A method for preparing rutile from high-titanium blast furnace slag

By converting titanium-containing blast furnace slag into rutile TiO2 through roasting and separation processes, the problems of low resource utilization and unstable quality in existing technologies are solved, and efficient and economical titanium resource recovery is achieved.

CN117138946BActive Publication Date: 2026-11-10GUANGXI UBRIDGE NEW MATERIAL TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311149086.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-06
Publication Date
2026-11-10
Estimated Expiration
2043-09-06

AI Technical Summary

Technical Problem

Existing technologies require large amounts of acid and alkali when processing titanium-containing blast furnace slag, resulting in complex acid hydrolysis solutions and unstable quality of the prepared rutile, and the titanium resources are not effectively utilized.

Method used

High-purity rutile ore is prepared by roasting titanium-containing blast furnace slag with pyrite and additives at a certain temperature, and converting it into rutile-type TiO2 through oxidation and reduction roasting. Impurities are then separated by magnetic separation, electrostatic separation and flotation processes.

Benefits of technology

This method enables efficient utilization of waste resources, reduces production costs, improves the recovery rate and purity of rutile, reduces the amount of composite collectors used, and obtains high-purity rutile concentrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117138946B_ABST
    Figure CN117138946B_ABST
Patent Text Reader

Abstract

This invention relates to a method for preparing rutile from high-titanium blast furnace slag. The method employs a combined process flow of oxidative roasting—wet weak magnetic separation—reduction roasting—electrostatic separation—flotation, which effectively utilizes valuable minerals such as titanium dioxide and iron tetroxide produced after the reaction of blast furnace slag and pyrite. Through the initial magnetic and electrostatic separation processes, the amount of rutile required for subsequent flotation is significantly reduced, thus minimizing the amount of rutile collector used while ensuring rutile quality and recovery rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metallurgy and mineral processing technology, and specifically relates to a method for preparing rutile from high-titanium blast furnace slag. Background Technology

[0002] Titanium-containing blast furnace slag is a byproduct of blast furnace smelting of vanadium-titanium magnetite, typically containing 20% ​​to 25% titanium dioxide. Currently, the comprehensive utilization rate of titanium-containing blast furnace slag resources is low. It is mainly used to produce low-end building materials such as slag cement, sanitary ware, and alkali-resistant mineral wool. The titanium resources within the slag have not been effectively utilized, and a large amount of titanium-containing blast furnace slag remains idle, with a total stock exceeding 80 million tons and increasing by more than 3.6 million tons annually. This wastes both land and resources, urgently requiring development and utilization.

[0003] For the recovery and utilization of titanium in titanium-containing blast furnace slag, patent CN107686897A provides a method for extracting titanium from titanium-containing blast furnace slag. This method uses a process of fine grinding and magnetic separation, grinding and screening, acid leaching, static stratification, water washing and drying, and calcination to obtain high-grade titanium dioxide. Patent CN103952568A provides a method for treating titanium-containing blast furnace slag. This method is particularly suitable for titanium-containing blast furnace slag obtained from iron smelting of vanadium-titanium magnetite mined in the Panzhihua area. It uses acid leaching, especially multi-stage acid leaching, to leach the slag and obtain acid leaching solution. Through an extraction process, useful metals such as titanium, aluminum, calcium, magnesium, manganese, iron, chromium, and vanadium are obtained from the acid leaching solution.

[0004] The existing technologies described above require large amounts of acid and alkali to process titanium-containing blast furnace slag, and the acid hydrolysis solution contains a large number of Al, Mg, Fe, and Ca ions, making the hydrolysis process complex and resulting in unstable TiO2 quality. Therefore, to reduce energy consumption and improve economic efficiency in the mineralization process, it is crucial to select suitable additives and simultaneously recover valuable titanium elements from the titanium-containing blast furnace slag. Summary of the Invention

[0005] This invention addresses key issues in existing technologies, such as the need for large amounts of acid and alkali in processing titanium-containing blast furnace slag and the unstable quality of the prepared rutile. It provides a method for preparing rutile from high-titanium blast furnace slag. This method involves roasting titanium-containing blast furnace slag with pyrite (mainly FeS2) and additives at a specific temperature. The perovskite and low-valent titanium oxides in the titanium-containing blast furnace slag are sulfated and oxidized, respectively, converting the titanium component into rutile-type TiO2. The calcium and magnesium elements in the blast furnace slag are converted into sulfates.

[0006] According to one aspect of the present invention, a method for preparing rutile from high-titanium blast furnace slag is provided, comprising the following steps: S1. Crushing and grinding titanium-containing blast furnace slag: Grind the blast furnace slag to a particle size of less than 0.15 mm, mix the titanium-containing blast furnace slag with pyrite and additives, introduce oxygen, and oxidize and roast at 700-900℃ for 2-3 hours to obtain a solid product. S2. Add an appropriate amount of carbon powder to the solid product obtained in step S1, perform high-temperature reduction roasting in a reduction roasting furnace, cool and crush, and then perform weak magnetic separation through a wet magnetic separator. The magnetic product is magnetite, and the tailings are scavenged. S3. The non-magnetic product obtained in step S2 is introduced into an electrostatic separator for a rough electrostatic separation. The conductive product obtained from the rough electrostatic separation is then subjected to a fine electrostatic separation. The finely separated conductive product is rutile ore, and the non-conductive product is gangue mineral. S4. The rutile ore obtained after electrostatic separation in step S3 is slurry prepared to obtain a slurry with a concentration of 15% to 30%. The slurry is fed into a flotation cell, and a rutile composite collector and a frother are added to the slurry. After one roughing and one cleaning process, rutile concentrate is obtained.

[0007] In step S1, the perovskite and low-valent titanium oxides in the titanium-containing blast furnace slag are sulfated and oxidized respectively, converting the titanium component into rutile TiO2. Since the oxidation and combustion of pyrite produces a large amount of sulfur dioxide, the calcium and magnesium elements in the blast furnace slag can be converted into sulfates.

[0008] In some embodiments, the additive in step S1 is phosphorus pentoxide, and the mass ratio of blast furnace slag to pyrite and additive is: blast furnace slag: pyrite: phosphorus pentoxide = 1:0.3:0.3. The role of the phosphorus pentoxide additive is as an oxidizing agent and acidifying agent, promoting the oxidation of pyrite, destroying the stable phases in the original blast furnace slag, and allowing calcium and magnesium elements to separate from the silicate phase and participate in the reaction.

[0009] In some embodiments, the carbon powder particle size in step S2 is within 0.1 mm, and its amount is 3% to 5% of the mass of the solid product. After the carbon powder is mixed with the solid product, a layer of +120 mesh large-particle coal is spread on its surface. The high-temperature roasting temperature is 850°C, the weak magnetic separation magnetic field strength is 0.15T, and the scavenging magnetic field strength is 0.35T.

[0010] In some embodiments, step S3, electrostatic separation, is high-voltage electrostatic separation, with a separation voltage of 16–23 kV, a separator roller speed of 120–140 rpm, and a separation temperature of 50–60°C. Electrostatic separation is used to select rutile with high conductivity. To separate impurities as much as possible, two electrostatic separations are required: a roughing separation and a finishing separation. Specifically, the electrostatic voltage during roughing is higher than that during finishing. The higher voltage during roughing ensures that all conductors are selected, while the lower voltage during finishing selects the rutile phase with high conductivity.

[0011] In some embodiments, in step S4, the roughing step is as follows: sulfuric acid is added to the slurry to adjust the pH of the slurry to 5.0~5.6, water glass is added as an inhibitor, rutile composite collector is added, and the mixture is stirred for 4 minutes; frother No. 2 oil is added, the mixture is stirred for 2 minutes, and aeration is carried out for flotation for 4 minutes to perform roughing; the cleaning step is as follows: water glass and rutile composite collector are added to the roughing product for secondary cleaning, and the cleaned product is collected.

[0012] In some embodiments, during the roughing process in step S4, the amount of water glass added is 200 g / t, the amount of rutile composite collector added is 450 or 500 g / t, and the amount of No. 2 oil added is 60 g / t, based on the weight of the slurry; during the cleaning process, the amount of water glass added is 200~300 g / t, and the amount of rutile composite collector added is 550 g / t, based on the weight of the slurry.

[0013] In some embodiments, the rutile composite collector is a mixture of dodecyl succinic acid, sodium phenylisothiourea acetate, sodium lignosulfonate, propylene glycol, n-octanol, and ammonium chloride in a mass ratio of 3:3:2:1:1:1. Dodecyl succinic acid regulates the pH, sodium lignosulfonate synergizes with sodium dodecyl succinate to supplement rutile collection, propylene glycol acts as a solvent, and ammonium chloride enhances the adsorption capacity with the rutile phase. The mixed collector, composed of these materials, exhibits better collection performance than a collector containing only sodium sulfonate.

[0014] For the preparation process of this invention, the main factors affecting titanium recovery are the roasting temperature and time of pyrite and blast furnace slag mixing, which affect the proportion of perovskite phase transforming into rutile phase. The preparation process of this invention ensures the separation of rutile phase from other phases by controlling the amount of pyrite and additives, and the oxidative roasting temperature, and then improves titanium recovery by separating the gangue phase through electrostatic separation and flotation.

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The raw materials for this process are blast furnace slag and pyrite, which are widely available, thus achieving effective utilization of waste, reducing environmental pollution, and saving production costs.

[0016] 2. This invention employs a combined process flow of oxidative roasting—wet weak magnetic separation—reduction roasting—electrostatic separation—flotation, which effectively utilizes valuable minerals such as titanium dioxide and iron tetroxide obtained from the reaction of blast furnace slag and pyrite. Through the initial magnetic and electrostatic separation processes, the amount of rutile required for subsequent flotation is significantly reduced, ensuring rutile quality and recovery rate while decreasing the amount of rutile composite collector used.

[0017] 3. Obtain rutile concentrate with TiO2 content greater than 93% and rutile mineral recovery rate exceeding 87%; magnetite with total iron content greater than 65% and iron recovery rate greater than 92%. Attached Figure Description

[0018] Figure 1 This is a schematic diagram of the process flow of the present invention. Detailed Implementation

[0019] The present invention will be further described in detail below with reference to specific embodiments. Unless otherwise specified, all raw materials are commercially available. Among them, foaming agent 2# oil is a complex higher alcohol with the molecular formula R-alkane group, which is divided into two types: pine alcohol oil and chemical oil. It is a conventional foaming agent in flotation.

[0020] Example 1 In this embodiment, the blast furnace slag came from a company in Panzhihua. The mass fraction of each component in the slag is shown in Table 1. Table 1. Mass fraction of each component in blast furnace slag

[0021] The mineral processing flow in this embodiment is as follows: Figure 1 As shown, the specific steps are as follows: (1) Crush and grind the blast furnace slag to a particle size of less than 0.15 mm. Mix the titanium-containing blast furnace slag with pyrite and phosphorus pentoxide in a mass ratio of 1:0.3:0.3. Introduce oxygen and oxidize and roast at 800°C for 3 hours to obtain a solid product. (2) Add carbon powder with a particle size of less than 0.1 mm to the solid product obtained in step (1). The amount of carbon powder added is 5% of the mass of the solid product. After mixing the carbon powder with the solid product, a layer of +120 mesh large-particle coal is spread on its surface. The product is heated to 850°C in a reduction roasting furnace for high-temperature reduction roasting. After cooling, it is crushed and then weakly magnetically separated by a wet magnetic separator with a magnetic field strength of 0.15T. The magnetic product is magnetite. The tailings are scavenged once with a scavenging magnetic field strength of 0.35T. (3) The non-magnetic product obtained in step (2) (i.e. the non-magnetic product obtained by weak magnetic separation and scavenging) is introduced into an electrostatic separator for a first electrostatic roughing separation. The electrostatic separation voltage is 23kV, the rotation speed of the electrostatic separator roller is 140rpm, and the electrostatic separation temperature is 60℃. The conductor product obtained by the electrostatic roughing separation is then subjected to a second electrostatic cleaning separation. The electrostatic separation voltage is 16kV, the rotation speed of the electrostatic separator roller is 130rpm, and the electrostatic separation temperature is 60℃. The cleaned conductor product is rutile ore. (4) The rutile ore obtained after electrostatic separation in step (3) is mixed with water to obtain a slurry with a slurry concentration of 25%. The slurry is sent to the flotation cell, sulfuric acid is added to adjust the pH of the slurry to 5.2, water glass is added as an inhibitor (200 g / t), and a mixture of dodecyl succinic acid, sodium phenylisothiourea acetate, sodium lignosulfonate, propylene glycol, n-octanol, and ammonium chloride (mass ratio of 3:3:2:1:1:1) is added as a rutile composite collector (addition amount of 450 g / t). Stir for 4 min; add 60 g / t of frother 2# oil, stir for 2 min, and aerate for flotation for 4 min for roughing; add water glass (300 g / t) and rutile composite collector (550 g / t) to the roughing product for cleaning, collect the cleaned product, and obtain rutile concentrate.

[0022] In this embodiment, the TiO2 content of the rutile concentrate was 93.3% and the rutile mineral recovery rate was 88.6%; the total iron content of the magnetite was 65.7% and the iron recovery rate was 92.7%.

[0023] Example 2 In this embodiment, the blast furnace slag came from a company in Panzhihua, and the mass fraction of each component in the slag is shown in Table 2.

[0024] Table 2 Mass fraction of each component in blast furnace slag

[0025] The mineral processing flow of this embodiment is roughly as follows: Figure 1 As shown, the specific steps are as follows: (1) Crush and grind the blast furnace slag to a particle size of less than 0.15 mm. Mix the titanium-containing blast furnace slag with pyrite and phosphorus pentoxide in a mass ratio of 1:0.3:0.2. Introduce oxygen and oxidize and roast at 800°C for 3 hours to obtain a solid product. (2) Add carbon powder with a particle size of less than 0.1 mm to the solid product obtained in step (1). The amount of carbon powder added is 4% of the mass of the solid product. After mixing the carbon powder with the solid product, a layer of +120 mesh large-particle coal is spread on its surface. The product is heated to 850°C in a reduction roasting furnace for high-temperature reduction roasting. After cooling, it is crushed and then weakly magnetically separated by a wet magnetic separator with a magnetic field strength of 0.15T. The magnetic product is magnetite. The tailings are scavenged once with a scavenging magnetic field strength of 0.35T. (3) The non-magnetic product obtained in step (2) is introduced into an electrostatic separator for a first electrostatic roughing process. The electrostatic high voltage is 20kV, the speed of the electrostatic separator roller is 140rpm, and the electrostatic temperature is 60℃. The conductor product obtained from the electrostatic roughing process is then subjected to a second electrostatic cleaning process. The electrostatic voltage is 16kV, the speed of the electrostatic separator roller is 130rpm, and the electrostatic temperature is 60℃. The cleaned conductor product is rutile ore. (4) The rutile ore obtained after electrostatic separation in step (3) is mixed with water to obtain a slurry with a slurry concentration of 20%. The slurry is sent to the flotation cell, sulfuric acid is added to adjust the pH of the slurry to 5.5, water glass is added as an inhibitor (200 g / t), and a mixture of dodecyl succinic acid, sodium phenylisothiourea acetate, sodium lignosulfonate, propylene glycol, n-octanol and ammonium chloride (mass ratio of 3:3:2:1:1:1) is added as a rutile composite collector (addition amount of 500 g / t). Stir for 4 min; add 60 g / t of frother 2# oil, stir for 2 min, aerate for flotation for 4 min, and perform roughing; add water glass (300 g / t) and rutile composite collector (550 g / t) to the roughing product for secondary cleaning, collect the cleaned product, and obtain rutile concentrate.

[0026] In this embodiment, the TiO2 content of the rutile concentrate was 92.7% and the rutile mineral recovery rate was 88.9%; the total iron content of the magnetite was 65.1% and the iron recovery rate was 92.3%.

[0027] Example 3 In this embodiment, the blast furnace slag came from a company in Xichang. The mass fraction of each component in the slag is shown in Table 3. Table 3 Mass fraction of each component in blast furnace slag

[0028] The mineral processing flow of this embodiment is roughly as follows: Figure 1 As shown, the specific steps are as follows: (1) Crush and grind the blast furnace slag to a particle size of less than 0.15 mm. Mix the titanium-containing blast furnace slag with pyrite and phosphorus pentoxide in a mass ratio of 1:0.3:0.3. Introduce oxygen and oxidize and roast at 850°C for 3 hours to obtain a solid product. (2) Add carbon powder with a particle size of less than 0.1 mm to the solid product obtained in step (1). The amount of carbon powder added is 4% of the mass of the solid product. After mixing the carbon powder with the solid product, a layer of +120 mesh large-particle coal is spread on its surface. The product is heated to 850°C in a reduction roasting furnace for high-temperature reduction roasting. After cooling, it is crushed and then weakly magnetically separated by a wet magnetic separator with a magnetic field strength of 0.15T. The magnetic product is magnetite. The tailings are scavenged once with a scavenging magnetic field strength of 0.35T. (3) The non-magnetic product obtained in step (2) is introduced into an electrostatic separator for a first electrostatic roughing process. The electrostatic high voltage is 22kV, the speed of the electrostatic separator roller is 140rpm, and the electrostatic temperature is 60℃. The conductor product obtained from the electrostatic roughing process is then subjected to a second electrostatic cleaning process. The electrostatic voltage is 16kV, the speed of the electrostatic separator roller is 130rpm, and the electrostatic temperature is 60℃. The cleaned conductor product is rutile ore. (4) The rutile ore obtained after electrostatic separation in step (3) is mixed with water to obtain a slurry with a slurry concentration of 20%. The slurry is sent to the flotation cell, sulfuric acid is added to adjust the pH of the slurry to 5.5, water glass is added as an inhibitor (200 g / t), and a mixture of dodecyl succinic acid, sodium phenylisothiourea acetate, sodium lignosulfonate, propylene glycol, n-octanol, and ammonium chloride (mass ratio of 3:3:2:1:1:1) is added as a rutile composite collector (addition amount of 500 g / t). Stir for 4 min; add 60 g / t of frother 2# oil, stir for 2 min, and aerate for flotation for 4 min for roughing; add water glass (300 g / t) and rutile composite collector (550 g / t) to the roughing product for cleaning, collect the cleaned product, and obtain rutile concentrate.

[0029] In this embodiment, the TiO2 content of the rutile concentrate was 91.8% and the rutile mineral recovery rate was 89.2%; the total iron content of the magnetite was 65.7% and the iron recovery rate was 92.1%.

[0030] Example 4 In this embodiment, the blast furnace slag came from a company in Xichang. The mass fraction of each component in the slag is shown in Table 4. Table 4 Mass fraction of each component in blast furnace slag

[0031] The mineral processing flow of this embodiment is roughly as follows: Figure 1 As shown, the specific steps are as follows: (1) Crush and grind the blast furnace slag to a particle size of less than 0.15 mm. Mix the titanium-containing blast furnace slag with pyrite and phosphorus pentoxide in a mass ratio of 1:0.3:0.3. Introduce oxygen and oxidize and roast at 830°C for 3 hours to obtain a solid product. (2) Add carbon powder with a particle size of less than 0.1 mm to the solid product obtained in step (1). The amount of carbon powder added is 5% of the mass of the solid product. After mixing the carbon powder with the solid product, a layer of +120 mesh large-particle coal is spread on its surface. The product is heated to 850°C in a reduction roasting furnace for high-temperature reduction roasting. After cooling, it is crushed and then weakly magnetically separated by a wet magnetic separator with a magnetic field strength of 0.15T. The magnetic product is magnetite. The tailings are scavenged once with a scavenging magnetic field strength of 0.35T. (3) The non-magnetic product obtained in step (2) is introduced into an electrostatic separator for a first electrostatic roughing process. The electrostatic high voltage is 22kV, the speed of the electrostatic separator roller is 140rpm, and the electrostatic temperature is 60℃. The conductor product obtained from the electrostatic roughing process is then subjected to a second electrostatic cleaning process. The electrostatic voltage is 16kV, the speed of the electrostatic separator roller is 130rpm, and the electrostatic temperature is 60℃. The cleaned conductor product is rutile ore. (4) The rutile ore obtained after electrostatic separation in step (3) is mixed with water to obtain a slurry with a slurry concentration of 20%. The slurry is sent to the flotation cell, sulfuric acid is added to adjust the pH of the slurry to 5.5, water glass is added as an inhibitor (200 g / t), and a mixture of dodecyl succinic acid, sodium phenylisothiourea acetate, sodium lignosulfonate, propylene glycol, n-octanol, and ammonium chloride (mass ratio of 3:3:2:1:1:1) is added as a rutile composite collector (addition amount of 500 g / t). Stir for 4 min; add 60 g / t of frother 2# oil, stir for 2 min, and aerate for flotation for 4 min for primary selection; add water glass (300 g / t) and rutile composite collector (550 g / t) to the primary selection product for secondary selection, collect the selected product, and obtain rutile concentrate.

[0032] In this embodiment, the TiO2 content of the rutile concentrate was 93.1% and the rutile mineral recovery rate was 88.6%; the total iron content of the magnetite was 65.5% and the iron recovery rate was 92.7%.

[0033] The above descriptions are merely some embodiments of the present invention. Those skilled in the art can make various modifications and improvements without departing from the inventive concept of the present invention, and these all fall within the scope of protection of the present invention.

Claims

1. A method for preparing rutile from high-titanium blast furnace slag, characterized in that, The steps are as follows: S1. Crushing and grinding titanium-containing blast furnace slag: The blast furnace slag is finely ground to a particle size of less than 0.15 mm. The titanium-containing blast furnace slag is mixed with pyrite and additives, oxygen is blown in, and the mixture is oxidized and roasted at 800-900℃ for 2-3 hours to obtain a solid product. The additive is phosphorus pentoxide. S2. Add the solid product obtained in step S1 to carbon powder, reduce and roast it in a reduction roasting furnace, cool it and then crush it, and then perform weak magnetic separation. The tailings are then scavenged. S3. The non-magnetic product obtained in step S2 is subjected to electrostatic roughing, and the conductor product obtained from the electrostatic roughing is then subjected to electrostatic finening. The fined conductor product is rutile ore. S4. The rutile ore obtained after electrostatic separation in step S3 is slurry prepared to obtain a slurry with a concentration of 15% to 30%. The slurry is fed into a flotation cell, and a rutile composite collector and a frother are added to the slurry. After roughing and cleaning, rutile concentrate is obtained. The rutile composite collector is obtained by mixing dodecyl succinic acid, sodium phenylisothiourea acetate, sodium lignosulfonate, propylene glycol, n-octanol, and ammonium chloride.

2. The method for preparing rutile from high-titanium blast furnace slag according to claim 1, characterized in that, The mass ratio of blast furnace slag to pyrite and additives in step S1 is 1:0.3:0.3 or 1:0.3:0.

2.

3. The method for preparing rutile from high-titanium blast furnace slag according to claim 1, characterized in that, In step S2, the reduction roasting temperature is 850~900℃, the weak magnetic separation magnetic field strength is 0.15~0.2T, and the scavenging magnetic field strength is 0.35~0.4T.

4. The method for preparing rutile from high-titanium blast furnace slag according to claim 1, characterized in that, Step S3 is a high-voltage electrostatic separation, with an electrostatic separation voltage of 16-23kV, an electrostatic separator roller speed of 120-140rpm, and an electrostatic separation temperature of 50-60℃.

5. A method for preparing rutile from high-titanium blast furnace slag according to claim 4, characterized in that, In step S4, the specific steps for roughing are as follows: add sulfuric acid to the slurry to adjust the pH value of the slurry to 5.0~5.6, add water glass as an inhibitor, add rutile composite collector, and stir for 4~5 minutes; add frother No. 2 oil, stir for 2~3 minutes, aerate for flotation for 4~5 minutes, and perform roughing.

6. The method for preparing rutile from high-titanium blast furnace slag according to claim 5, characterized in that, In step S4, during roughing, the amount of water glass added is 200 g / t, the amount of rutile composite collector added is 450 or 500 g / t, and the amount of No. 2 oil added is 60 g / t, based on the weight of the slurry.

7. A method for preparing rutile from high-titanium blast furnace slag according to claim 5, characterized in that, In step S4, the specific steps for fine selection are as follows: add water glass and rutile composite collector to the rough product for secondary fine selection, and collect the fine product.

8. A method for preparing rutile from high-titanium blast furnace slag according to claim 7, characterized in that, During step S4, when refining the mineral slurry, the amount of water glass added is 200~300g / t, and the amount of rutile composite collector added is 550g / t.

Citation Information

Patent Citations

  • Method for treating titaniferous blast furnace slag

    CN103952568A

  • Method for extracting titanium from titanium-containing blast furnace slag

    CN107686897A

  • Ilmenite treatment method

    CN111944991A

  • Efficient resource utilization method for rutile ore

    CN113369009A