Powders used in additive manufacturing methods and methods for preparing ceramic products using the powders

By introducing silicon monoxide and other oxide particles into the powder, the problems of expensive powder and low shaping accuracy are solved, realizing efficient and economical preparation of ceramic products with excellent heat resistance and high temperature stability.

CN117120229BActive Publication Date: 2026-11-17CANON KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202280027270.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-04-01
Filing Date
2022-04-08
Publication Date
2026-11-17
Estimated Expiration
2042-04-08

AI Technical Summary

Technical Problem

In the existing technology, when using rare earth oxides as absorbents in powder bed melting to prepare ceramics, there are problems such as expensive powders and difficulty in achieving high shaping accuracy.

Method used

A powder comprising silicon monoxide particles and other oxide particles, such as aluminum oxide and silicon dioxide particles, is used. By controlling the mass fraction of each component, the powder contains silicon and aluminum, ensuring that the SiO particles effectively absorb laser light as absorbers, avoiding light diffusion, and improving shaping accuracy.

Benefits of technology

This technology enables the inexpensive fabrication of ceramic products with high shaping precision using additive manufacturing techniques, ensuring the heat resistance and high-temperature stability of the ceramic products while reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117120229B_ABST
    Figure CN117120229B_ABST
Patent Text Reader

Abstract

A powder, which is heated by light, comprises: silicon monoxide particles; and other particles besides the silicon monoxide particles, wherein the other particles comprise at least one type of particles selected from the group consisting of alumina particles, silicon dioxide particles, and oxide particles comprising silicon and aluminum as elements, and wherein, when the other particles are converted into oxides represented by Al2O3 and SiO2, the mass fractions x, y, and z of Al2O3, SiO2, and SiO, respectively, in the entire powder satisfy the following relationship.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to powders used in the preparation of ceramic products using laser-based additive manufacturing techniques. Background Technology

[0002] With advancements in additive manufacturing technology, there is a growing expectation to use additive modeling techniques to produce dense and diverse ceramic products. In recent years, raw material powders have been developed for use in preparing ceramic products with excellent thermal properties, such as thermal shock resistance and low rates of thermal expansion, using powder bed melting, a method known for its superior shaping accuracy.

[0003] However, if powders with low light absorption, such as alumina or gallium oxide, are used as raw materials in powder bed melting, the laser light diffuses within the powder, leading to localized melting failure. Therefore, achieving high forming accuracy is difficult.

[0004] In patent document (PTL) 1, rare earth oxides with higher absorption capacity than aluminum oxide (Al2O3) are added to Al2O3 powder as absorbers to prevent light diffusion and achieve excellent shaping accuracy.

[0005] Reference List

[0006] Patent documents

[0007] PTL 1: Japanese Patent Application Publication No. 2019-19051 Invention Overview

[0009] Technical issues

[0010] In PTL 1, the powder used as a raw material is expensive because rare earth oxides are used as absorbents. To apply additive manufacturing technology to various applications, inexpensive powders capable of high-precision shaping are needed.

[0011] Solution to the problem

[0012] According to one aspect of the invention, a powder is used in an additive manufacturing method for shaping by irradiation with laser light, the powder comprising silicon monoxide (SiO) particles and at least one type of oxide particles other than SiO, wherein the at least one type of oxide particles other than SiO is selected from the group consisting of aluminum oxide (Al2O3) particles, silicon dioxide (SiO2) particles, and compound particles of Al2O3 and SiO2, such that the powder other than SiO particles comprises silicon and aluminum as elements, and wherein when the composition of the powder other than SiO particles is converted into oxides represented by Al2O3 and SiO2, the mass fractions x, y, and z of Al2O3, SiO2, and SiO in the total powder respectively satisfy the following relationship:

[0013] 20≤x<99.8,

[0014] 0<y≤80, and

[0015] 0.2≤z≤50.

[0016] Advantageous Effects of the Invention

[0017] Using the powder according to the present invention, ceramic articles can be produced and provided inexpensively with high shaping accuracy by additive manufacturing techniques.

[0018] Brief Description of the Drawings

[0019] Figure 1 is a conceptual diagram of temperature rise characteristics when laser light is irradiated to a powder containing silicon monoxide (SiO) particles and a powder not containing SiO particles.

[0020] Figure 2 is a conceptual diagram of a three-dimensional shaping apparatus using a powder bed fusion method.

[0021] Figure 3 is a conceptual diagram illustrating shaping using a coating method.

[0022] Description of Embodiments

[0023] Exemplary embodiments for carrying out the present invention (hereinafter referred to as "the present exemplary embodiments") will be described with reference to the accompanying drawings. However, the present invention is not limited to the following specific examples.

[0024] (Powder)

[0025] The powder according to the present invention is suitable as a raw material powder for use in producing ceramic articles that are excellent in heat resistance and contain a compound of alumina (Al₂O₃) and silica (SiO₂) by an additive shaping method. The powder includes silicon monoxide (SiO) particles and one or more types of oxide particles other than SiO. As the oxide particles other than SiO, at least one type is selected from the group consisting of Al₂O₃ particles, SiO₂ particles, and compound particles of Al₂O₃ and SiO₂, such that the powder other than the SiO particles contains silicon and aluminum as elements. Then, in a case where the components of all the oxide particles other than SiO (the powder other than the SiO particles) are converted into oxides represented by Al₂O₃ and SiO₂, x, y, and z which respectively represent the mass fractions of Al₂O₃, SiO₂, and SiO in the entire raw material powder satisfy the following relationships:

[0026] 20≤x<99.8,

[0027] 0<y≤80, and

[0028] 0.2≤z≤50.

[0029] Each of the SiO particles, Al2O3 particles, SiO2 particles, and compound particles of Al2O3 and SiO2 may include 1000 ppm or less of impurities other than the compound.

[0030] In this invention, the particles included in the powder refer to so-called primary particles, and the state of the particles included in the powder may be in the form of primary particles or in the form of secondary particles obtained by sintering multiple primary particles. The crystallinity of the particles may be amorphous or crystalline. In exemplary embodiments, the case of the powder "comprising multiple compounds" indicates the coexistence of many types of primary particles (each composed of one type of compound), the coexistence of one type or many types of secondary particles (composed of primary particles of multiple types of compounds), and the coexistence of these particles. Hereinafter, the primary particles constituting the powder will be simply referred to as "particles". For example, in the case where the powder comprises Al2O3 particles and SiO2 particles that are independent of each other, each of the Al2O3 particles and SiO2 particles is referred to as a "particle". In the case where the powder is composed of secondary particles obtained by sintering SiO particles, Al2O3 particles, and SiO2 particles, each of the SiO particles, Al2O3 particles, and SiO2 particles constituting the secondary particles is referred to as a "particle".

[0031] As an example of a powder composed of individual, independent particles, if Al2O3 particles are A, SiO2 particles are B, compound particles of Al2O3 and SiO2 are C, and SiO particles are D, then multiple combinations are possible. Specifically, combinations of A+D, A+B+D, A+C+D, A+B+C+D, B+C+D, and C+D can be selected.

[0032] While the following description primarily focuses on powder in its unused state, it does not preclude the possibility of including particles other than those described above through the use of powder in additive molding. For example, the following is possible: The powder is a mixture of unused Al2O3 particles, SiO2 particles, and SiO particles, but through a molding step, the powder includes composite oxide particles of Al2O3 and SiO2, wherein the Al2O3 particles and SiO2 particles are melted and integrated together.

[0033] As an example of the particles constituting the powder, there are multiple primary particles. If the primary particles of Al2O3 are A, the primary particles of SiO2 are B, the primary particles of the composite oxide including aluminum and silicon are C, and the primary particles of SiO are D, then multiple combinations are possible. The combinations of primary particles constituting the powder can be A+B, A+C, A+D, A+B+C, A+B+D, A+C+D, A+B+C+D, B+C, B+C+D, C, and C+D.

[0034] In this invention, the representation of compounds such as Al₂O₃, SiO₂, or SiO is not limited to compositions having the represented stoichiometric ratio, and an error within ±30% of the stoichiometric ratio standardized by the metal elements is allowed. For example, compounds having a Si:O ratio of 1:1.30 are also included in the representation of SiO. That is, SiO can be represented as SiO₂. m (0.7≤m≤1.3).

[0035] SiO is brown or black in color and has a relatively higher light absorption capacity for the wavelength of light (laser light) irradiated during molding compared to Al2O3 and SiO2 contained in the powder. When SiO absorbs laser light, the silicon (Si) changes from divalent to tetravalent, the metastable SiO transforms into the more stable SiO2, and its light absorption capacity for laser light decreases. Using powder obtained by adding SiO with these properties as an absorber to alumina (Al2O3) and silicon dioxide (SiO2) for molding yields the following effects.

[0036] The primary effect is that SiO, acting as an absorbent, effectively absorbs the laser light used in the preparation process and reaches a high temperature. This heat is then conducted to other compounds present in the region corresponding to the focal size of the laser light, causing a temperature increase. As a result, the area corresponding to the focal size of the laser light can be effectively and locally heated, clearly defining the interface between the area where the powder should solidify (the area irradiated by the laser light) and the area where the microparticles should not solidify (the area not irradiated by the laser light). Therefore, shaping accuracy can be improved.

[0037] The second effect is that, due to laser irradiation, SiO transforms into SiO2 with low light absorption, and the light absorption of the portion of the powder that solidifies upon laser irradiation (the solidified portion) is reduced. If the light absorption of SiO decreases to 5 / 6 times that before laser irradiation, and even when the solidified portion is irradiated under the same conditions as when the powder is solidified, the powder is not so affected as to cause a deterioration in shaping accuracy. That is, because the absorber is almost absent in the solidified portion, no temperature rise occurs as it did before laser irradiation. Even when the powder adjacent to the solidified portion is irradiated with laser light, deformation and transformation of the solidified portion are prevented. As a result, for example, the process margin of the laser irradiation conditions is widened, which leads to a reduction in the impact of changes in irradiation conditions on shaping accuracy. To obtain sufficient shaping accuracy, it is desirable that the light absorption of SiO alone before laser irradiation should be 1.2 times or greater different from the light absorption of the absorber (whose composition has changed after laser irradiation). It is further expected that the light absorption capacity of SiO alone before laser irradiation should be twice or more different from that of the absorber (whose composition has changed after laser irradiation).

[0038] The third effect is that after being irradiated with laser light, SiO is transformed into SiO2 and incorporated into the shaped product. However, SiO2 is composed of elements that make up compounds of Al2O3, represented by mullite, and SiO2. Therefore, it does not damage the physical properties of the shaped product.

[0039] As described above, by selectively irradiating the powder according to the invention with laser light for molding, the first to third effects described above are obtained, and ceramic products including compounds such as Al2O3 (represented by mullite) and SiO2 can be molded with high precision. Furthermore, SiO is marketed as a negative electrode for lithium-ion secondary batteries, and is therefore relatively inexpensive among possible compounds that can be used as absorbents.

[0040] refer to Figure 1 The conceptual diagrams provided further detail these effects. Figure 1 In the diagram, the horizontal axis represents the duration of laser irradiation, and the vertical axis represents the temperature of the irradiated region. Line A represents the temperature rise of a powder comprising Al2O3 particles and SiO2 particles but excluding SiO particles. Line B represents the concept of the temperature rise characteristics of a powder comprising Al2O3 particles, SiO2 particles, and SiO particles according to this exemplary embodiment. Each powder contains the same mass fraction of Al2O3 and SiO2. Figure 1 The diagram is merely for illustrating the concept, and the temperature rise process is not limited to the linear temperature rise process described.

[0041] Because powders excluding SiO particles have low light absorption, the irradiated laser light is scattered, and the powder temperature cannot be locally increased. Therefore, the powder's heating efficiency is poor. To raise the temperature of the powder in the irradiated region to the temperature required for sintering or melting and solidification, it is necessary to increase the input energy per unit volume. Therefore, the powder exhibits a temperature rise characteristic represented by line A. If a high input energy is used to irradiate the powder with laser light to solidify it, the scattered laser light raises the temperature of the powder in nearby areas, resulting in an unclear temperature difference between the irradiated region and the powder surrounding it. Therefore, a low-density sintered portion is formed near the area to be solidified, and high shaping accuracy cannot be obtained.

[0042] In this invention, the expression "sintering or melting and solidifying" is not limited to the case where the powder does not melt during sintering or the case where the powder does not remain unmelted during melting. The expression "sintering or melting and solidifying" includes a sintered state in which the powder is bonded together, a state that partially includes unsintered portions, a liquid-phase sintered state in which molten products exist around the powder, and a molten state in which powder still retains a portion of unmelted powder. In the following text, "sintering or melting and solidifying" is collectively referred to as "solidification".

[0043] When laser light is irradiated onto a powder containing SiO particles, the SiO absorbs the laser light, and the temperature of the powder rises rapidly, as if... Figure 1 Line B in the diagram represents the powder. Therefore, the powder exhibits excellent heating efficiency and can be locally heated. The temperature difference between the laser-irradiated area and the surrounding area is sufficiently ensured, and the range of the sintered portion near the solidified portion is narrow. Therefore, excellent shaping accuracy can be obtained. In the solidified portion, SiO changes to SiO2, and the light absorption capacity decreases. Therefore, the powder exhibits properties similar to powders without absorbers. Therefore, due to changes in process conditions, even when laser light is irradiated onto the already shaped portion, the temperature rise is relatively small, and the powder is almost unaffected by the temperature rise. Due to heat conduction between the two regions, the area being irradiated by the laser light and the solidified area are combined through fusion. Therefore, no problems arise in the connection between the earlier and later solidified areas and the strength of the boundary portions between regions. As described above, if additive molding is performed using a powder with characteristics represented by line B according to the present invention, the above three effects can be obtained.

[0044] In powder bed fusion methods where a recoating machine is used to form a powder bed, or in coating methods where powder is sprayed from a nozzle, it is important for the powder to have a flowability suitable for the situation. Therefore, it is desirable that the powder according to this exemplary embodiment has a flowability index of 40 [sec / 50g] or less. To ensure such flowability, it is desirable that each particle has a spherical shape. However, the shape of the particles is not limited to a spherical shape, as long as the above flowability index is met.

[0045] It is particularly desirable that the SiO particles acting as the absorber be in a state independent of other components, regardless of the state of other compounds included in the powder. This allows for higher light absorption than when multiple SiO particles form a secondary particle or when SiO particles form a secondary particle with other particles. Furthermore, the laser light easily reaches the absorber, and the absorber's light absorption capacity can be effectively utilized. Additionally, if the SiO particles are independent of other components, the particle size of the SiO particles and other particles can be adjusted individually. Therefore, the flowability of the powder is easily controlled, and the amount of absorber within the spot diameter of the laser light to be irradiated is also easily controlled. This will be described in detail below.

[0046] In the absence of secondary particles in the powder, regarding achieving the desired flowability, it is desirable that the average particle size of each of the oxide particles other than SiO should be 5 micrometers (μm) or larger and greater than the average particle size of SiO particles. More preferably, the average particle size of each of the oxide particles other than SiO should be 5 μm or larger and five times or larger than the average particle size of SiO particles. Even more preferably, the average particle size of each of the oxide particles other than SiO should be 10 μm or larger and five times or larger than the average particle size of SiO particles. Furthermore, regarding achieving high shaping accuracy and ease of sintering or melting the powder, it is desirable that the average particle size should be 200 μm or smaller. More preferably, the average particle size should be 150 μm or smaller.

[0047] Ideally, the average particle size of SiO particles should be 10 μm or smaller and one-fifth or smaller of the particle size of each of the oxide particles other than SiO. If this condition is met, the likelihood of dispersed SiO particles and the presence of multiple SiO particles near the oxide particles other than SiO increases. Therefore, the heat generated by SiO absorbing laser light is effectively conducted to the oxide particles other than SiO, and the powder in the laser-irradiated section is easily melted. Considering the dispersibility of SiO in the powder and achieving a high packing density, the average particle size of SiO particles should be as small as possible. On the other hand, if the average particle size of SiO particles is 1 μm or larger, scattering of SiO particles into the atmosphere due to laser irradiation is prevented, and the amount of SiO particles in the powder required as an absorbent can be maintained. Therefore, the average particle size of SiO particles should ideally be 1 μm or larger and 10 μm or smaller. More ideally, the average particle size of SiO particles should be 1 μm or larger and less than 5 μm.

[0048] When the powder includes secondary particles, to achieve flowability suitable for additive manufacturing, it is desirable that the average particle size of the secondary particles be 5 μm or larger. More preferably, the average particle size should be 5 μm or larger and five times or larger than the average diameter of the SiO particles. Even more preferably, the average particle size should be 10 μm or larger and five times or larger than the average diameter of the SiO particles. Regarding achieving high shaping accuracy and ease of sintering or melting the powder, it is desirable that the average particle size be 200 μm or smaller. More preferably, the average particle size should be 150 μm or smaller. The average particle size of the primary particles constituting the secondary particles can be smaller than the average particle size of the SiO particles.

[0049] The average particle size of SiO particles contained in a powder is obtained as follows: The powder is observed using a scanning electron microscope (SEM), and regions composed of SiO particles are identified through compositional analysis using energy-dispersive X-ray spectroscopy (EDS) provided in the SEM. The area of ​​the identified region is measured, and the equivalent circle diameter of that area is calculated. The region composed of multiple (100 or more) SiO particles is measured, and the median of the multiple SiO particles is determined as the average particle size. This calculation method can be used to calculate the average particle size regardless of the type or state of the particles. A similar technique can also be used to calculate the average particle size of secondary particles. The powder is observed using a scanning electron microscope (SEM), compositional analysis is performed, and regions of secondary particles aggregated from primary particles and the types of primary particles constituting the secondary particles are identified. The equivalent circle diameter of the area of ​​the region containing multiple (100 or more) secondary particles is calculated, and the median of the multiple secondary particles is determined as the average particle size.

[0050] The particle size according to this exemplary embodiment refers to the equivalent circular diameter (Heywood diameter) of a single particle. The average particle size of the powder comprising particles of a particular composition does not refer to the particle size of an individual particle, but is the median of a group of particles having the same composition. This does not mean that the powder does not contain particles having sizes other than those expressed as the average particle size.

[0051] It is desirable that the powder according to this exemplary embodiment should not contain resin binders. This is because resin binders have a significantly lower melting point than other compounds included in the powder. Therefore, resin binders can be explosively burned off by irradiation with laser light, creating pores or defects that are present inside the molding area.

[0052] If the powder contains elemental carbon with sublimation properties, carbon and oxygen can combine and escape as gas, and the volume occupied by the elemental carbon can become pores. Furthermore, elemental carbon can sublimate due to laser irradiation, and rapid vaporization adversely affects the shaping process. In particular, rapid vaporization can apply stress to the molten or solidified portions of the powder, leading to deformed products. Therefore, it is desirable that the amount of elemental carbon in the powder be low. Specifically, it is desirable that the amount of elemental carbon in the powder be 1000 ppm or less relative to the molar ratio of the various metal elements included in the powder.

[0053] The powder according to this exemplary embodiment may be in any of the following states: crystalline, amorphous, and mixed. The compositions of the powder and the shaped ceramic article do not need to match. In particular, the powder and the shaped ceramic article may have differences, such as being in an oxidized or nitrided state.

[0054] As described above, the powder according to the present invention includes SiO particles and one or more types of oxide particles other than SiO. As the oxide particles other than SiO, one or more types of particles are selected from the group including Al₂O₃ particles, SiO₂ particles, and compound particles of Al₂O₃ and SiO₂, such that the powder includes silicon and aluminum as elements. Then, in the case where the components of the oxide particles other than SiO included in the powder according to the present invention are converted into oxides represented by Al₂O₃ and SiO₂, and the mass fractions (mass%) of Al₂O₃, SiO₂ and SiO are represented by x, y and z respectively, 20≤x<99.8, 0<y≤80 and 0.2≤z≤50 are satisfied. It does not matter in what particle form the particles are included, as long as the converted amounts of the aluminum and silicon oxides included in the powder respectively satisfy x and y described above. As combinations of the compositions of the oxide particles other than SiO constituting the powder, the following combinations are possible: SiO₂-Al₂O₃, SiO₂-Al₂O₃-(compound or mixture of Al₂O₃ and SiO₂), SiO₂-(compound or mixture of Al₂O₃ and SiO₂), and Al₂O₃-(compound or mixture of Al₂O₃ and SiO₂). If the stability of the composition of the powder is considered, SiO₂-Al₂O₃, SiO₂-Al₂O₃-(compound of Al₂O₃ and SiO₂), SiO₂-(compound of Al₂O₃ and SiO₂), and Al₂O₃-(compound or mixture of Al₂O₃ and SiO₂) are desirable. If the powder according to the present invention is used, a ceramic article including a compound of Al₂O₃ and SiO₂ represented by mullite can be produced using an additive manufacturing technique. Ceramics including the compound of Al₂O₃ and SiO₂ are characterized by being more excellent than alumina in terms of thermal shock resistance and high-temperature creep.

[0055] Al₂O₃ and the compound of Al₂O₃ and SiO₂ have a higher thermal conductivity than SiO₂ and have a lower viscosity upon melting than SiO₂. Therefore, since the powder satisfies x≥20, the heat emitted from SiO when irradiated with laser can be efficiently conducted to other particles via Al₂O₃ or the compound of Al₂O₃ and SiO₂ to melt the other particles. Then, the molten Al₂O₃ or the molten compound of Al₂O₃ and SiO₂ can fuse with adjacent particles to form a dense shaped product. It is more desirable that the powder should satisfy x≥30.

[0056] In another aspect, since Al₂O₃ has low viscosity when molten, Al₂O₃ is suitable for shaping, but the following problem arises. When Al₂O₃ solidifies from the molten state, Al₂O₃ tends to grow along a specific crystal axis direction. If crystals start to grow randomly at various positions in the molten Al₂O₃, the gaps between crystal grains are not sufficiently filled, and pores are prone to form in the solidified portion. Therefore, in the powder according to the present invention, it is desirable that the mass fraction of Al₂O₃ satisfies x<99.8. It is more desirable that the mass fraction of Al₂O₃ satisfies x≤99. Then, an appropriate amount of SiO₂ is added. By adding an appropriate amount of SiO₂, a compound of Al₂O₃ and SiO₂ is generated when Al₂O₃ solidifies, and multiple phases appear. This makes the crystal composition of the solidified portion fine and prevents the occurrence of pores.

[0057] Regarding the prevention of pores in the solidified portion by adding SiO₂ to the powder, it is desirable that the mass fraction of SiO₂ satisfies 0<y. It is more desirable that the mass fraction of SiO₂ satisfies 1.0≤y. It is even more desirable that the mass fraction of SiO₂ satisfies 3.0≤y. In another aspect, SiO₂ has high viscosity when molten. Therefore, if the powder contains excessive SiO₂, SiO₂ tends to form a spherical shape in the molten state and solidify as it is, and the shaped product to be formed tends to be porous. For shaping a dense ceramic article, it is desirable that y≤80 is satisfied. It is more desirable that y<50 is satisfied. Therefore, for shaping a dense ceramic article with few pores, it is desirable that the mass fraction of SiO₂ satisfies 1.0≤y<50. It is more desirable that the mass fraction of SiO₂ satisfies 3.0≤y<50. Also, in the case where x, y and z (which are the mass fractions of Al₂O₃, SiO₂ and SiO respectively) satisfy y<x+z, a dense shaped product (which is desirable) can be easily obtained.

[0058] Even in the case of including components other than Al₂O₃, SiO₂ and SiO, in order to realize a ceramic article with high thermal shock resistance and low thermal expansion rate, it is desirable to use a powder that satisfies 90≤x+y+z. It is more desirable that the powder satisfies 95≤x+y+z.

[0059] The mass fraction of SiO in the powder satisfies 0.2 ≤ z ≤ 50. If the mass fraction of SiO, z, is less than 0.2, the heat generated per unit time when the powder is irradiated with laser is insufficient, making it difficult to melt the powder. If the input heat is increased by increasing the laser output or extending the irradiation time to melt the powder, the heat is conducted to the surrounding area of ​​the laser irradiation site, making it difficult to locally melt the powder, which leads to a deterioration in shaping accuracy. For efficient local melting of the powder, it is necessary to satisfy 0.2 ≤ z, and more preferably 0.5 ≤ z. This condition holds true whether the SiO particles are independent of oxide particles other than SiO, or whether the SiO particles and oxide particles other than SiO constitute secondary particles.

[0060] If the mass fraction z of SiO in the powder is 0.2 or greater, then SiO acts as an absorbent.

[0061] If the powder contains more than 50% by mass of SiO, the shaping accuracy tends to decrease. This is believed to be because the temperature rises rapidly in the area irradiated by the laser, causing the molten material to disperse around it. Therefore, to obtain excellent shaping accuracy, the amount of SiO in the powder should be z ≤ 50%.

[0062] As mentioned above, it is desirable for SiO particles to be independent of other particles (independent particles) and to have a small grain size. However, if the powder includes many SiO particles with small diameters, the powder's flowability may be reduced, and a flowability index suitable for additive manufacturing methods may not be obtained. If SiO particles are included as independent particles in the powder, the desired amount of SiO is z ≤ 20.

[0063] If the SiO particles are independent particles, then in order to achieve a more effective temperature rise by irradiating with a laser, it is desirable that the area irradiated by the laser beam includes at least one SiO particle. Therefore, it is desirable to select the average particle size of SiO based on the focal size of the laser beam to be irradiated onto the powder during the preparation process. This also applies to the case where SiO particles are combined with oxide particles other than SiO to form secondary particles.

[0064] Regarding thermal uniformity during laser irradiation, it is desirable for the laser beam focal size to probabilistically include two or more SiO particles. Ideally, the distance between SiO particles in the powder should probabilistically be 100 μm or less. More ideally, the distance between SiO particles in the powder should be 50 μm or less. This can be achieved by setting the mass fraction of SiO in the powder to 0.2 or greater.

[0065] The focal size of the laser beam can also be adjusted to include two or more SiO particles. Regarding shaping accuracy, if the desired focal size of the laser beam is 100 μm or smaller, then the desired average particle size of the SiO particles should be 1 μm or larger and 10 μm or smaller. The focal size of the laser beam to be irradiated can be determined according to the desired shaping accuracy, and can be 100 μm or larger, depending on the required shaping accuracy. In this case, if the focal size of the laser beam includes two or more SiO particles, the average particle size of the SiO particles can be greater than 10 μm. This also applies to cases where SiO particles form secondary particles with other particles.

[0066] Regarding achieving sufficient light absorption capacity, it is desirable that the light absorption capacity of SiO alone should be 10% or greater. More ideally, it should be 40% or greater. Even more desirable would be 60% or greater. Because the light absorption capacity of SiO varies depending on the elemental ratio between Si and O, the desired deviation of the constituent element ratio is within ±20% of the stoichiometric ratio. If the ratio of silicon to oxygen is approximately 1:1, SiO exhibits high absorption capacity for general light (Nd:YAG) with a wavelength of approximately 1 μm, which is particularly desirable. Regarding achieving high light absorption capacity while maintaining the silicon-oxygen composition ratio in SiO, it is desirable that the SiO particles in the powder be independent particles.

[0067] The elemental ratios of compounds included in the powder according to this exemplary embodiment can be identified using scanning electron microscopy-energy dispersive X-ray spectroscopy (SEM-EDX), transmission electron microscopy-energy dispersive X-ray spectroscopy (TEM-EDX), electron diffraction, or X-ray diffraction. Alternatively, the elemental ratios of compounds included in the powder can also be identified by combining inductively coupled plasma atomic emission spectrometry (ICP-AES), inductively coupled plasma mass spectrometry (ICP-MS), X-ray fluorescence spectrometry, or inert gas melting methods.

[0068] A general spectrometer can be used to measure light absorption capacity. Light of a predetermined wavelength (the wavelength of the laser to be irradiated during preparation or a wavelength close to that laser) is emitted into the sample-filled sample disk of the target powder, and an integrating sphere is used to measure the light reflection. Using the reflection in the absence of a sample as reference data, the light absorption capacity can be calculated based on the ratio between the measured reflection and the reference data.

[0069] The absorber (whose composition has been altered) is a compound that constitutes at least a part of the ceramic product. The envisioned wavelength refers to the wavelength of the laser light to be irradiated during the preparation process, or a wavelength close to that laser wavelength. The powder (measuring its light absorption capacity) can be a compound equivalent to the ceramic product and does not need to be a powder used in the preparation of the ceramic product itself.

[0070] Due to this reduction in light absorption, once a portion has been sintered or melted and solidified by laser irradiation, it is less susceptible to subsequent laser irradiation and retains its shape. Therefore, precise three-dimensional ceramic products can be fabricated as designed.

[0071] Prolonged exposure to crystalline SiO2 powder can damage the respiratory system. Therefore, it is preferable that the powder should include amorphous SiO2 as SiO2.

[0072] (Methods for preparing ceramic products)

[0073] The powder according to this exemplary embodiment is suitable for use in additive manufacturing methods, wherein a ceramic article is shaped by irradiating the powder with laser light based on slice data generated from three-dimensional data of the ceramic article to be prepared. In particular, the powder according to this exemplary embodiment is used in manufacturing methods employing powder bed fusion or coating methods. In this manufacturing process, the ceramic article is prepared by alternating steps (i) and (ii) multiple times.

[0074] Step (i): Placing the powder in the laser irradiation section

[0075] Step (ii): The step of curing the powder by irradiating it with laser light.

[0076] When molding ceramic articles using a powder bed fusion method, steps (i) and (ii) are performed by spreading powder according to this exemplary embodiment onto a substrate at a predetermined thickness and then irradiating the powder with laser light. When molding ceramic articles using a covering method, steps (i) and (ii) are performed by spraying powder according to this exemplary embodiment onto a predetermined portion and irradiating that predetermined portion with laser light.

[0077] While there are no restrictions on the wavelength of the laser light used in the shaping process, it is desirable to use a laser light with a diameter adjusted in a lens or fiber to a desired focal size, such as 10 μm to 2 mm. Focal size is one of the parameters affecting shaping accuracy. To achieve a shaping accuracy of 100 μm (0.1 mm), although this may vary depending on the circumstances, the desired linewidth should be commensurate with the shaping accuracy. The desired focal size should be a diameter of 100 μm or less. Whether the irradiating laser light is continuous or pulsed is irrelevant. As the laser light, lasers with wavelengths close to 1000 nm from sources such as Nd:YAG lasers and Yb fiber lasers are suitable. This is because the SiO composition exhibits particularly high absorption capacity with respect to light at wavelengths of approximately 1 μm.

[0078] Figure 2 This is a conceptual diagram of a 3D modeling device using the powder bed fusion method. (Example:) Figure 2 The description states that the three-dimensional modeling apparatus includes a powder lift 11, a modeling unit 13, a recoating unit 15, a laser light source 16, and a scanner unit 17 that scans the laser light generated by the laser light source 16. In the preparation of the ceramic product, the following operations are performed: First, powder 22 is raised by lifting the bottom 12 of the powder lift 11, and the platform 14 of the modeling unit 13, on which the substrate 19 is placed, is lowered by a predetermined distance. Next, the recoating unit 15 supplies powder 22 to the modeling unit 13 and spreads the powder 20 at a predetermined thickness in an area wider than the intended ceramic product. Based on slice data generated from the three-dimensional data of the ceramic product, the scanner unit 17 scans the laser light 18 generated by the laser light source 16, thereby directly drawing on the powder 20 spread on the substrate 19. The drawn area is sintered or melted and solidified. This process is repeated to obtain a ceramic product 21 with a laminated and solidified portion.

[0079] refer to Figure 3 The text describes a coating method. A coating method is a technique in which powder is ejected from multiple powder supply holes 222 in a coating nozzle 221, laser light 223 is irradiated onto an area where the powder is focused, and ceramic articles are sequentially shaped at desired locations. The coating method is characterized by its ability to shape on curved surfaces.

[0080] During the preparation process, the atmosphere can be controlled. In addition to an atmospheric atmosphere, an atmosphere in which the compounds included in the powder are readily reduced is also desirable, such as an inactive atmosphere including nitrogen or other rare gases, an atmosphere containing hydrogen, a reduced pressure atmosphere, or an oxygen atmosphere. Controlling such an atmosphere allows the use of powders containing compounds in oxidized or reduced states relative to stoichiometry in the preparation of ceramic products.

[0081] In the preparation process according to the present exemplary embodiment as described above, the powder according to the present exemplary embodiment is used, thereby enabling the ceramic article to be shaped in a stable manner and ensuring the shaping accuracy of the ceramic article.

[0082] Ceramic articles prepared using the powder according to this exemplary embodiment are not limited to crystalline inorganic materials. A portion or more than half of the ceramic article may be in an amorphous state, provided that desired physical properties are obtained. Alternatively, ceramic articles comprising regions approaching a metallic state can be prepared by reducing the powder using the above preparation process.

[0083] (Evaluation Method)

[0084] The porosity of ceramic products was evaluated using a method based on the Japanese Industrial Standard (JIS) R1634 regarding the measurement of sintered body density and open porosity of fine ceramics. Specifically, for three ceramic products prepared using the same material as the sample used to measure mechanical strength, the porosity of the ceramic products was calculated using {(W3-W1) / (W3-W2)}×100, where the dry mass of each ceramic product is W1, the mass of the ceramic product in water is W2, and the saturated mass of the ceramic product is W3, and the results were averaged.

[0085] The composition of powders or molded products is measured using inductively coupled plasma atomic emission spectrometry (ICP-AES). Example

[0086] Specific examples of powders according to this exemplary embodiment are described.

[0087] Ceramic products were prepared using powders 1 to 21, including silicon monoxide (SiO) and alumina (Al2O3) and silicon dioxide (SiO2) other than silicon monoxide, by a powder bed fusion method, and the porosity of the ceramic products was measured.

[0088] Powders 1 to 15 and 18 to 22 are prepared by stirring the following powders, weighed in the amounts described in Table 1, for 2 hours using a rock-type mixer.

[0089] Powder composed of Al2O3 particles (CB-A20S from Showa Denko Corporation): average particle size 20 μm

[0090] Powder composed of amorphous SiO2 particles (HS-304 from Nippon Steel Chemicals & Materials Co., Ltd.): average particle size 28 μm

[0091] Powdered SiO2 particles (SiO-P-002 from NER Corporation, Japan): average particle size 4μm

[0092] Al2O3 particles and SiO2 particles have a roughly spherical shape.

[0093] Each of powders 16 and 17 is prepared by the following steps. A slurry is prepared by weighing and mixing the following powders to achieve the composition ratios described in Table 2, and then dispersing the mixed powders in water. The prepared slurry is then used to prepare granular powder with an average particle size of 30 μm by a spray dryer method, and subsequently subjected to heat treatment at a temperature between 600°C and 800°C, thereby preparing granular powder composed of spherical secondary particles, wherein individual particles in the spherical secondary particles comprise Al2O3 particles and SiO2 particles.

[0094] Powder composed of Al2O3 particles (Taimicron TM-DA from Daming Chemical Industry): average particle size 0.17 μm

[0095] Powder composed of SiO2 particles (Seahoster W10 from Nippon Shokubai): average particle size 0.2 μm

[0096] The powder composed of SiO particles described above was added to the obtained granular powder, resulting in a powder with the composition ratios described in Table 2. The powder was then stirred for 10 minutes using a rocker mixer.

[0097] When the composition of powders 1 to 22 was analyzed, the components other than Al2O3, SiO2 and SiO in each powder were less than 1% by weight.

[0098] Next, ceramic articles were fabricated using each of the prepared powders, and the shaping accuracy and density of the ceramic articles were evaluated. The ceramic articles were fabricated using the DMP200 from the ProX series of 3D Systems, Inc., which incorporates a Yb fiber laser.

[0099] Through the above steps, a cuboid with a length of 40 mm, a width of 6 mm, and a height of 5 mm is prepared as a ceramic product. Using an Al2O3 plate as the substrate, the ceramic product is shaped by setting the thickness of each powder layer (reducing the value of the molding stage unit 14) to 20 μm. A laser beam with a focal size of 100 μm and a power of 270 W is irradiated onto the powder at a scanning speed of 500 mm / s.

[0100] Regions with a length of 40 mm and a width of 6 mm are drawn at 100 μm intervals, and the drawn regions are stacked to a height of 5 mm. Since each layer is approximately 20 μm thick, the powder includes particles with a thickness greater than or equal to the thickness of a single layer; however, these particles are removed when the powder is spread out during the initial stage of stacking. Due to laser irradiation, the powder layers melt and shrink in the thickness direction. Therefore, with repeated stacking, the apparent thickness of the powder layers gradually increases, eventually converging in the range of 67-133 μm. Therefore, there are no problems with use even if the average particle size of the powder to be used is greater than 20 μm of the powder layer.

[0101] The surface of the molded products was observed using an optical microscope. It was confirmed that ceramic articles prepared using each of powders 1 to 15 were molded with high precision, resulting in an average surface roughness (Ra) of less than 30 μm. It was confirmed that ceramic articles prepared using each of powders 1 to 7, powders 12 to 14, and powders 16 and 17 were molded with particularly excellent precision, containing 20% ​​by weight or less SiO, resulting in a surface Ra of 25 μm or less. In contrast, the ceramic article prepared using powder 22 had an Ra of 40 μm or greater for comparison, and did not achieve excellent molding precision. This is believed to be because powder 22 does not contain SiO particles, so light diffuses within the powder when irradiated with laser light, causing the powder to melt or sinter over a large area.

[0102] Tables 1 and 2 illustrate the evaluation results of density. For the density of each ceramic product, porosity was measured, and density was categorized into the following four levels: If the porosity is 11% or less, density is categorized as A. If the porosity is greater than 11% and 14% or less, density is categorized as B. If the porosity is greater than 14% and 16% or less, density is categorized as C. If the porosity is greater than 16%, density is categorized as D.

[0103] In the above classification, A represents a product in an extremely dense state. B represents a product in a relatively dense state. C represents a product in a dense state. D represents a product in a porous state or a state containing many cracks.

[0104] [Table 1]

[0105]

[0106]

[0107] [Table 2]

[0108]

[0109] Each shaped product produced using each of Powders 1 to 17 is a dense body classified into denseness A to C. In particular, the denseness of the shaped products using each of Powders 1 to 8, Powders 10 to 13, and Powders 16 and 17 (which satisfy z≤20 and y<x+z) is classified as A or B, indicating extremely excellent or excellent denseness. In contrast, the denseness of the shaped products produced for comparison using each of Powders 18 to 20 (which satisfy x<20) is classified as D, indicating a porous body.

[0110] In each of Comparative Examples 1 to 3, when a molten material having a spherical shape heated and melted by laser irradiation is formed through solidification, many pores remain in the molten material, and a porous ceramic article is obtained. This is considered to be because the viscosity of molten SiO2 is higher than the viscosity of Al2O3. In Comparative Example 4, the reason for the high porosity is considered to be that highly anisotropic crystal grains are formed when Al2O3 melts and solidifies, resulting in a large number of voids.

[0111] In a shaped product produced for comparison using Powder 21 that does not contain SiO2, a plurality of large cracks with a width of 10 μm or more are present, and the denseness is low, that is, classified as C. This is considered to be because the stress relaxation effect of SiO2 is not obtained when highly anisotropic Al2O3 melts and solidifies.

[0112] When the shaped product of each Comparative Example, which contains many cracks and has a denseness rated as C, is subjected to heat treatment at about 1700°C, an effect of repairing the cracks is observed.

[0113] Although the shaping method described above utilizes heat generated by SiO particles serving as an absorber that absorbs laser light to melt and then solidify particles of other metal oxides such as Al2O3 particles or SiO2 particles, the powder according to the present invention is not limited to this method. The powder according to the present invention can also be used in the following shaping method: a resin binder is added to the powder according to the present invention, and the resin binder is melted by the heat generated by the SiO particles that absorb laser light and then solidified, so as to bind the particles with the resin binder. The resin binder may be added to the powder as particles independent of other particles, or may be attached to the surfaces of Al2O3 particles, SiO2 particles, or SiO particles.

[0114] The powder according to the present invention is capable of producing dense ceramic articles with high precision, without using a rare earth component as an absorber that is used in additive manufacturing methods for shaping by laser light irradiation. The powder according to the present invention can provide low-cost ceramic articles to fields that require complex shapes.

[0115] This invention is not limited to the exemplary embodiments described above, and can be changed and modified in various ways without departing from the spirit and scope of the invention. Therefore, the following claims are appended to disclose the scope of the invention.

[0116] This application claims the benefits of Japanese Patent Application No. 2021-067069, filed on April 12, 2021, and Japanese Patent Application No. 2022-061812, filed on April 1, 2022, the entire contents of which are incorporated herein by reference.

Claims

1. An oxide powder for use in an additive manufacturing method for forming a shape by laser irradiation, the powder comprising: silicon monoxide particles; and other particles different from the silicon monoxide particles, wherein the other particles include at least one type of particles selected from the group consisting of alumina particles, silica particles, and oxide particles containing silicon and aluminum as constituent elements, and wherein when the other particles are converted into oxides represented by Al₂O₃ and SiO₂, x representing the mass fraction of Al₂O₃, y representing the mass fraction of SiO₂, and z representing the mass fraction of SiO in the entire powder satisfy the following relationships: 20≤x<99.8, 0<y≤80, and 0.5≤z≤20。 2. The powder according to claim 1, wherein the powder satisfies 90≤x+y+z.

3. The powder according to claim 1, wherein the powder satisfies 95≤x+y+z.

4. The powder according to claim 1, wherein the powder satisfies 1.0≤y<50.

5. The powder according to claim 1, wherein the powder satisfies 3.0≤y<50.

6. The powder according to claim 1, wherein the powder satisfies y<x+z.

7. The powder according to any one of claims 1 to 6, comprising SiO particles as independent particles.

8. The powder according to claim 7, wherein the average particle size of the silicon monoxide particles is one fifth or less of the average particle size of the other particles.

9. The powder according to claim 7, wherein the average particle size of the silicon monoxide particles is 1 micrometer (μm) or more and 10 μm or less.

10. The powder according to claim 9, wherein the average particle size of the silica particles is 5 micrometers (μm) or more and 200 μm or less, and the silica particles include amorphous SiO₂.

11. The powder according to any one of claims 1 to 6, wherein the powder comprises secondary particles of Al₂O₃ particles and SiO₂ particles.

12. A method for producing a ceramic article, the method comprising: performing multiple times placing a powder, and irradiating the powder with a laser to cure the powder, wherein the powder comprises silicon monoxide particles and other particles different from the silicon monoxide particles, wherein the other particles include at least one type of particles selected from the group consisting of alumina particles, silica particles, and oxide particles containing silicon and aluminum as constituent elements, and wherein when the other particles are converted into oxides represented by Al₂O₃ and SiO₂, x representing the mass fraction of Al₂O₃, y representing the mass fraction of SiO₂, and z representing the mass fraction of SiO in the entire powder satisfy the following relationships: 20≤x<99.8, 0<y≤80, and 0.5≤z≤20。 13. The method for producing a ceramic article according to claim 12, wherein the powder satisfies 90≤x+y+z.

14. The method for producing a ceramic article according to claim 12, wherein the powder satisfies 95≤x+y+z.

15. The method for producing a ceramic article according to claim 12, wherein the powder satisfies 1.0≤y<50.

16. The method for producing a ceramic article according to claim 12, wherein the powder satisfies y<x+z.

17. The method for preparing ceramic articles according to any one of claims 12 to 16, wherein SiO particles are used as independent particles.

18. The method for preparing a ceramic article according to any one of claims 12 to 16, wherein a laser is irradiated based on slice data generated from three-dimensional data of the ceramic article.

19. The method for preparing ceramic articles according to any one of claims 12 to 16, wherein the laser is light from an Nd:YAG laser or a Yb fiber laser.

Citation Information

Patent Citations

  • Powder for ceramic shaping, ceramic shaped article, and method for manufacturing the same

    JP2019019051A

  • Brake device of sliding door

    JP2021067069A

  • Surgical instrument

    JP2022061812A

  • Inorganic material powder, and method for producing structure

    JP2020100141A