 3 The ammonium chloride solution is added to the regeneration preparation tank, 0.8m 3 The ammonium chloride solution contains 220 kg of ammonium chloride, and then while stirring, sampling is performed to test the chloride ion content. According to industry standards, 50 kg / m 3 The ammonium chloride is added, and ammonia gas is introduced into the regeneration mixing tank, and the reaction end point is controlled so that the ammonia concentration reaches 5.1-5.3 mol / L and the solution pH value is 8.5-9.5, and the alkaline etching solution is obtained for reuse.
[0067] The process for treating alkaline copper etching waste liquid by the copper precipitation method of breaking the chelation in the present embodiment 1 can fully convert the alkaline copper etching waste liquid into environmentally friendly pure substances, namely, the additive basic copper chloride of the superior feed and the regenerated alkaline etching solution. The recycled regenerated alkaline etching solution is stable, and various detection indicators meet the industry standards, achieving "zero discharge" of waste, no pollution, green and environmental protection, good energy-saving effect, and high economic and social benefits.
[0068] The basic cupric chloride obtained in Example 1 was subjected to quality analysis according to GB / T 21696-2008 standard.
[0069] Table 1 Analysis and test results
[0070]
[0071] Among them, the feed additive basic copper chloride should meet the following requirements:
[0072] Table 2 Physical and chemical index standards
[0073] project index <![CDATA[Basic copper chloride Cu(NH3)4Cl2 (mass fraction) / % ≥]]> 98.0 Copper (Cu) (mass fraction) / %≧ 58.12 Arsenic (As) (mass fraction) / % ≦ 0.002 Lead (Pb) (mass fraction) / % ≦ 0.001 Cadmium (Cd) (mass fraction) / % ≦ 0.0003 Acid insoluble matter (mass fraction) / % ≦ 0.2 Fineness (through a test sieve with a pore size of 250μm) / %≧ 95
[0074] Among them, 1. Sensory properties: dark green and light green powder or granules, insoluble in water, soluble in acid and ammonia water, stable in air.
[0075] 2. Physical and chemical indicators: The physical and chemical indicators of feed additive basic copper chloride should meet the requirements of Table 1.
[0076] According to the analysis and test results (Table 1) in report number 2020161219b, the basic cupric chloride prepared in Example 1 of the present invention is in the form of powder, and the standards of various physical and chemical indicators meet the standards of various physical and chemical indicators in Table 2.
[0077] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0078] The above-mentioned embodiments only express several embodiments of the present application, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present application, which all belong to the protection scope of the present application. Therefore, the protection scope of the patent of this application shall be based on the attached claims.
Claims
1. A process for treating alkaline copper etching waste liquid by a copper-degrading method, characterized in that: The following steps are involved: Adding alkaline copper etching waste liquid into the copper precipitation reaction tank, and stirring the alkaline copper etching waste liquid; Adding a complex-breaking agent to the copper precipitation reaction tank, and then adding basic copper salt seed crystals to react to obtain a primary reaction product; filtering the primary reaction product to obtain a basic salt precipitate and an ammonium chloride mother liquor; Stirring and rinsing the basic salt precipitate, and dehydrating and drying to obtain the basic salt; Wherein, the copper deposition reaction tank comprises: a reaction tank body, a stirring paddle and a motor, a stirring chamber is provided in the reaction tank body, the stirring paddle is rotatably arranged in the stirring chamber, the motor is arranged on a first side of the reaction tank body, and the motor is drivingly connected to the stirring paddle, the stirring paddle comprises: a stirring shaft and a stirring plate, the motor is drivingly connected to the first end of the stirring shaft, the first side of the stirring plate is connected to the second end of the stirring shaft, a plurality of conducting grooves are provided on the stirring plate, each of the conducting grooves is arranged to penetrate the second side of the stirring plate, a countercurrent groove is provided on the side wall of the conducting groove, the countercurrent groove is an arc-shaped groove, the height of the first side of the countercurrent groove is less than the height of the second side of the countercurrent groove, when the alkaline copper etching waste liquid flows from the first side of the countercurrent groove to the second side of the countercurrent groove, due to the height difference, part of the alkaline copper etching waste liquid The kinetic energy increases, and part of the alkaline copper etching waste liquid can flow upward, which is beneficial to promoting the contact and collision between the basic copper chloride crystals, and can better agglomerate and precipitate. A plurality of guide plates are obliquely arranged on the side wall of the stirring chamber, and the first side of each of the guide plates is connected to the side wall of the stirring chamber, and the second side of each of the guide plates faces the central axis of the stirring chamber. A plurality of limit blocks are arranged on the guide plate, and each of the limit blocks is distributed in a matrix shape with respect to the central axis of the guide plate. The height of the limit blocks gradually decreases in the direction from the first side of the guide plate to the second side of the guide plate. An annular air pipe is arranged around the side wall of the stirring chamber, and the annular air pipe is spaced apart from the guide plate in the upper and lower parts. A plurality of aeration holes are opened on the annular air pipe, and each of the aeration holes faces the bottom of the stirring chamber. The reaction tank body is a flat-top round-bottom tank body.
2. The process for treating alkaline copper etching waste liquid by the copper precipitation method according to claim 1, characterized in that: The complex breaking agent is one of hydrochloric acid, carbonic acid and sulfuric acid.
3. The process for treating alkaline copper etching waste liquid by the copper precipitation method according to claim 1, characterized in that: The basic copper salt seed crystal is one of basic copper chloride, basic copper carbonate and basic copper sulfate.
4. The process for treating alkaline copper etching waste liquid by the copper-degrading method according to claim 1, characterized in that: When adding the complex breaking agent into the copper precipitation reaction tank and then adding the basic copper salt seed crystals for reaction, the pH value of the alkaline copper etching waste liquid is controlled to be 4-5.
5.
5. The process for treating alkaline copper etching waste liquid by the copper precipitation method according to claim 1, characterized in that: Also includes: The ammonium chloride mother liquor is added into the regeneration preparation tank, and while stirring, samples are taken to test the content of chloride ions, and ammonia gas is introduced after equilibrium to obtain an alkaline etching solution.
6. The process for treating alkaline copper etching waste liquid by the copper precipitation method according to claim 5, characterized in that: When sampling and testing the chloride ion content, the chloride ion content is controlled to be 165-175 g / L.
7. The process for treating alkaline copper etching waste liquid by the copper precipitation method according to claim 5, characterized in that: When ammonia gas is introduced into the reaction after the equilibrium, the reaction end point is controlled so that the ammonia concentration reaches 5.1-5.3 mol / L and the pH is 8.5-9.5.