Process for the preparation of pure lithium oxide
By compacting and mixing lithium carbonate with carbon and using corrosion-resistant container materials, the problems of high equipment costs, significant safety hazards, and product inhomogeneity in lithium oxide production have been solved, enabling the economical production of high-purity lithium oxide.
Patent Information
- Application Number
- CN202280010078.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-01-14
- Filing Date
- 2022-01-03
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-01-03
AI Technical Summary
Existing technologies for producing lithium oxide suffer from problems such as high equipment costs, significant safety hazards, product inhomogeneity, and severe elemental carbon contamination, making it difficult to economically obtain high-purity, free-flowing powder form of lithium oxide.
By mixing lithium carbonate and carbon in a specific molar ratio and compacting them to form a carbon coating, followed by calcination in the range of 600 to 1200°C, using container materials that are resistant to high temperatures and alkali corrosion, controlling the reaction atmosphere, and optimizing energy input and temperature conditions, the full reaction of lithium carbonate and carbon can be achieved.
This process produces high-purity, highly uniform, and free-flowing lithium oxide powder, significantly reducing elemental carbon pollution and improving production efficiency and product quality.
Abstract
Description
Technical Field
[0001] This invention relates to an economical method for producing pure lithium oxide in powder form and its uses.
[0002] Lithium oxide is currently used as a raw material in the production of glass, glass-ceramics, ceramics, and lithium-ion battery cathodes. Additionally, it can be used to produce lithium hydroxide. Background Technology
[0003] Lithium oxide can be produced by the thermal decomposition of Li₂CO₃ at approximately 1000°C (i.e., molten lithium carbonate) in a platinum crucible under a pressure of up to 267 Pa (2000 μm Hg) according to the following formula:
[0004] Li2CO3→Li2O+CO2 (1).
[0005] This manufacturing method produces bulk oxides that must be ground before further use (DS Appleton, RB Poeppel in: Advances in Ceramics, Vol. 25, "Fabrication and properties of lithium ceramics," ed. IJ Hastings and G.W. Hollenberg, 1989, 111-116). In <10 -5 At extremely low pressures, thermal decomposition may also occur below the melting point of Li₂CO₃ (T. Takahashi, H. Watanabe, Fusion Eng. Design 8 (1989) 399-405). However, such low pressures are economically impractical for technical equipment.
[0006] In addition, it is known that lithium carbonate can be reduced using hydrogen in the temperature range of 400-725°C according to the following formula:
[0007] Li2CO3 + H2 → Li2O + H2O + CO (2)
[0008] (JP 2014047117 A). This process has safety-related drawbacks due to the use of explosive hydrogen at high temperatures.
[0009] Finally, carbon black can be used as a reducing agent for lithium carbonate (J.-W. Kim, H.-G. Lee, Metallurgical Mat. Trans. B, 32B (2001) 17-24). Carbothermal decomposition does not require a vacuum, but can be carried out in an Ar atmosphere above about 720°C according to the following reaction in an alumina crucible:
[0010] Li2CO3 + C → Li2O + 2CO (3)
[0011] The disadvantage is the strong corrosive effect of the carbonate melt on the alumina container material used. Carbothermal decomposition using coke, charcoal, activated carbon, sugar, synthetic graphite, and similar materials can also be carried out at temperatures above 500°C but below 720°C, thus avoiding the melting of lithium carbonate (JP 2012121780 A). In this case, a relatively long reaction time must be expected. Similarly, lithium carbonate embedded in polymer resins can be reduced to particulate lithium oxide in the temperature range of 600 to 700°C (JP 11209122a). The disadvantage is that the reaction time is at least 6 hours, and the oxide is obtained in particulate form, requiring prior grinding for further use, such as as a raw material for the production of lithium-ion battery electrode materials.
[0012] WO 18114760 A1 also describes a method for producing lithium oxide in powder form from lithium carbonate and elemental carbon or a carbon source that forms elemental carbon under reaction conditions in the temperature range of 720 to 1200 °C, wherein the reaction is carried out under substantially oxygen-free conditions, and wherein the chemical reaction is carried out in a container composed of glassy carbon, lithium aluminate, carbon-coated ceramic, or C-coated quartz glass or tantalum on the surface in contact with the product. In a preferred embodiment of the method, the reaction is carried out in a fluidized bed or moving bed reactor, or under vacuum conditions (10-5000 Pa (0.1-50 mbar)), or in a gas atmosphere that is inert or substantially inert to carbon, at a temperature of about 50 to 2 x 10⁻⁶ °C. 5 Under pressures of Pa (0.5 to 2 bar), a mixture of nitrogen or a rare gas (preferably argon) or an inert gas atmosphere is used. A disadvantage of the method described in WO 18114760A1 is that the reaction product Li₂O partially agglomerates and is contaminated with elemental carbon. Typically, products ranging from gray to black are obtained, and these products appear optically inhomogeneous. Summary of the Invention
[0013] The present invention aims to provide a simple process for producing high-purity, free-flowing lithium oxide in powder form using lithium carbonate as a basic raw material, particularly a product with elemental carbon contamination of <0.2 wt.%.
[0014] According to the present invention, the objective is achieved by a process for preparing lithium oxide, wherein the production of lithium oxide is carried out by...
[0015] - Determination of median particle size (D) by laser diffraction 50 Lithium carbonate with a particle size ranging from 2 to 150 μm, and
[0016] -Median primary particle size (D) determined by electron microscopy 50 Carbon in powder form with a particle size <1 μm
[0017] Calcination is carried out in a temperature range of 600 to 1200°C, wherein the process is characterized by:
[0018] Prior to calcination, lithium carbonate and carbon are mixed and compacted at a molar ratio of 1:0.1 to 1:1.2, thereby causing carbon particles to surround lithium carbonate particles and form a coating, and the resulting mixture has a bulk density that is at least 5% higher than that of an uncompacted mixture of lithium carbonate and carbon particles, wherein the bulk density is determined in accordance with EN ISO 697.
[0019] Therefore, in the lithium oxide production process, lithium carbonate reacts with finely powdered elemental carbon at a temperature range of 600 to 1200°C. The two reactants are thoroughly premixed by compaction before the pyrolysis process, resulting in a bulk density increase of at least 5%, preferably at least 15%, compared to the bulk density of the two starting materials mixed without compaction. The bulk density of the two raw materials without compaction is determined by homogenizing them through a purely mechanical mixing process in a container at the desired molar ratio without any significant mechanical pressure or shear force. In this non-compacted mixing process, the energy input is less than 2 kWh / m³. 3 For example, to perform actual measurements, a laboratory volume (5-1000 mL) of the mixture is poured into a bottle approximately twice the nominal volume and homogenized by prolonged shaking (at least 5 minutes) and / or rotating the bottle on a roller rack for several hours (e.g., 10 hours). The bulk density is determined according to DIN ISO 697.
[0020] The enhanced mixing method according to the invention results in the deagglomeration of carbon agglomerates, i.e., the breakup into individual primary particles and an effective coating of crystalline lithium carbonate. During the mixing process, spatially separated primary carbon particles are deposited on and coated onto the surfaces of larger lithium carbonate particles. The mixing process aims to achieve a uniform macroscopic distribution of carbon particles in the mixture and, as completely as possible, a surface coating of individual lithium carbonate particles. It is assumed that under enhanced mixing conditions, introducing small carbon particles (see below) into the pore volume and interstices of the carbonate particles would result in an observed increase in the bulk density of the mixture.
[0021] Direct contact between carbon-based particles and lithium carbonate particles facilitates mass transfer, thereby benefiting the reaction kinetics between the two components. Furthermore, it prevents the separated lithium carbonate particles from melting when the melting temperature is exceeded.
[0022] Enhanced mixing, namely decoagulation and compaction of mixtures, can be achieved through the application of shear forces or multi-stage compression / grinding processes.
[0023] Surprisingly, it was found that when a compacted mixture of the two raw materials was used, a lithium oxide final product with significantly improved uniformity, purity and improved flowability could be obtained compared with the uncompacted mixture shown in WO 18114760A1.
[0024] To achieve the desired deagglomeration and compaction of the particulate carbon fraction during the mixing process, various equipment and process technologies can be applied. Grinding devices, rotary intensified mixers, or compaction devices are suitable. These include most types of mills, particularly rotor stirred mills (impact mills), media mills, or pin mills; cutting tools or cutters may also be used to a limited extent. In media mills, mixing takes place in grinding drums using hard abrasive media, such as balls, rods, etc., composed of metals (steel or nickel-based alloys) or hard ceramics (metal oxides, metal carbides, metal nitrides). The Vickers hardness of the grinding container and grinding media is at least 400, preferably at least 600. Materials made of stainless steel or metal oxides, such as alumina or zirconium oxide, are particularly preferred. Ball mills, rod mills, or hammer mills can be used.
[0025] In addition, it can be used to generate approximately 10 to 500 kW / m 3 A rotary mixer with energy input within a certain range. Both rotary mixers with rotating containers and rotary mixing tools are suitable.
[0026] The key is to generate a sufficiently strong energy input for compaction. Such a device can be designed based on counter-current or cross-current principles, such as the "intensive mixer" offered by Eirich. Other suitable mixer designs include paddle dryers with an additional mounted blade grinder, such as... The company provides, as well as enhanced mixers with high-speed rotors, such as those offered by Hosokawa under the "Nobilta" brand.
[0027] Furthermore, compactors, such as single-stage or multi-stage roller presses or roller mills, are suitable for compaction. In this case, in the second step, it is preferable to granulate and / or grind the compacted raw material mixture. To achieve good deagglomeration and uniform distribution of carbon particles, the compaction / grinding process is preferably performed several times (e.g., 2-10 times).
[0028] Alternatively, a non-beaded grade of carbon black can be used, or the carbon product can be de-agglomerated in a separate step (i.e., without lithium carbonate), and then the de-agglomerated process product can be mixed with lithium carbonate in a second step to carbon coat and densify it. Non-beaded carbon black, due to its typically low flowability and high dust content, requires special processing techniques for industrial-scale use. It has been found that non-beaded carbon black, such as the product offered by Cabot under the name "Vulkan P fluffy," can convert lithium carbonate to lithium oxide more quickly and completely. In particular, this non-beaded grade is used in the method of the present invention where a Li₂O final product with a particularly low combustible carbon content (i.e., TOC) is required. The two-step process can produce a mixture of equal mass, but is less preferred due to higher equipment requirements and lower costs. In both cases, to achieve the advantages desired by the present invention, the two components need to be thoroughly mixed by appropriate compaction.
[0029] Typically, the energy input during the mixing process, such as the intensity of shear forces, does not result in a significant reduction in the particle size of crystalline lithium carbonate particles. Therefore, the mixing energy input is usually only sufficient to break up carbon particle agglomerates held together by relatively weak van der Waals forces into separate primary particles. However, if relatively coarse-grained lithium carbonate (e.g., D...) is used... 50 Lithium carbonate >50μm) and simultaneously produce particularly fine-particle lithium oxide (e.g., D 50 According to the present invention, even stronger shear forces can be applied to the mixture (approximately 10-20 μm). Such higher shear forces occur, for example, in classifying mills, planetary ball mills, or jet mills. These intense grinding and mixing processes are also according to the present invention and are superior to grinding the final Li₂O product. In fact, its advantage is that lithium carbonate is non-hygroscopic and indefinitely resistant to air. Therefore, the grinding process can be carried out under normal ambient air atmosphere. This contrasts with the requirements for grinding lithium oxide. This oxide is extremely hygroscopic and reacts violently with CO₂. Therefore, oxide grinding requires maintaining strictly inert conditions, i.e., excluding air and moisture, which is associated with relatively high costs.
[0030] Premixing can be carried out over a wide temperature range of approximately 0 to 500°C. Preferably, it is carried out at an ambient temperature without active heating or cooling. To avoid the risk of dust explosion, it is preferable to carry out the mixture under inert conditions, i.e., in an oxygen-free or oxygen-deficient atmosphere. Inert conditions can be achieved by overflow with an inert gas (rare gas or nitrogen) or under vacuum conditions. Preferably, the oxygen content in the mixing unit used is <12 vol.%, more preferably <5 vol.%.
[0031] The subsequent thermally induced conversion (calcination) is carried out in an apparatus with a surface for the product made of a material resistant to high temperatures and alkaline lithium salt corrosion. Contrary to the teachings established in WO 18114760 A1 that metallic materials other than tantalum are generally unavailable, it has been found that a variety of metallic materials selected from high-temperature resistant Cr- and / or Al-containing materials are available. In particular, nickel-based alloys containing Cr and / or Al, austenitic steels containing Ni and Cr, and low-Ni or Ni-free, Cr- and Al-containing ferritic steels and chromium-containing mixed austenitic-ferritic steels can be used as container materials for converting a mixture of elemental carbon and lithium carbonate compacted according to the invention into pure lithium oxide. Suitable alloys have a chromium content of at least 15 wt.%, preferably at least 20 wt.%, and particularly preferably at least 30 wt.%. With an Al content of at least 1 wt.%, the chromium content can be selected to be significantly lower (at least 5 wt.%). A preferred Al content is at least 1 wt.%, particularly preferably at least 2 wt.%. In addition to chromium and aluminum, the metallic alloys used in the methods of this invention may contain elements niobium, titanium, tantalum, and / or silicon, in each case up to 10 wt%. Low-Mo alloys are preferred. The Mo content is <2 wt.%, preferably <1 wt.%.
[0032] The following commercially available metal materials are particularly advantageous to use:
[0033] Nickel-based alloys: Inconel 600, Inconel 601, Inconel 693, Inconel 702, Inconel 800, Inconel 825; Incoloy 901, Nichrome, Nichrome V, Nimonic 75, Nimonic 80A, Nimonic 90, RA602CA / Alloy 602 CA, Alloy X and similar grades;
[0034] Austenitic steels: SS347 (1.4550), 253MA (1.4835), Nitronic 50, 310S, 316L, SS310, SS304, RA253MA, etc.
[0035] Ferritic steels: Kanthal (e.g., Kanthal A1, Kanthal AF, Kanthal D(FeCrAl)), PM2000, Incoloy MA 956, etc.
[0036] Solid metal materials selected from the above-mentioned material group and correspondingly coated high-temperature resistant black steel or stainless steel can be used. The corrosion-inhibiting coating applied to the side facing the product contains at least 10 wt.%, preferably at least 30 wt.%, of chromium. Furthermore, it may contain elements Ni, Fe, Nb, Al, Ti, Ta, and Si, each in a maximum content of 10 wt.%.
[0037] The thickness of the chromium-containing anti-corrosion coating is at least 5 μm, preferably at least 10 μm. The coating thickness is determined by electron microscopy. For example, only moderately corrosion-resistant austenitic steels, such as 1.4401, can have their corrosion resistance significantly improved by applying a 50 μm thick Cr and Al-containing coating. Such a coating process can be achieved by various electrochemical or physical techniques, such as embedding bonding processes (Kim, Mater. Transact. 43, 2002, 593).
[0038] In addition to the aforementioned metallic materials, carbon-based materials, certain oxide ceramics (e.g., Al2O3, lithium aluminate ceramics (LiAlO2), or Ce-based ceramics, such as Ce-stabilized ZrO2), and non-oxide ceramics (such as carbides of SiC, BC, and TiC; nitrides such as TiN and AlN; and borides such as NbB2, BN, Al-infiltrated TiB2, and "TiBAl") can also be used as container materials. Materials coated with the aforementioned ceramics (preferably LiAlO2), such as high-temperature steel, can also be used. As a carbon-based material, graphite (carbon graphite, hard carbon) can be used, especially pure carbon (glassy carbon) with a disordered graphite structure and ceramic properties. However, the use of carbon-based materials in high-temperature calcination processes, i.e., processes at temperatures >400°C, requires particularly strict control of inert conditions, i.e., complete exclusion of oxidants such as oxygen or other oxygen donors such as water or carbon dioxide. Oxidation-stable graphite materials are particularly preferred, exhibiting a significantly lower burnup rate than high-purity graphite upon contact with ambient air (DVSavchenko, New Carbon Materials 2012, 27, 12-18). Graphite materials are high-temperature resistant materials produced from raw materials such as petroleum coke, pitch coke, carbon black, and graphite using a filler / binder system. They are first ground to a specified particle size distribution, mixed at high temperature, shaped and compacted into a green body in a press, and then carbonized through a high-temperature pyrolysis process.
[0039] Carbon-based materials can be used for solid reaction vessels or for hollow bodies coated or lined with graphite materials (e.g., metal tubes lined with graphite foil).
[0040] The carbothermic conversion of elemental carbon-coated lithium carbonate to lithium oxide is carried out under conditions that ensure effective removal of carbon monoxide byproducts formed during the reaction. Preferably, the reaction is carried out under reduced pressure, such as a "technical vacuum" (i.e., a negative pressure in the range of about 0.01 to 50 mbar (1 to 5000 Pa)). It can also be operated under overflow conditions, in which case the overflow gas or gas mixture must be inert or substantially inert relative to carbon, even at temperatures >600°C. Preferably, nitrogen or a rare gas (preferably argon) can be used as such an inert gas, or a mixture of inert gases can be used. The inert gas must be of high purity to prevent contamination by water and oxygen. The content of these two substances generally must not exceed about 0.1% by volume.
[0041] To achieve a commercially satisfactory reaction rate, a temperature range of 600 to 1200 °C is selected. Depending on the selected temperature, the calcination duration typically ranges from 5 minutes to 48 hours, preferably 10 to 300 minutes, for example at 900 °C. Particularly preferred process factors include maintaining a specific temperature distribution comprising a reaction stage below the melting temperature of lithium carbonate (approximately 720 °C) and a second stage above 720 °C, during which the conversion to lithium oxide is completed. In the first reaction stage, the residence time is approximately 1 to 120 minutes, and the mixture is calcined in a temperature range of 600 to 700 °C. This is followed by a reaction stage with a further increase in product temperature, during which the conversion to oxide is completed. The second stage has a temperature range of 700 to 1200 °C and lasts from 10 hours to 5 minutes, depending on the temperature of the selected product. A product temperature between 800 and 950 °C is particularly preferred, with a corresponding residence time of 2 hours to 10 minutes. Surprisingly, it was found that the lithium oxide produced in this manner exhibited neither sintering nor agglomeration during the high-temperature stage.
[0042] The elemental carbon used is in powder form, composed of particles with a high surface area to volume ratio. Preferably, powdered industrial carbon black, graphite, activated carbon, or graphene is used. The molar ratio of lithium carbonate to carbon in the elemental carbon used is 1:0.1 to 1:1.2, preferably 1:0.6 to 1:1.1. Preferably, the C raw material used has a high specific surface area (10 to 1500 m²). 2 / g, preferably 20 to 200m 2 / g (determined by the BET method) and has a very small primary particle size. According to standard specification ASTM D6556, the specific surface area is measured by gas adsorption; this method is called "BET measurement," named after the developers Stephen Brunauer, Paul Hugh Emmett, and Edward Teller. Primary particle size and agglomerate content are determined by electron microscopy (using the morphology determination method of electron microscopy ASTM D 3849). Particle size can also be determined by laser diffraction according to ISO standard 13320 (published January 2020), but these methods do not allow for differentiation between primary particles and aggregated particles. The median primary particle size D, determined according to ASTM D3849... 50 <1μm, but median primary particle size D is preferred. 50 Carbon particles <100nm, with a minimum preferred size of <50nm. Based on the total mass of all particles, the median D... 50 This indicates that there are 50wt% of the corresponding particle size type above and below it.
[0043] Finely differentiated carbon powder is supplied by various companies and used as filler, colorant, or conductive carbon black, the latter used to improve conductivity. Many commercially available carbon grades, especially carbon black, contain a large number of agglomerates. These agglomerates improve the flowability of finely differentiated carbon and are produced by carbon black producers through granulation.
[0044] The toner used is of high purity, i.e., with a low sulfur content of <1000 ppm, preferably <500 ppm, and a low residual ash content of <1000 ppm, preferably <500 ppm. The sulfur content is determined by atomic emission spectroscopy, for example by inductively coupled plasma (ICP-OES). The residual ash content is determined according to DIN EN 15403 standard.
[0045] For example, typical BET surface areas of 20 and 80 m² can be used. 2 High-purity conductive carbon black in the range of / g, such as that sold by Timcal Graphite & Carbon under the trade names TIMCAL C45, C-NERGY Super C65, or Super P-Li. Suitable high-purity industrial carbon black, for example, is supplied by Cabot under the brands ELFTEX 254, ELFTEX TP, or ELFTEX P100.
[0046] The average particle size D of the lithium carbonate 50The particle size is 2 to 150 μm, preferably 10 to 80 μm (measured by laser diffraction, for example using a device from Malvern Pananalytical called the "Mastersizer 3000"). For the application of Li₂O end products in the production of energy storage technology materials, high purity is typically required. Therefore, pure lithium carbonate is used for this purpose, for example, commercially as "battery grade." For example, this product grade has a sodium content of no more than 500 ppm and a total heavy metal content of no more than 100 ppm. Impurities are typically measured by atomic emission spectrometry such as ICP-OES, or by atomic absorption spectrometry (AAS) of elements that exhibit low detection sensitivity in atomic emission spectra (e.g., suitable for Na).
[0047] To achieve the most uniform coating between crystalline lithium carbonate particles and primary carbon particles during the enhanced mixing pretreatment, the carbon particles must have a significantly smaller particle size (D) compared to the lithium carbonate crystals. 50 Typically, the particle size D of carbon and Li2CO3 is... 50 The ratio is from 1:50 to 1:20,000, preferably from 1:100 to 1:10,000.
[0048] Under the spirit of this invention, the micro-fine carbon required for the carbothermic reaction can also be produced in the presence of lithium carbonate through the upstream pyrolysis reaction of an organic, low-ash (maximum ash content 0.1 wt.%) organic compound. This mixture is then compacted / compressed according to the above process and subsequently converted to lithium oxide by calcination at 600-1200°C. In this process, lithium carbonate is premixed with a suitable organic material (such as sugar, cellulose, edible oil, etc.) and pyrolyzed in an anaerobic environment at a temperature of 200-600°C. Volatile components and pyrolysis gases are discharged to an exhaust gas treatment device via a valve system. The residue, consisting preferably of elemental carbon and lithium carbonate in a molar ratio of 0.6-1.2:1, is then compacted in a mill or compaction device at a rate of at least 5%, preferably at least 15%, and then pyrolyzed according to the invention.
[0049] In its simplest form, pyrolysis to lithium oxide can be carried out under static, i.e., unstirred and non-moving conditions. However, it is preferably carried out under moving bed conditions. For moving bed technology, reactors with fluidized bed or floating bed technology are used, as well as fluidized bed reactors (e.g., rotary tube or oscillating tube reactors). For this purpose, the reaction mixture is brought to the desired temperature in the moving bed reactor, and the product lithium oxide is converted while removing the CO-containing waste gas stream. Production in a moving bed reactor is preferably not carried out in batches, but rather using continuous feedstock and corresponding continuous reaction and product discharge.
[0050] Depending on the reaction conditions, a certain proportion of elemental carbon may remain in the calcined product. To reduce or completely eliminate this residual C, which is undesirable for some applications, purification can be performed downstream of the synthesis reaction. For this purification process, an oxygen-containing gas or gas mixture (decarburizing gas) selected from O2, CO2, and H2O is used, possibly diluted with other carbon-inert gases such as nitrogen or rare gases. The purification process can be carried out in the same apparatus as the carbothermic Li2O formation or in a separate second apparatus. As with the synthesis process, the purification process requires high temperatures, typically at least 300°C, preferably at least 600°C, and particularly preferably at least 700°C. Materials suitable for use as containers in this step are selected from high-temperature metal alloys, ceramics, or inorganic glasses. Carbon-based materials such as glassy carbon and graphite cannot be used at temperatures above approximately 600°C because they will be attacked by the decarburizing gas and converted to a gaseous state. During the conversion of C-containing lithium oxide, the following carbon gasification reaction occurs:
[0051] C + O₂ → CO₂ (4)
[0052] C + CO₂ → 2CO (5)
[0053] C + H₂O → CO + H₂ (6)
[0054] To minimize the reaction between the generated carbon-containing gases (CO and CO2) and Li2O, the reactant gases must be removed as efficiently as possible. This is achieved by simultaneously introducing an inert carrier gas, either as a separate gas stream or preferably as a mixture with the O-containing decarbonizing gases. Air is preferred for decarbonization, and if necessary, its oxygen content can be diluted to <10 vol.% by mixing with nitrogen. Furthermore, nitrogen or argon, with a water content corresponding to its H2O saturation concentration, is a preferred decarbonizing agent in the temperature range of 0 to 400°C. The overflow velocity of the decarbonizing gas or gas mixture is typically 0.1–10 cm / s.
[0055] The pure lithium oxide according to the present invention can be used to produce cathode materials (positive electrode materials) for lithium batteries and for the production of glass, glass ceramics, or crystalline ceramics. Particularly preferred is that the pure lithium oxide prepared by the method of the present invention is used to produce lithium-rich nickel compounds such as Li₂NiO₂ (G. Cedar, Chem. Mater. 2004, 2685) or to produce lithium-conductive glass, glass ceramics, or ceramics, such as LLZO (lithium lanthanum zirconium oxide with a garnet-type structure) or oxygen-stabilized thiophosphate compounds (H. Tsukasaki, Solid State Ionics 347, 2020, 115267) or Li-containing silver-germanium sulfide (e.g., Li₆PS₄OCl, US 2020 / 0087155). Detailed Implementation
[0056] The following examples are intended to explain the method according to the present invention without making any limitations.
[0057] The Li2O reaction products were analyzed and characterized using the following methods:
[0058] • Determination of Li₂O content: Acidity titration method
[0059] • Metallic impurities: ICP-OES (atomic emission spectrometry)
[0060] • Carbon content: The contents of inorganic C (carbonate, “TIC”) and elemental / organic C (“TOC”) were determined using equipment from Seifert Instruments (C / S-Max). For TIC determination, the sample was decomposed using dilute phosphoric acid, and the resulting CO2 was measured by passing a carrier gas flow through an IR detector. For TOC determination, the sample was burned in an O2 stream at 1350°C, and the generated CO2 was also detected by IR.
[0061] Example 1 (using beaded carbon black mixture under compaction conditions, followed by calcination under vacuum or in a nitrogen stream):
[0062] 1.1 Mixing:
[0063] 618g of battery-grade lithium carbonate powder (bulk density 650g / L) was used. 50 =26μm) and 100.4g of carbon black (from Cabot's ELFTEX TP, bulk density 370g / L, primary particle size D) 50 =<25nm) and two 50mm diameter agate balls and ten 20mm diameter agate balls were weighed into a 3-L PE bottle with a screw cap. The raw material weight corresponds to a 1:1 Li2CO3:C stoichiometric ratio. After tightening the bottle, its contents were homogenized on a roller rack for 9 hours. Then, the spheres were separated by sieving.
[0064] Weighing: 716g of black mixture, bulk density 0.67g / mL.
[0065] 1.2 Calcination under vacuum conditions:
[0066] 20.0 g of compacted Li₂CO₃ / C mixture was placed in a stainless steel crucible lined with lithium aluminate. The crucible was placed in a tube furnace with stainless steel tubing and heated to the product temperature of 900 °C under vacuum (20 mbar (2000 Pa)). After pyrolysis at the specified temperature for three hours, cooling was performed. The crucible was placed in an argon-filled glove box, and the homogeneous, almost agglomerated light gray material was transferred to glass vials. When sieved and transferred using a 1 mm sieve, the slightly agglomerated portions decomposed into powder.
[0067] Yield: 6.5g (95% d.Th).
[0068] analyze:
[0069] Total inorganic carbon (TIC) = 0.2%.
[0070] Total organic carbon (TOC) = 0.1%
[0071] Fe(ICP-OES) = 60ppm
[0072] Li2O content (titration) = 98%.
[0073] 1.3 Calcination in a nitrogen stream:
[0074] 10.0 g of compacted Li₂CO₃ / C mixture from 1.1 g was placed in an alumina crucible. The crucible was placed in a tube furnace with a quartz tube and heated to the product temperature of 900 °C under a nitrogen flow (40 L / h). The CO concentration in the gas effluent was measured using a CO-sensitive gas sensor. Initially, the CO detector showed a CO concentration >2000 ppm (maximum measurable concentration). After pyrolysis at the specified temperature for 6.5 hours, CO was no longer detectable (<3 ppm), and the mixture was cooled. The crucible was transferred to an Ar-filled glove box using an intermediate transfer container, and the homogeneous, almost non-caking, slightly grayish material was transferred to glass vials. Slightly agglomerated portions decomposed into powder during sieving and transfer through a 1 mm sieve.
[0075] Yield: 3.2g (92% d.Th).
[0076] analyze:
[0077] Total inorganic carbon (TIC) = 0.14%;
[0078] Total organic carbon (TOC) = 0.14%.
[0079] Example 2 (Comparative example according to WO 18114760 A1, (mixing beaded carbon black under non-compacted conditions and subsequently calcining):
[0080] 2.1 Mixing:
[0081] 620 g of battery-grade lithium carbonate powder and 100.6 g of carbon black (ELFTEX TP from Cabot) were weighed into a 3-L PE bottle with a screw cap. These materials were the same as those used in Example 1.1. The raw material weights correspond to a stoichiometric ratio of Li₂CO₃:C of 1:1. After tightening the bottle, the contents were homogenized on a roller rack for 9 hours.
[0082] Weighing: 717g of black mixture, bulk density 0.58g / mL.
[0083] 2.2 Calcination:
[0084] 20.0 g of uncompacted Li₂CO₃ / C mixture was placed in a stainless steel crucible lined with lithium aluminate. The crucible was placed in a tube furnace with stainless steel tubing and heated to the product temperature of 900 °C under vacuum (20 mbar (2000 Pa)). After pyrolysis at the specified temperature for three hours, the mixture was cooled. The crucible was placed in a glove box filled with Ar, and the uneven, partially agglomerated gray material was removed from the lumpy portion through a 1 mm sieve and transferred to a glass bottle.
[0085] Yield: 6.1g (88% of Th). (0.6g of residue on a >1mm sieve was obtained).
[0086] analyze:
[0087] Total inorganic carbon (TIC) = 0.8%;
[0088] Total organic carbon (TOC) = 0.6%;
[0089] Fe(ICP) = 160 ppm;
[0090] Li2O content (titration) = 98%.
[0091] Example 3 (Post-purification with oxygen to reduce TOC):
[0092] In an Ar-filled glove box, 7.9 g of Li₂O with a TOC content of 1.3% and a TIC content of 0.19% was added to a ceramic crucible (pure Al₂O₃). The crucible was placed in a tube furnace with a quartz tube of 40 mm diameter, air was purged, and the mixture was heated to a process temperature of 800 °C at a nitrogen flow rate of approximately 400 L / h. After reaching the target temperature, ambient air was added to the gas stream multiple times at a rate of approximately 10-40% for 30-60 s. The sample began to decolorize after the first contact with air containing the overflow gas. The air mixing was repeated until no further CO was detected in the exhaust gas. The system was then switched to pure nitrogen and calcined for another 30 minutes. Cooling was then performed under a nitrogen flow, and the crucible was emptied in the glove box.
[0093] Yield: 6.7g of colorless, slightly clumped product.
[0094] analyze:
[0095] TOC < 50 ppm (limit of detection!);
[0096] TIC = 0.18%.
[0097] Example 4 (Post-purification by reducing TOC through water vapor):
[0098] In an Ar-filled glove box, 8.3 g of Li₂O with a TOC content of 1.3% and a TIC content of 0.19% was added to a ceramic crucible (pure Al₂O₃). The crucible was placed in a quartz tube furnace with a diameter of 40 mm and heated to a process temperature of 900 °C under a nitrogen flow rate of 400 L / h. After reaching the target temperature, moisture was added to the gas flow. This was done by passing the N₂ gas flow through a Willf bottle filled with water. The sample immediately began to decolorize. The gas flow containing air moisture was maintained for 1–2 hours. Then, it was switched back to pure nitrogen and calcined for another 30 minutes. Finally, it was cooled under a nitrogen flow and the crucible was emptied in the glove box.
[0099] Yield: 6.9g of white, partially clumped product
[0100] analyze
[0101] TOC 350ppm;
[0102] TIC = 0.023%.
[0103] Example 5 (using beadless carbon black, mixed under compaction conditions, and then calcined in a nitrogen stream):
[0104] 5.1 Mixing:
[0105] 350g of battery-grade lithium carbonate powder (bulk density 650g / L) was weighed into a 3L PE bottle with a screw cap. 50 =26μm) and 56.8g of carbon black (from Cabot's Vulcan P fluffy, bulk density 220g / L, primary particle size D) 50 =<25nm) and 2 agate spheres with a diameter of 50mm and 10 agate spheres with a diameter of 20mm. The raw material weight corresponds to a stoichiometric ratio of Li2CO3:C of 1:1. After tightening the bottle, its contents were homogenized on a roller rack for 9 hours. Then the spheres were separated by sieving.
[0106] Weighing: 395g of black mixture, bulk density 0.63g / mL.
[0107] 5.2 Calcination in a nitrogen stream:
[0108] 10.0 g of compressed Li₂CO₃ / C mixture from 5.1 was placed in an alumina crucible. The crucible was placed in a tube furnace with a quartz tube and heated to a product temperature of 900 °C under a nitrogen flow (40 L / h). The CO concentration in the gas discharge was measured using a CO-sensitive gas sensor. Initially, the CO detector showed a CO concentration >2000 ppm. After pyrolysis at the specified temperature for 3 hours, the CO content decreased to <3 ppm, and the mixture was cooled. The crucible was transferred to an Ar-filled glove box using an intermediate transfer container, and the homogeneous, almost agglomerated, snow-white material was transferred to a glass bottle. Slightly agglomerated portions decomposed into powder during sieving and transfer through a 1 mm sieve.
[0109] Yield: 3.3g (95% d.Th).
[0110] analyze:
[0111] Total inorganic carbon (TIC) = 0.10%;
[0112] Total organic carbon (TOC) = 0.01%.
[0113] Examples 1 and 2 show the effects of different mixing processes on the bulk density of the raw material mixture and the quality of the final product Li2O.
[0114] The compaction mixing method in Example 1 increased the bulk density of the Li₂CO₃ / C mixture from 0.58 g / mL (compared to Example 2, without any pressure or significant shear force) to 0.67 g / mL. This corresponds to a compaction degree of 16%. When beadless carbon black was used in Example 5.1, a compaction degree of 26% was observed compared to the sum of the volumes of carbon black and lithium carbonate used.
[0115] When calcined under vacuum conditions, the compacted raw material mixture of Example 1 produces a product with less aggregation and significantly reduced TOC and TIC content.
[0116] Experiments 3 and 4 describe two possible post-purification processes, specifically the decomposition of elemental carbon by reacting with oxygen (air) and water vapor, respectively.
[0117] By using oxygen contained in the air for post-combustion, TOC can be reduced to below the analytical detection limit of 50 ppm (Example 3). In Example 4, the C content was reduced from 1.3 wt.% to 230 ppm.
[0118] A comparison of the calcination results in Examples 1.3 and 5.2 demonstrates the advantages of using non-beaded carbon black (“fluffy grades”). While it took 6.5 hours to decompose CO using beaded carbon black with the same primary particle size <25 nm, this time was reduced to 3 hours when using non-beaded carbon black “Vulkan P floffy”. Furthermore, the total carbon content (TOC) was significantly lower when using “Vulkan P floffy” (0.01% vs. 0.14%).
Claims
1. A method for producing lithium oxide, wherein the production of lithium oxide is achieved by: - Determination of median particle size D by laser diffraction 50 Lithium carbonate with a thickness of 2 to 150 µm, and - Determination of median primary particle size D by electron microscopy 50 Elemental carbon in powder form <1µm, Calcination is carried out in the temperature range of 600 to 1200°C. Its features are: Prior to calcination, lithium carbonate and carbon are combined, mixed and compacted in a molar ratio of 1:0.1 to 1:1.2, so that carbon particles surround lithium carbonate particles and form a coating, and the resulting mixture has a bulk density that is at least 5% higher than that of an uncompacted mixture of lithium carbonate particles and carbon particles, wherein the bulk density is determined in accordance with EN ISO 697. The calcination is carried out under the following conditions: - Vacuum conditions, which include negative pressures ranging from 0.01 to 50 mbar, or - Overflow conditions, wherein the overflow gas is inert to carbon at temperatures >600°C.
2. The method according to claim 1, characterized in that, The bulk density of the compacted mixture is increased by at least 15% compared to the bulk density of the uncompacted mixture.
3. The method according to claim 1 or 2, characterized in that, Combination, mixing, and compaction are carried out in a grinding unit, a rotary intensified mixer, or a compaction device.
4. The method according to claim 1, characterized in that, Combination, mixing, and compaction occur in a) Energy input of 10 to 500 kW / m 3 Rotary intensified mixer, or b) Rotary agitator, pin mill, or grinding media mill, or c) Compactor.
5. The method according to claim 1, characterized in that, The calcination is carried out in an apparatus whose product-facing surface is made of a material resistant to high temperatures and alkaline lithium salt corrosion, wherein the material is: a) Carbon-based materials, or b) Oxide ceramics, or c) Non-oxide ceramics, or d) Metallic materials containing chromium and / or aluminum.
6. The method according to claim 5, characterized in that, The calcination is carried out in a device where the surface facing the product is a metallic material, the metallic material being selected from: - High-temperature resistant nickel-based alloys containing Cr and / or Al. - Austenitic steel containing Ni and Cr, - Low-Ni and / or Ni-free, Cr- and Al-containing ferritic steels or Cr-containing austenitic-ferritic mixed steels. Where Al < 0.1 wt.%, the chromium content of the metallic material is at least 15 wt.%, and where at least 1 wt.% Al is present, the chromium content is at least 5 wt.%.
7. The method according to claim 5, characterized in that, In addition to chromium and aluminum, the metallic material also contains the elements niobium, titanium, tantalum and / or silicon, each in a proportion of 0 to 10 wt.%.
8. The method according to claim 5, characterized in that, The metallic material contains <2 wt.% molybdenum.
9. The method according to claim 5, characterized in that, The metal material includes high-temperature resistant black steel or stainless steel, which has a Cr-containing metal coating on the side facing the product, wherein the chromium content in the coating is at least 10 wt.%.
10. The method according to claim 9, characterized in that, The coating thickness, as measured by electron microscopy, is at least 5 µm.
11. The method according to claim 1, characterized in that, The gas includes nitrogen, rare gases, or mixtures of inert gases.
12. The method according to claim 1, characterized in that, The molar ratio of lithium carbonate to carbon is in the range of 1:0.6 to 1:1.
1.
13. The method according to claim 1, characterized in that, The carbon includes elemental carbon in powder form, having a particle size of 10 to 1500 m. 2 Specific surface area per g.
14. The method according to claim 1, characterized in that, The carbon includes carbon powder, which has a sulfur content of <1000ppm and a residual ash content of <1000ppm.
15. The method according to claim 1, characterized in that, Median primary particle size D of elemental carbon in powder form 50 Compared with the median particle size D of Li2CO3 50 The ratio is from 1:50 to 1:20,000.
16. The method according to claim 1, characterized in that, The calcination is carried out under moving bed conditions.
17. The method according to claim 1, characterized in that, The prepared lithium oxide is subjected to a decarbonization purification step, wherein the prepared lithium oxide is contacted with a gas stream including oxygen-containing gas at a temperature of at least 300°C.
18. The method according to claim 1, characterized in that, The elemental carbon used is in powder form and is non-particulate carbon black.
Citation Information
Patent Citations
Production of lithium oxide granule
JP1999209122A
Method for manufacturing lithium oxide
JP2012121780A
Method of producing lithium oxide
JP2014047117A
Lithium oxide argyrodites
US20200087155A1
Method for producing lithium oxide
WO2018114760A1