Palladium(II) calixarene-based organic porous polymers, their preparation methods and applications
By preparing palladium(II) calixarene-based organic porous polymers, the problem of existing catalysts being unable to achieve both low cost and high efficiency in desulfurization was solved. Highly efficient catalytic hydrolysis of carbon disulfide and carbonyl sulfide was achieved under mild conditions. The catalyst can be recycled, and the catalytic efficiency is significantly improved.
Patent Information
- Application Number
- CN202310962977.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-01
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-08-01
AI Technical Summary
Existing desulfurization catalysts cannot simultaneously achieve low cost and high efficiency in catalytic desulfurization, especially under mild conditions, where the catalytic hydrolysis efficiency of carbon disulfide and carbonyl sulfide needs to be improved.
A catalyst with a multi-metal center was prepared by using a palladium(II) calixarene-based organic porous polymer and reacting it with compound A via a nucleophilic substitution reaction of 5,5'-dibromomethyl-2,2'-bipyridine and a coordination reaction with Pd(NO3)2. The catalyst was then loaded into the pores of the calixarene-based organic porous material to form a multinucleated cluster active center.
It achieves highly efficient catalytic hydrolysis of carbon disulfide and carbonyl sulfide at room temperature and atmospheric pressure. The catalyst is recyclable, low in cost, and significantly improves catalytic efficiency, which is far higher than that of traditional catalysts.
Smart Images

Figure CN117164823B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of desulfurization catalyst technology, and in particular relates to a palladium(II) calixarene-based organic porous polymer, its preparation method and application. Background Technology
[0002] Carbon disulfide (CS2) and carbonyl sulfide (COS) account for 80% of the total organic sulfur compounds in crude oil and natural gas, with even higher concentrations in crude oil and natural gas from some countries or regions. These chemically inert small organic sulfur molecules have a strong toxic effect on the metal catalysts used in petroleum distillation processes, making desulfurization an indispensable key step and technology in petroleum and natural gas desulfurization processes. In addition, carbon disulfide (CS2) and carbonyl sulfide (COS) can also react with OH- in the atmosphere. - Free radicals spontaneously transform into sulfur dioxide (SO2), a source molecule of acid rain, through photoinduced reactions and disperse in the atmosphere, providing the chemical basis for the eventual formation of more harmful smog and acid rain. Therefore, designing and developing novel, high-efficiency, low-cost, and environmentally friendly desulfurization technologies to achieve activated pyrolysis desulfurization under mild conditions has become an urgent problem to be solved in environmental science and industrial production.
[0003] Organic polymer porous materials, as a class of multifunctional solid materials, have been widely used in gas adsorption, separation, and heterogeneous catalysis. Numerous research results have shown that by modifying and functionalizing the cavities within molecular units and the multidimensional pores of polymer materials using different chemical synthesis methods, the dimensions, size, shape, and internal cavity size of organic polymer porous materials can be precisely controlled. Furthermore, post-modification methods can be used to load highly active metals onto the surface of organic polymer porous materials, resulting in metal-organic polymer porous materials with specific catalytic functions. Chinese patent CN110343240A discloses a palladium(II)-containing organic porous polymer, its preparation method, and its applications. This patent uses palladium(II)-containing organic polymer porous materials to catalyze the hydrolysis of carbon disulfide (CS2) and carbonyl sulfide (COS) under mild conditions, demonstrating that palladium(II)-containing organic polymer porous materials can effectively catalyze the hydrolysis of sulfur-containing small molecules under heterogeneous conditions and achieve recyclability; however, its catalytic efficiency still needs improvement.
[0004] Therefore, designing new, low-cost desulfurization catalysts with high catalytic desulfurization efficiency remains an urgent technical problem to be solved. Summary of the Invention
[0005] The purpose of this invention is to overcome the above-mentioned technical deficiencies and propose a palladium(II) calixarene-based organic porous polymer, its preparation method and application, to solve the technical problem that desulfurization catalysts in the prior art cannot simultaneously achieve low cost and high desulfurization effect.
[0006] In a first aspect, the present invention provides a palladium(II) calixarene-based organic porous polymer having the following structural formula:
[0007]
[0008] Where n = 4 to 8, and X is nitrate.
[0009] Secondly, the present invention provides a method for preparing a palladium(II) calixarene-based organic porous polymer, comprising the following steps:
[0010] (1) 5,5'-dibromomethyl-2,2'-bipyridine was subjected to a nucleophilic substitution reaction with compound A to obtain organic porous polymer B; wherein, the structural formula of compound A is as follows:
[0011]
[0012] Where n = 4 to 8;
[0013] (2) The organic porous polymer B was subjected to a coordination reaction with Pd(NO3)2 to obtain the target product.
[0014] Thirdly, the present invention provides an application of a palladium(II) calixarene-based organic porous polymer, which is used in catalytic hydrolysis desulfurization.
[0015] Compared with the prior art, the beneficial effects of the present invention include:
[0016] (1) This invention provides a novel organic porous polymer based on calixarene containing palladium(II) metal active centers, which can serve as an ideal material for heterogeneous room temperature and atmospheric pressure activation of hydrolyzed organic sulfur molecules.
[0017] (2) This invention uses 5,5'-dibromomethyl-2,2'-bipyridine and compound A as starting materials, and obtains palladium(II)-containing calixarene-based organic porous polymers through nucleophilic substitution and coordination reactions. The synthesis method is simple, the reaction conditions are mild, the yield is high, and it is suitable for industrial production.
[0018] (3) The present invention uses the palladium(II)-containing calixarene-based organic porous polymer as a catalyst, which can catalyze hydrolysis and desulfurization at room temperature and pressure. Compared with traditional catalysts, it has milder operating conditions, lower cost, and wider application range. Attached Figure Description
[0019] Figure 1 Infrared spectra of organic porous polymers B1, B2, and B3;
[0020] Figure 2 X-ray diffraction energy dispersive spectroscopy (XPS) analysis of organic porous polymer B1;
[0021] Figure 3 X-ray diffraction energy dispersive spectroscopy (XPS) analysis of organic porous polymer B2;
[0022] Figure 4 X-ray diffraction energy dispersive spectroscopy (XPS) analysis of organic porous polymer B3;
[0023] Figure 5 The infrared spectra of palladium-containing organic porous polymers P1, P2, and P3 are shown.
[0024] Figure 6 X-ray diffraction energy dispersive spectroscopy (XPS) analysis of palladium-containing organic porous polymer P1;
[0025] Figure 7 X-ray diffraction energy dispersive spectroscopy (XPS) analysis of palladium-containing organic porous polymer P2;
[0026] Figure 8 X-ray diffraction energy dispersive spectroscopy (XPS) analysis of palladium-containing organic porous polymer P3;
[0027] Figure 9 A comparison of the catalytic efficiencies of palladium-containing organic porous polymers P1, P2, and P3 on carbon disulfide (CS2) at room temperature and atmospheric pressure.
[0028] Figure 10 Infrared spectra of polymer B1, palladium-containing organic porous polymers P1 and P4;
[0029] Figure 11 Infrared spectra of polymer B2, palladium-containing organic porous polymers P2 and P5;
[0030] Figure 12 Infrared spectra of polymer B3, palladium-containing organic porous polymers P3 and P6;
[0031] Figure 13 The test results of the three prepared catalysts P1, P2 and P3 on the hydrolysis and cracking of carbon disulfide (CS2) at room temperature and atmospheric pressure, as well as the test results of the blank catalytic control group and the organic polymer porous material catalytic control group;
[0032] Figure 14The test results of the three prepared catalysts P1, P2 and P3 on the hydrolysis and cracking of carbon disulfide (CS2) at room temperature and atmospheric pressure, the test results of the applicant's previously independently developed palladium-supported organic porous polymer catalyst BPY-Pd(NO3)2 on the hydrolysis and cracking of carbon disulfide (CS2) under the same conditions, and the test results of the blank catalytic control group are presented.
[0033] Figure 15 Gas chromatography-mass spectrometry (GC-MS) spectrum of the gas generated by the palladium-containing organic porous polymer P1;
[0034] Figure 16 Gas chromatography-mass spectrometry (GC-MS) spectrum of the gas generated by the palladium-containing organic porous polymer P2;
[0035] Figure 17 Gas chromatography-mass spectrometry (GC-MS) spectrum of the gas generated by the palladium-containing organic porous polymer P3;
[0036] Figure 18 Figure 1 shows the test results for investigating the catalytic cycle performance of compounds P4, P5, and P6 after catalytic hydrolysis and desulfurization.
[0037] Figure 19 The results of catalytic hydrolysis and cracking experiments of palladium-containing organic porous polymers P1, P2, and P3 on COS at room temperature and atmospheric pressure are presented, along with a blank catalytic control group. Detailed Implementation
[0038] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the embodiments described herein are merely illustrative and not intended to limit the invention.
[0039] In a first aspect, the present invention provides a palladium(II)-calixarene-based organic porous polymer, wherein the palladium(II)-based organic porous polymer uses a calixarene-based organic porous polymer material with chelating coordination characteristic groups as a carrier, and palladium is loaded on nitrogen-containing loading sites within the pores of the calixarene-based organic porous polymer material. The palladium(II)-based organic porous polymer has the following structural formula:
[0040]
[0041] Where n = 4 to 8, for example, it can be 4, 6, 8, etc., and those skilled in the art can choose according to the actual situation; X is nitrate.
[0042] This invention uses palladium(II) as the metal active center and selects calixarene functional modules of different sizes and internal cavities as organic monomers to synthesize a novel calixarene-based organic porous polymer containing palladium(II) centers. Its tunable pore size and multiple metal active sites enable this type of metal-supported catalyst material to exhibit unprecedented adsorption performance and catalytic desulfurization efficiency, making it an ideal material for heterogeneous room temperature and atmospheric pressure catalytic hydrolysis of small organic sulfur molecules. This invention introduces corresponding bipyridine palladium(II) active units into the lower edge of cavity-shaped organic monomer molecules of different sizes, including calixarene[4], calixarene[6], and calixarene[8], so that the palladium-containing active sites can form multinuclear cluster active centers, making the distribution of metal catalytic sites more dense, which is conducive to improving the multi-center synergistic catalytic effect, thereby improving the catalytic hydrolysis activity and efficiency. This invention utilizes the synergistic effect of the two to achieve efficient room temperature and atmospheric pressure activation hydrolysis and cracking of carbon disulfide (CS2) and carbonyl sulfide (COS), realize in-situ catalyst regeneration, and rapid product separation. In addition, calixarene monomers can be used to control the microstructure of cross-linked polymer materials through different chemical modifications, such as the pore size, shape and microstructure of the polymer materials, providing a rich pathway and platform for subsequent metal coordination modification.
[0043] Secondly, the present invention provides a method for preparing a palladium(II) calixarene-based organic porous polymer, comprising the following steps:
[0044] (1) Preparation of an organic porous polymer containing a bipyridine group: 5,5'-dibromomethyl-2,2'-bipyridine was subjected to a nucleophilic substitution reaction with compound A to obtain organic porous polymer B; wherein, the structural formula of compound A is as follows:
[0045]
[0046] Where n = 4 to 8;
[0047] (2) Loaded palladium(II): Organic porous polymer B is coordinated with Pd(NO3)2 to obtain the target product.
[0048] The specific reaction formula is as follows:
[0049]
[0050] This invention utilizes an organic polymer porous material containing calixarene and bipyridine monomers of different sizes as a loading platform. Palladium is then loaded onto nitrogen-containing coordination sites within the framework of this organic polymer porous material through coordination modification, thereby preparing a metal-supported organic porous material catalyst capable of spontaneously forming multi-metal catalytic sites within its pores. The synthesis method of this invention is simple, the reaction conditions are mild, and the yield is high, making it suitable for industrial production.
[0051] In this embodiment, in step (1), the temperature of the nucleophilic substitution reaction is 100-110°C, and the time of the nucleophilic substitution reaction is 48-72h; the molar ratio of 5,5'-dibromomethyl-2,2'-bipyridine to compound A is (2-4):1.
[0052] In some specific embodiments of the present invention, when n = 4, the molar ratio of 5,5'-dibromomethyl-2,2'-bipyridine to compound A is 2:1; when n = 6, the molar ratio of 5,5'-dibromomethyl-2,2'-bipyridine to compound A is 3:1; and when n = 8, the molar ratio of 5,5'-dibromomethyl-2,2'-bipyridine to compound A is 4:1.
[0053] In this embodiment, in step (1), a base, a catalyst, and a first organic solvent are also added during the nucleophilic substitution reaction.
[0054] The base is one or more of potassium carbonate, cesium carbonate, and sodium hydride; more preferably, the base is potassium carbonate and cesium carbonate; the catalyst is potassium iodide.
[0055] The mass ratio of 5,5'-dibromomethyl-2,2'-bipyridine to the base is 1:(3-9), and the mass ratio of 5,5'-dibromomethyl-2,2'-bipyridine to the catalyst is 1:(0.1-0.8).
[0056] The first organic solvent is one or more of N,N'-dimethylformamide (DMF) and tetrahydrofuran; more preferably, the first organic solvent is N,N'-dimethylformamide.
[0057] The ratio of the first organic solvent to 5,5'-dibromomethyl-2,2'-bipyridine is 1 mL: (10-20) mg.
[0058] In this embodiment, in step (1), the reaction is carried out under the protection of nitrogen.
[0059] In this embodiment, in step (1), after the reaction is completed, the mixture is cooled to room temperature, the reactants are poured into distilled water and stirred, then filtered and dried; then washed by centrifugation with DMSO and ethanol in sequence, and dried again to obtain an organic porous polymer.
[0060] In this embodiment, in step (2), the temperature of the coordination reaction is 60-70°C and the time of the coordination reaction is 48-72h.
[0061] In this embodiment, in step (2), the mass ratio of organic porous polymer B to Pd(NO3)2 is 1:(0.5~1).
[0062] In this embodiment, in step (2), Pd(NO3)2 is first dissolved in the second organic solvent and then undergoes a coordination reaction with the organic porous polymer B.
[0063] The second organic solvent is acetonitrile, and the ratio of the second organic solvent to Pd(NO3)2 is 1 mL:(10-50) mg, preferably 1 mL:(10-30) mg.
[0064] In this embodiment, in step (2), after the reaction is complete, the mixture needs to be washed with acetonitrile and then vacuum dried.
[0065] The temperature for vacuum drying is 60–150℃.
[0066] Thirdly, the present invention provides an application of a palladium(II) calixarene-based organic porous polymer, which is used in catalytic hydrolysis desulfurization.
[0067] In this embodiment, the catalytic hydrolysis desulfurization process is carried out at room temperature and atmospheric pressure.
[0068] In this embodiment, the reaction system for catalytic hydrolysis desulfurization includes: a palladium(II)-containing calixarene-based organic porous polymer, water, and organic sulfides.
[0069] Among them, the aforementioned organic sulfides include, but are not limited to, carbon disulfide (CS2) and carbonyl sulfide (COS).
[0070] In this embodiment, the reaction system for catalytic hydrolysis and desulfurization further includes a sacrificial agent. The palladium(II)-containing calixarene-based organic porous polymer can be recycled under the action of the sacrificial agent.
[0071] The sacrificial agent is one or more of nitric acid, acetic acid, and hydrogen peroxide. More preferably, the sacrificial agent is nitric acid.
[0072] Unless otherwise specified, the experimental methods used in this invention are conventional methods. Unless otherwise specified, all experimental materials used in this invention were commercially available, and 5,5'-dibromomethyl-2,2'-bipyridine and compound A were synthesized according to previously reported literature.
[0073] Example 1:
[0074] Example 1 of the present invention provides a method for synthesizing an organic porous polymer B1, the synthetic route of which is as follows:
[0075]
[0076] Accurately weigh 5,5'-dibromomethyl-2,2'-bipyridine (316 mg, 0.92 mmol), 4-tert-butylcalix[4]arene (compound A, n=4) (300 mg, 0.46 mmol), CS2CO3 (1.2 g) and KI (100 mg) and place them into a straight tube in sequence. Then add 20 mL of ultra-dry DMF, evacuate and purge with nitrogen for protection, and react at 110 °C for two days. Then cool to room temperature, pour the reaction mixture into 200 mL of distilled water, stir for 2 h, filter and dry. Then put the dried product into an assembly tube, add 6 mL of DMSO, wash 3 times at 80 °C, centrifuge and transfer the solid to an assembly tube containing 6 mL of ethanol, wash 2 times at 80 °C. After centrifugation, put the obtained precipitate into a freeze dryer and dry to obtain organic porous polymer B1 (yield 82%).
[0077] Example 2:
[0078] Example 2 of the present invention provides a method for synthesizing an organic porous polymer B2. The synthetic route and method are the same as those in Example 1 (the synthetic route is shown in the figure below), except that the reactant 4-tert-butylcalix[4]arene is replaced with 4-tert-butylcalix[6]arene (compound A, n=6), and the rest is the same as the synthetic method in Example 1. The amounts of 4-tert-butylcalix[6]arene (200 mg, 0.314 mmol), 5,5'-dibromomethyl-2,2'-bipyridine (343 mg, 1 mmol), CS2CO3 (1.5 g), KI (100 mg), and ultra-dry DMF (20 mL) are used to obtain organic porous polymer B2 (yield 81%).
[0079]
[0080] Example 3:
[0081] Example 3 of the present invention provides a method for synthesizing organic porous polymer B3. The synthesis route and method are the same as those in Example 1 (the synthesis route is shown in the figure below), except that the reactant 4-tert-butylcalix[4]arene is replaced with 4-tert-butylcalix[8]arene (compound A, n=8). The amounts of 4-tert-butylcalix[8]arene (200mg, 0.154mmol), 5,5'-dibromomethyl-2,2'-bipyridine (221mg, 0.648mmol), CS2CO3 (1.8g), KI (100mg) and ultra-dry DMF (20mL) are respectively. The rest are the same as the synthesis method in Example 1, and organic porous polymer B3 (yield 67%) is obtained.
[0082]
[0083] Example 4:
[0084] Example 4 of the present invention provides a method for synthesizing a palladium(II)-containing calixarene-based organic porous polymer P1, the synthetic route of which is as follows:
[0085]
[0086] Palladium nitrate (70 mg) was accurately weighed into a 10 mL assembly tube, and 4 mL of acetonitrile was added as a solvent. The mixture was stirred to dissolve the palladium (II) nitrate, followed by the addition of polymer B1 (100 mg). The mixture was stirred at room temperature for 3 hours, then slowly heated to 60 °C and reacted for 2 days. Heating was stopped, and the mixture was cooled to room temperature. The mixture was filtered and washed three times with acetonitrile. Finally, it was dried under vacuum to obtain palladium(II)-containing calixarene-based organic porous polymer P1 (75% yield).
[0087] Example 5:
[0088] Example 5 of the present invention provides a method for synthesizing palladium-containing calixarene-based organic porous polymer P2. The synthesis route and method are the same as those in Example 4 (the synthesis route is shown in the figure below), except that reactant B1 is replaced with B2; the rest are the same as the synthesis method in Example 4, to obtain palladium(II)-containing calixarene-based organic porous polymer P2 (yield 70%).
[0089]
[0090] Example 6:
[0091] Example 6 of the present invention provides a method for synthesizing palladium-containing calixarene-based organic porous polymer P3. The synthesis route and method are the same as those in Example 4 (the synthesis route is shown in the figure below), except that reactant B1 is replaced with B3; the rest are the same as the synthesis method in Example 4, to obtain palladium(II)-containing calixarene-based organic porous polymer P3 (yield 75%).
[0092]
[0093] Experimental Example 1:
[0094] Qualitative and quantitative analyses were performed on organic porous polymers B1, B2, and B3. The characterization methods for organic porous polymers B1, B2, and B3 were the same. Quantitative analysis of B1, B2, and B3 was performed using organic-inorganic elemental analysis (EA) and X-ray diffraction energy dispersive spectroscopy (XPS), while qualitative analysis was performed using Fourier transform infrared spectroscopy (FT-IR). The elemental analysis (EA) results for organic porous polymers B1, B2, and B3 are shown in Table 1.
[0095] Table 1
[0096]
[0097]
[0098] As shown in Table 1, the elemental composition of organic porous polymers B1, B2, and B3 conforms to the simulated unit structure and is close to the theoretical value, proving that the polymerization reaction was successful.
[0099] Figure 1 The images show the infrared spectra of B1, B2, and B3 prepared in Examples 1, 2, and 3. The infrared spectrum is shown at 1448 cm⁻¹. -1 The characteristic peak of the C=N stretching vibration signal exists at this location. The stretching vibration signal of the benzene ring C=N is located at 1650–1500 cm⁻¹. -1 There are 2 to 4 characteristic peaks, and at 1600 cm⁻¹ -1 There is a characteristic peak of C=C stretching vibration signal at 1120cm. -1 and 1190cm -1 Characteristic peaks of the stretching vibration signal of COC are present. Clearly, the characteristic peaks of the phenolic hydroxyl groups on the calixarene skeleton and the brominated hydrocarbons on the bipyridine disappear, while the characteristic peaks of the ether bond appear. These results prove that the target polymerization reaction was successfully completed.
[0100] Figure 2 , Figure 3 , Figure 4 The XPS spectra of polymers B1, B2, and B3 are shown below. As can be seen from the figures, the elemental distribution in the tested materials is C, N, and O, and the C to N ratio is close to the C to N ratio in the elemental analysis shown in Table 2. These results further confirm that the target polymerization reaction was completed.
[0101] Table 2
[0102] Atomic ratio of elements (%) C N O Polymer B1 84.89 5.33 9.79 Polymer B2 78.55 6.15 15.30 Polymer B3 80.08 6.03 13.89
[0103] Experimental Example 2:
[0104] Qualitative and quantitative analyses were performed on palladium(II)-containing organic porous polymers P1, P2, and P3. Fourier transform infrared spectroscopy (FT-IR) was used for qualitative analysis of the target compounds, and X-ray diffraction energy dispersive spectroscopy (XPS) was used for quantitative analysis of the target compounds.
[0105] Figure 5 The images show the infrared spectra of P1, P2, and P3 prepared in Examples 4, 5, and 6. Theoretically, nitrate (NO3) - ) in 1560~1300cm -1 There is a characteristic peak at this location, due to Figure 5 Mid-infrared spectroscopy reveals that at 1380 cm⁻¹ -1 The presence of characteristic stretching vibrations of nitrate ions indicates that palladium nitrate was successfully loaded onto the polymer, resulting in a palladium(II)-containing organic porous polymer.
[0106] Figure 6 , Figure 7 , Figure 8 The XPS spectra of polymers P1, P2, and P3 are shown below. The figures reveal that the elemental distribution in the tested materials is C, N, O, and Pd. Peak separation analysis shows that all materials contain palladium, and all are divalent palladium. The elemental quantitative (XPS) analysis results are shown in Table 3. Table 3 shows that N:Pd ≈ 2:1, confirming successful palladium nitrate loading, with a loading rate (palladium mass ratio, wt%) of 2–4%.
[0107] Table 3
[0108] Atomic ratio of elements (%) C N O <![CDATA[Pd 2+ ]]> P1 71.42 7.05 19.32 2.20 P2 69.85 7.47 19.92 2.76 P3 69.86 7.67 19.58 2.93
[0109] Experimental Example 3:
[0110] This paper discusses the catalytic hydrolysis desulfurization performance of organic porous polymers P1, P2, and P3 containing palladium(II) centers. Taking P1 as an example: 100 μL of distilled water, 50 μL of carbon disulfide (CS2), and 10 mg of catalyst P1 were added to a 2.5 mL sample vial. The vial was sealed with a sample cap suitable for gas chromatography (GC) sampling, and the catalytic reaction was carried out with stirring at room temperature. Five vials were prepared simultaneously. At 0, 2, 4, 6, 8, and 10.5 hours of reaction, 500 μL of gas was drawn from each vial using a gas chromatograph with a gas valve for GC analysis to test the change in CO2 content. The final results are as follows: Figure 9 As shown, the palladium-loaded organic polymer porous material prepared in this invention exhibits hydrolytic cracking activity against carbon disulfide. After catalyst P1 reacts completely, the mixture is centrifuged, the supernatant is removed, and the precipitate is repeatedly washed with ethanol and dried under vacuum at 60°C to obtain the catalytically modified target compound P4. Using the same treatment method, compound P5 is obtained with P2 as a catalyst, and compound P6 is obtained with P3 as a catalyst.
[0111] Figure 10 The figures show the infrared spectra of B1, catalyst P1, and compound P4 after desulfurization catalyzed by catalyst P1. As can be seen from the figures, the characteristic peak of nitrate ions departs after catalysis.
[0112] Figure 11The figures show the infrared spectra of B2, catalyst P2, and compound P5 after desulfurization catalyzed by catalyst P2. As can be seen from the figures, the characteristic peak of nitrate ions departs after catalysis.
[0113] Figure 12 The figures show the infrared spectra of B3, catalyst P3, and compound P6 after desulfurization catalyzed by catalyst P3. As can be seen from the figures, the characteristic peak of nitrate ions departs after catalysis.
[0114] Experimental Example 4:
[0115] To rule out the hydrolysis of carbon disulfide (CS2) with water itself, a set of experiments was conducted under the same conditions as in Example 3, the only difference being that no catalyst was added in this process; this was recorded as a blank catalytic control. To rule out the inherent catalytic properties of the polymer itself, a set of experiments was conducted under the same conditions as in Example 3, the only difference being that unsupported palladium nitrate porous organic polymer materials B1, B2, and B3 were added to replace the corresponding catalysts for comparative catalytic experiments. The final results are as follows: Figure 13 As shown, carbon disulfide (CS2) does not react with water at room temperature, and the three prepared organic polymer porous materials B1, B2, and B3 also have no catalytic effect on carbon disulfide. Furthermore, the test results indicate that the catalytic effect arises from the catalyst's action. The comparison of catalytic efficiency in the experimental results also reflects that the catalytic efficiency of the material is not only related to the loading of the active metal center but also to the material support structure, such as pore size, specific surface area, and spatial arrangement, all of which directly or indirectly affect its catalytic efficiency.
[0116] Experimental Example 5:
[0117] To compare the catalytic effects of catalysts P1, P2, and P3 with the catalytic efficiency difference between the applicant's previously developed catalyst BPY-Pd(NO3)2 (the chelate coordination structure of palladium nitrate and bipyridine is shown below), a set of experiments with the same palladium content as in Experimental Example 3 were conducted on BPY-Pd(NO3)2. The final results are as follows. Figure 14 As shown, the results of P1 are used as a control example here. The other two catalyst controls also showed the same effect. The catalytic efficiencies of the organometallic catalysts P1, P2 and P3 reached as high as 4.12 μmol g⁻¹ within 10.5 h. -1 h -1 5.15 μmol g -1 h -1 and 6.4 μmol g -1 h -1These figures represent 4.9, 6.11, and 7.61 times the catalytic efficiencies of BPY-Pd(NO3)2 reported by the applicant, respectively. It is evident that the palladium(II)-containing organic polymer porous material developed in this patent exhibits excellent heterogeneous catalytic desulfurization activity and catalyst recycling characteristics. Therefore, the catalytic efficiencies of catalysts P1, P2, and P3 prepared in this invention are significantly higher than those of the corresponding catalysts previously developed by the applicant.
[0118]
[0119] Experimental Example 6:
[0120] To investigate whether this catalytic desulfurization process is a hydrolysis-cracking desulfurization, an isotope tracking experiment was conducted using P1 as an example. 18 H2 marked with O 18 O conducted the following experiment: P1 (30 mg) was accurately weighed into a 10 mL reaction tube, a vacuum was drawn and protected with N2, and 0.5 mL of CS2 and 0.5 mL of H2 were injected using a syringe. 18 O, seal and react at room temperature for 3 days (to ensure detectable catalytic products). Take the gas from the flask for gas chromatography-mass spectrometry (GC-MS) analysis. The test results are as follows: Figure 15 , Figure 16 and Figure 17 As shown.
[0121] The results of gas chromatography-mass spectrometry (GC-MS) testing show that... 18 O-labeled carbon dioxide (C 18 O2, m / z = 48) and carbonyl sulfide (C 18 The reaction is produced by carbonyl sulfide (COS, m / z = 62). Extensive research indicates that carbonyl sulfide (COS) readily reacts with water to form carbon dioxide (CO2) under catalytic conditions. Furthermore, hydrogen sulfide (H2S) was not detected in the gas chromatography-mass spectrometry (GC-MS), and XPS analysis shows that sulfur (S) is captured by the catalyst. Therefore, it can be concluded that carbonyl sulfide (COS) is produced by the catalyst. 18 OS is an intermediate product, and carbon dioxide (C) is an intermediate product. 18 O2) is the final catalytic product, so this type of catalyst can also catalyze the hydrolysis and cracking of carbonyl sulfide (COS). Figure 19 ).
[0122] Experimental Example 7:
[0123] The reusability of a catalyst is one of its important properties. To investigate whether the prepared catalyst can be recycled, a catalyst activation catalytic experiment was designed, using compounds P4, P5, and P6 that had undergone complete catalytic deactivation. After a certain period of time in the catalytic experiment, once the catalyst was confirmed to be deactivated, a sacrificial agent was added to restore its catalytic performance. Nitric acid was used as an example here, and the experimental results are as follows: Figure 18 As shown.
[0124] Figure 18 The figure shows the results of catalytic activation tests after deactivation of the three prepared catalysts with the addition of sacrificial agents. Solid dots in the figure indicate the results obtained after the addition of the sacrificial agent. The test results confirm that the prepared catalysts can recover their catalytic effect under the action of the sacrificial agent.
[0125] In summary, the palladium (II) calixarene-based organic polymer of this invention utilizes a covalent organic polymer porous material as a support. Leveraging the ease with which palladium, the active metal center, is introduced into the material's framework through coordination bonds and non-covalent interactions such as host-guest relationships, stable coordination synergistic catalytic sites are formed within the pores, thereby enhancing the catalyst's stability, adsorption performance, and confined space catalytic performance. This palladium-supported organic polymer porous material, under the action of the palladium active metal center, can achieve heterogeneous room-temperature and atmospheric-pressure activated hydrolysis and cracking of carbon disulfide (CS2), which is unprecedented. Furthermore, it allows for catalyst recycling, and its catalytic efficiency is significantly higher than that of the palladium-supported organic porous polymer catalyst previously developed by the applicant. Compared with palladium-supported organic porous polymer catalysts with the same structure, the palladium-supported organic polymer porous material prepared in this invention has lower production costs and higher catalytic efficiency, providing new ideas and possible pathways for the green and efficient hydrolysis and desulfurization of petroleum, natural gas, and flue gas. The material synthesis method of this invention is simple, mature, has mild reaction conditions, and high yield, possessing very high application value.
[0126] The specific embodiments of the present invention described above do not constitute a limitation on the scope of protection of the present invention. Any other corresponding changes and modifications made in accordance with the technical concept of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A palladium(II) calixarene-based organic porous polymer, characterized in that, The palladium(II)-containing calixarene-based organic porous polymer has the following structural formula: ; Where n = 4–8, and X is nitrate; the calixarene-based organic porous polymer is prepared by the following method: 5,5'-dibromomethyl-2,2'-bipyridine is reacted with compound A via a nucleophilic substitution reaction to obtain organic porous polymer B; the structural formula of compound A is as follows: ; Where n = 4 to 8; The nucleophilic substitution reaction is carried out at a temperature of 100–110 °C for 48–72 h; the molar ratio of 5,5'-dibromomethyl-2,2'-bipyridine to compound A is (2–4):
1.
2. A method for preparing the palladium (II) -containing calixarene-based organic porous polymer according to claim 1, characterized in that, Includes the following steps: S1. 5,5'-dibromomethyl-2,2'-bipyridine is reacted with compound A via a nucleophilic substitution reaction to obtain an organic porous polymer B; the structural formula of compound A is as follows: ; Wherein, n=4~8; the temperature of the nucleophilic substitution reaction is 100~110 ℃, and the time of the nucleophilic substitution reaction is 48~72 h; the molar ratio of 5,5'-dibromomethyl-2,2'-bipyridine to compound A is (2~4):1; S2. The organic porous polymer B is subjected to a coordination reaction with Pd(NO3)2 to obtain the target product.
3. The method for preparing the palladium(II) calixarene-based organic porous polymer according to claim 2, characterized in that, In step S1, the nucleophilic substitution reaction further includes a base reagent, a catalyst, and a first organic solvent; wherein the base is one or more of potassium carbonate, cesium carbonate, and sodium hydride, and the mass ratio of 5,5'-dibromomethyl-2,2'-bipyridine to the base is 1:(3-9); the catalyst is potassium iodide, and the mass ratio of 5,5'-dibromomethyl-2,2'-bipyridine to the catalyst is 1:(0.1-0.8); the first organic solvent is one or more of N,N'-dimethylformamide and tetrahydrofuran, and the volume ratio of the first organic solvent to 5,5'-dibromomethyl-2,2'-bipyridine is 1 mL:(10-20) mg.
4. The method for preparing the palladium(II)-calixarene-based organic porous polymer according to claim 2, characterized in that, In step S2, the temperature of the coordination reaction is 60-70 °C, and the time of the coordination reaction is 48-72 h; the mass ratio of the organic porous polymer B to Pd(NO3)2 is 1:(0.5-1).
5. The method for preparing the palladium(II)-calixarene-based organic porous polymer according to claim 2, characterized in that, In step S2, Pd(NO3)2 is first dissolved in a second organic solvent and then undergoes a coordination reaction with organic porous polymer B; wherein, the second organic solvent is acetonitrile, and the ratio of the second organic solvent to Pd(NO3)2 is 1 mL: (10-50) mg.
6. Use of the palladium (II) -containing calixarene-based organic porous polymer according to claim 1, characterized in that, The palladium (II) calixarene-based organic porous polymer is used in catalytic hydrolysis desulfurization.
7. Use of the palladium (II) -containing calixarene-based organic porous polymer according to claim 6, characterized in that, The catalytic hydrolysis desulfurization process is carried out at room temperature and atmospheric pressure.
8. The application of the palladium(II) calixarene-based organic porous polymer according to claim 6, characterized in that, The reaction system for catalytic hydrolysis desulfurization includes: palladium (II)-containing calixarene-based organic porous polymer, water, and organic sulfides.
9. The application of the palladium(II) calixarene-based organic porous polymer according to claim 8, characterized in that, The reaction system for catalytic hydrolysis and cracking of organic sulfides further includes a sacrificial agent; wherein the sacrificial agent is one or more of nitric acid, acetic acid, and hydrogen peroxide.
Citation Information
Patent Citations
Organic porous polymer containing palladium, preparation method and application thereof
CN110343240A
Multicore palladium cluster compound for catalytically hydrolyzing carbon disulfide and carbonyl sulfide
CN106046058A
Catalyst CaPOP3@Pd adopting porous polymer of triazinyl linked calix[4]arene for loading palladium and preparation method and application thereof