An organic cathode material and its preparation method

By preparing organic cathode materials with specific microstructures, the problems of unsatisfactory specific capacity utilization and cycle performance in multivalent ion batteries were solved, and the performance of high-efficiency zinc-ion batteries was improved.

CN117164851BActive Publication Date: 2026-11-17YANSHAN UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311134906.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-05
Publication Date
2026-11-17
Estimated Expiration
2043-09-05

AI Technical Summary

Technical Problem

Existing organic cathode materials have unsatisfactory electrochemical performance in multivalent ion batteries, including specific capacity utilization, rate capability, and long-cycle performance, and their charge-discharge capacity decays rapidly.

Method used

Organic cathode materials are prepared by using 1,4-benzoquinone and 1,3-phenylenediamine or 2,5-dichloro-1,4-benzoquinone and 1,3-phenylenediamine as reaction raw materials through oxidative addition or condensation reactions, forming specific microstructures that are poorly soluble in electrolytes and inhibit the loss of active materials.

Benefits of technology

The prepared organic cathode material exhibits good cycle reversibility and rate performance in zinc-ion batteries, with a maximum discharge specific capacity of 124 mAh g⁻¹ and a capacity retention rate of 66% after 1000 cycles, which is superior to existing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117164851B_ABST
    Figure CN117164851B_ABST
Patent Text Reader

Abstract

This invention provides an organic cathode material and its preparation method. The organic cathode material belongs to the quinone polymer family, is poorly soluble in electrolytes, and can effectively suppress the loss of active materials when applied to ion batteries. Furthermore, this organic cathode material has a stable configuration for intercalating multivalent ions, making it suitable for multivalent ion batteries. It can be prepared using two methods: Method 1: 1,4-benzoquinone and 1,3-phenylenediamine are dissolved in a reaction solvent and prepared via an oxidative addition reaction; Method 2: 2,5-dichloro-1,4-benzoquinone and 1,3-phenylenediamine are dissolved in a reaction solvent and prepared via a condensation reaction under inert gas protection. Experiments have shown that this organic cathode material exhibits good capacity and cycle performance in zinc-ion batteries, with a capacity of 0.02 Ag. ‑1 The highest discharge specific capacity at current density can reach 124 mAh g. ‑1 In 0.1Ag ‑1 The discharge specific capacity reaches 73 mAh g at current density. ‑1 After 1000 charge-discharge cycles, the capacity retention rate is 66%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, specifically to an organic cathode material and its preparation method. Background Technology

[0002] Cathode materials are a key component of ion batteries, determining their electrochemical performance. The most widely used cathode materials are inorganic materials such as iron-based, manganese-based, and vanadium-based compounds. Organic cathode materials, however, are an emerging class of energy storage materials with advantages such as abundant resources, designable structures, easy large-scale production, and convenient degradation and recycling. Developing organic cathode materials aligns with the needs and application trends of current novel energy storage technologies and is an important means to replace metal mineral resources and develop new energy storage devices. Organic cathode materials are expected to become ideal cathode materials for ion batteries, demonstrating enormous application potential in the field of energy storage.

[0003] Currently, organic cathode materials mainly exhibit certain application performance in lithium-ion, sodium-ion, and potassium-ion batteries. However, the number of organic cathode material structures suitable for multivalent ion batteries is relatively small. In multivalent ion batteries, the electrochemical performance of organic cathode materials, such as specific capacity utilization, rate capability, and long-cycle performance, is not ideal, exhibiting characteristics such as low actual specific capacity and rapid capacity decay during charge and discharge. Given the rich variety and relatively complex three-dimensional configurations of organic materials, developing novel organic cathode materials with structures more suitable for the intercalation and deintercalation of multivalent ions is of great significance for promoting the development and application of organic cathode materials. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides an organic cathode material and its preparation method.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0006] This invention provides an organic cathode material, the structural formula of which is:

[0007] Where n is a natural number greater than or equal to 1.

[0008] The present invention also provides a method for preparing the organic cathode material, the method comprising the following steps: dissolving 1,4-benzoquinone and 1,3-phenylenediamine in reaction solvent A and carrying out an oxidative addition reaction; after the reaction is completed, filtering is performed to obtain a filter cake; the filter cake is washed with a washing solvent and then dried to obtain the organic cathode material.

[0009] Furthermore, the method specifically includes the following steps: dissolving 1,4-benzoquinone and 1,3-phenylenediamine in reaction solvent A at a ratio of 0.2 g to 1.2 g of 1,3-phenylenediamine to 5 mL to 150 mL of reaction solvent A; and bubbling 0 mL / min into each 5 mL of reaction solvent A. -1 ~20mLmin -1 The ratio of the oxidizing gas flow is determined, and the oxidizing gas flow is introduced and reacted at 20℃~150℃ for 1h~48h. After the reaction is completed and cooled, the mixture is filtered to obtain a filter cake. The filter cake is washed with a washing solvent and then dried to obtain a black solid powder, which is the organic cathode material.

[0010] Furthermore, the reaction solvent A is methanol, ethanol, isopropanol, n-butanol, or N,N-dimethylformamide.

[0011] Furthermore, the oxidizing gas flow is an oxygen flow or an air flow.

[0012] This invention also provides another method for preparing the organic cathode material, which includes the following steps: dissolving 2,5-dichloro-1,4-benzoquinone and 1,3-phenylenediamine in reaction solvent B, and then heating under inert gas protection to carry out a condensation reaction; after the reaction is completed, filtering is performed to obtain a filter cake; the filter cake is washed with a washing solvent and then dried to obtain the organic cathode material.

[0013] Furthermore, the method specifically includes the following steps: 2,5-dichloro-1,4-benzoquinone and 1.1-2.2 grams of 1,3-phenylenediamine are dissolved in reaction solvent B at a ratio of 5-150 mL per gram of 2,5-dichloro-1,4-benzoquinone, and 1.1-2.2 grams of 1,3-phenylenediamine are dissolved in reaction solvent B. The mixture is reacted at 20°C-150°C for 1-48 hours under inert gas protection. After the reaction is complete and cooled, the mixture is filtered to obtain a filter cake. The filter cake is washed with a washing solvent and then dried to obtain a black solid powder, which is the organic cathode material.

[0014] Furthermore, the reaction solvent B is methanol, ethanol, isopropanol, n-butanol, pyridine, N,N-dimethylformamide, or N-methylpyrrolidone.

[0015] Furthermore, the washing solvent is one or more of methanol, ethanol, isopropanol, n-butanol, N,N-dimethylformamide, and water.

[0016] This invention also provides the application of the organic cathode material described above in the field of ion batteries.

[0017] Compared with the prior art, the technical solution provided by the present invention has at least the following advantages:

[0018] This invention provides an organic cathode material, its preparation method, and its application. This organic cathode material belongs to the quinone polymer family and possesses a specific microstructure, allowing for more stable intercalation of multivalent ions. It is poorly soluble in electrolytes, effectively suppressing the loss of active materials. Furthermore, the organic cathode material can be prepared using two methods: Method 1: 1,4-benzoquinone and 1,3-phenylenediamine are dissolved in a reaction solvent and prepared via an oxidative addition reaction; Method 2: 2,5-dichloro-1,4-benzoquinone and 1,3-phenylenediamine are dissolved in a reaction solvent and prepared via a condensation reaction under inert gas protection. Both methods are simple and feasible. Experiments have shown that when this organic cathode material is applied to zinc-ion batteries, it exhibits good cycle reversibility and rate performance at 0.02 Ag. -1 The highest discharge specific capacity at current density can reach 124 mAh g. -1 ; at 0.1Ag -1 The discharge specific capacity reaches 73 mAh g at current density. -1 After 1000 charge-discharge cycles, the capacity retention rate is 66%. Attached Figure Description

[0019] One or more embodiments are illustrated by way of example with reference to the accompanying drawings. These illustrations do not constitute a limitation on the embodiments, and unless otherwise stated, the figures in the drawings are not to be limited by scale.

[0020] Figure 1 The X-ray diffraction pattern of the organic cathode material prepared in Example 1 of this invention;

[0021] Figure 2 This is a scanning electron microscope image of the organic cathode material prepared in Example 1 of the present invention;

[0022] Figure 3 The infrared spectrum of the organic cathode material prepared in Example 1 of this invention;

[0023] Figure 4 Thermogravimetric spectrum of the organic cathode material prepared in Example 1 of this invention;

[0024] Figure 5 This is a cyclic voltammetry curve of the organic cathode material prepared in Example 1 of the present invention in a zinc-ion battery;

[0025] Figure 6 The organic cathode material prepared in Example 1 of this invention is used in a zinc-ion battery at 0.02 Ag. -1 0.03Ag -1 0.05Ag -1 0.1Ag -1 0.2Ag -1 0.3Ag-1 0.5Ag -1 1Ag -1 2Ag -1 5Ag -1 and 0.02Ag -1 Rate performance at current density;

[0026] Figure 7 The organic cathode material prepared in Example 1 of this invention was used in a zinc-ion battery at a concentration of 0.1 Ag. -1 Long-cycle diagram of 1000 charge-discharge cycles at current density. Detailed Implementation

[0027] As can be seen from the background technology, organic cathode materials in multivalent ion batteries currently have unsatisfactory electrochemical performance in terms of specific capacity utilization, rate capability, and long cycle life, such as low actual specific capacity and rapid capacity decay during charge and discharge.

[0028] This invention provides an organic cathode material, the structural formula of which is:

[0029] Where n is a natural number greater than or equal to 1.

[0030] The present invention also provides a method for preparing the organic cathode material, the method comprising the following steps: dissolving 1,4-benzoquinone and 1,3-phenylenediamine in reaction solvent A and carrying out an oxidative addition reaction; after the reaction is completed, filtering is performed to obtain a filter cake; the filter cake is washed with a washing solvent and then dried to obtain the organic cathode material.

[0031] The synthetic route for this reaction is shown below:

[0032]

[0033] Furthermore, the method specifically includes the following steps: dissolving 1,4-benzoquinone and 1,3-phenylenediamine in reaction solvent A at a ratio of 0.2 g to 1.2 g of 1,3-phenylenediamine to 5 mL to 150 mL of reaction solvent A; and bubbling 0 mL / min into each 5 mL of reaction solvent A. -1 ~20mLmin -1 The ratio of the oxidizing gas flow is determined, and the oxidizing gas flow is introduced and reacted at 20℃~150℃ for 1h~48h. After the reaction is completed and cooled, the mixture is filtered to obtain a filter cake. The filter cake is washed with a washing solvent and then dried to obtain a black solid powder, which is the organic cathode material.

[0034] Furthermore, the reaction solvent A is methanol, ethanol, isopropanol, n-butanol, N,N-dimethylformamide, or N-methylpyrrolidone.

[0035] Furthermore, the oxidizing gas flow is an oxygen flow or an air flow.

[0036] This invention also provides another method for preparing the organic cathode material, which includes the following steps: dissolving 2,5-dichloro-1,4-benzoquinone and 1,3-phenylenediamine in reaction solvent B, and then heating under inert gas protection to carry out a condensation reaction; after the reaction is completed, filtering is performed to obtain a filter cake; the filter cake is washed with a washing solvent and then dried to obtain the organic cathode material.

[0037] The synthetic route for this reaction is shown below:

[0038]

[0039] Furthermore, the method specifically includes the following steps: 2,5-dichloro-1,4-benzoquinone and 1.1-2.2 grams of 1,3-phenylenediamine are dissolved in reaction solvent B at a ratio of 5-150 mL per gram of 2,5-dichloro-1,4-benzoquinone, and 1.1-2.2 grams of 1,3-phenylenediamine are dissolved in reaction solvent B. The mixture is reacted at 20°C-150°C for 1-48 hours under inert gas protection. After the reaction is complete and cooled, the mixture is filtered to obtain a filter cake. The filter cake is washed with a washing solvent and then dried to obtain a black solid powder, which is the organic cathode material.

[0040] Furthermore, the reaction solvent B is methanol, ethanol, isopropanol, n-butanol, pyridine, N,N-dimethylformamide, or N-methylpyrrolidone.

[0041] Furthermore, the inert gas is nitrogen, helium, or argon.

[0042] Furthermore, the washing solvent is one or more of methanol, ethanol, isopropanol, n-butanol, N,N-dimethylformamide, and water.

[0043] This invention also provides the application of the organic cathode material described above in the field of ion batteries.

[0044] The present invention will now be described in detail with reference to specific embodiments.

[0045] Example 1

[0046] 0.324 g (3 mmol) of 1,4-benzoquinone and 0.108 g (1 mmol) of 1,3-phenylenediamine were dissolved in 20 mL of N,N-dimethylformamide and reacted at 120 °C for 24 h. After the reaction was completed and cooled, the mixture was filtered to obtain a filter cake. The filter cake was washed three times with ethanol and water and then dried to obtain a black solid powder, which is the organic cathode material of the present invention.

[0047] Figure 1The image shows the X-ray diffraction pattern of the organic cathode material prepared in this embodiment. The main diffraction peak is a broad peak at 21°. It can be seen from the image that the organic cathode material in this invention is amorphous.

[0048] Figure 2 The image shows a scanning electron microscope (SEM) image of the organic cathode material prepared in this embodiment, which exhibits a granular distribution at the micrometer scale.

[0049] Figure 3 The image shows the infrared spectrum of the organic cathode material prepared in this embodiment. The main absorption peak range is around 1240 cm⁻¹. -1 1350cm -1 1500cm -1 and 1635cm -1 and 3056cm -1 .

[0050] Figure 4 The thermogravimetric spectrum of the organic cathode material prepared in this embodiment shows a weight loss of approximately 4.28% at around 100°C, followed by a significant weight loss after 277°C.

[0051] The organic cathode material prepared in this embodiment was used as the active material for the positive electrode of a zinc-ion battery. The organic cathode material, acetylene black, and polyvinylidene fluoride were mixed and ground in a mass ratio of 6:3:1. N-methylpyrrolidone was added dropwise during grinding, and the mixture was coated onto a stainless steel mesh and vacuum dried to form a positive electrode sheet. A zinc sheet was used as the negative electrode. (1 mol·L⁻¹) -1 A CR2032 coin cell was assembled using ZnSO4 solution as the electrolyte and glass fiber as the separator, and its electrochemical performance was tested.

[0052] Figure 5 The organic cathode material prepared in Example 1 of this invention is used in zinc-ion batteries at 0.1 mV s. -1 0.2mV s -1 0.3mV s -1 0.4mV s -1 0.5mV s -1 0.6mV s -1 0.8mV s -1 and 1mV s -1 Cyclic voltammetry curves at different scan rates. The oxidation peak is located around 0.89 V, and the reduction peak is located around 0.63 V. The redox peaks are distinct and symmetrical, indicating that the organic cathode material of this invention exhibits good cycle reversibility.

[0053] Figure 6 The organic cathode material prepared in this embodiment is used in zinc-ion batteries at 0.02Ag. -1 0.03Ag -10.05Ag -1 0.1Ag -1 0.2Ag -1 0.3Ag -1 0.5Ag -1 1Ag -1 2Ag -1 and 5Ag -1 Rate performance at current density corresponds to a discharge specific capacity of 124 mAh g. -1 104mAh g -1 92mAh g -1 81mAh g -1 60mAh g -1 46mAh g -1 38mAh g -1 24mAh g -1 17mAh g -1 and 14mAh g -1 When the current density drops back to 0.02Ag -1 At that time, the discharge specific capacity recovered to 93mAh g. -1 .

[0054] Figure 7 The organic cathode material prepared in this embodiment is used in a zinc-ion battery at a concentration of 0.1 Ag. -1 The long-cycle graph at current density shows a capacity retention of 66% after 1000 charge-discharge cycles.

[0055] The electrochemical performance obtained from the above tests, including discharge specific capacity, rate performance stability, and long-cycle capacity retention, is superior to existing cathode materials such as poly(1,4-benzoquinone-4,4'-diaminobiphenyl), poly(1,4-benzoquinone-ethylenediamine), poly(1,4-benzoquinone-urea), and poly(1,4-benzoquinone-1,4-phenylenediamine). For example, the discharge specific capacity of poly(1,4-benzoquinone-ethylenediamine) cathode material in the first cycle at a current density of 0.02 A / g is 102 mAh g. -1 After 250 charge-discharge cycles, the capacity retention rate is 49%, demonstrating the significant performance advantages of the quinone polymer cathode material of this invention.

[0056] Example 2

[0057] 0.324 g (3 mmol) of 1,4-benzoquinone and 0.389 g (3.6 mmol) of 1,3-phenylenediamine were dissolved in 5 mL of ethanol, and 20 mL of the solution was bubbled through the ethanol. -1An oxidizing gas stream was introduced and reacted at 75°C for 48 hours. After the reaction was completed and cooled, the mixture was filtered to obtain a filter cake. The filter cake was washed three times with methanol and water and then dried to obtain a black solid powder, which is the organic cathode material of the present invention.

[0058] Example 3

[0059] 0.324 g (3 mmol) of 1,4-benzoquinone and 0.065 g (0.6 mmol) of 1,3-phenylenediamine were dissolved in 5 mL of n-butanol, and 2 mL of the solution was bubbled through. -1 An oxidizing gas stream was introduced and reacted at 110°C for 1 hour. After the reaction was completed and cooled, the mixture was filtered to obtain a filter cake. The filter cake was washed three times with isopropanol and N,N-dimethylformamide and then dried to obtain a black solid powder, which is the organic cathode material of the present invention.

[0060] Example 4

[0061] 0.324 g (3 mmol) of 1,4-benzoquinone and 0.108 g (1 mmol) of 1,3-phenylenediamine were dissolved in 45 mL of isopropanol and reacted at 80 °C for 24 h. After the reaction was completed and cooled, the mixture was filtered to obtain a filter cake. The filter cake was washed three times with n-butanol and N,N-dimethylformamide and then dried to obtain a black solid powder, which is the organic cathode material of the present invention.

[0062] Example 5

[0063] 0.176 g (i.e., 1 mmol) of 2,5-dichloro-1,4-benzoquinone and 0.076 g (i.e., 0.7 mmol) of 1,3-phenylenediamine were dissolved in 10 mL of N-methylpyrrolidone and reacted at 140 °C for 1 h under helium protection. After the reaction was completed and cooled, the mixture was filtered to obtain a filter cake. The filter cake was washed three times with ethanol and water and then dried to obtain a black solid powder, which is the organic cathode material of the present invention.

[0064] Example 6

[0065] 0.176 g (i.e., 1 mmol) of 2,5-dichloro-1,4-benzoquinone and 0.141 g (i.e., 1.3 mmol) of 1,3-phenylenediamine were dissolved in 10 mL of N,N-dimethylformamide and reacted at 140 °C for 12 h under argon protection. After the reaction was completed and cooled, the mixture was filtered to obtain a filter cake. The filter cake was washed three times with ethanol and then dried to obtain a black solid powder, which is the organic cathode material of the present invention.

[0066] Example 7

[0067] 0.176 g (i.e., 1 mmol) of 2,5-dichloro-1,4-benzoquinone and 0.118 g (i.e., 1.1 mmol) of 1,3-phenylenediamine were dissolved in 20 mL of pyridine and reacted at 110 °C for 8 h under nitrogen protection. After the reaction was completed and cooled, the mixture was filtered to obtain a filter cake. The filter cake was washed three times with ethanol and N,N-dimethylformamide and then dried to obtain a black solid powder, which is the organic cathode material of the present invention.

[0068] Those skilled in the art will understand that the above-described embodiments are specific examples of implementing this application, and in practical applications, various changes in form and detail may be made without departing from the spirit and scope of this application. Any person skilled in the art can make their own modifications and alterations without departing from the spirit and scope of this application; therefore, the scope of protection of this application should be determined by the scope defined in the claims.

Claims

1. A method for preparing an organic cathode material, characterized in that, The method specifically includes the following steps: According to the ratio of 1 gram of 1,4-benzoquinone to 0.2 to 1.2 grams of 1,3-phenylenediamine dissolved in 5 to 150 mL of reaction solvent A, 1,4-benzoquinone and 1,3-phenylenediamine were dissolved in reaction solvent A; 0 mL of 1,4-benzoquinone and 1,3-phenylenediamine were bubbled into each 5 mL of reaction solvent A. -1 ~20mL min -1 The ratio of the oxidizing gas flow is determined, and the oxidizing gas flow is introduced and reacted at 20℃~150℃ for 1 h~48 h; after the reaction is completed and cooled, the mixture is filtered to obtain a filter cake; the filter cake is washed with a washing solvent and then dried to obtain a black solid powder, which is the organic cathode material. The structural formula of this organic cathode material is: Where n is a natural number greater than or equal to 1.

2. The method for preparing the organic cathode material according to claim 1, characterized in that, The reaction solvent A is methanol, ethanol, isopropanol, n-butanol, N,N-dimethylformamide, or N-methylpyrrolidone.

3. The method for preparing the organic cathode material according to claim 1, characterized in that, The oxidizing gas flow is an oxygen flow or an air flow.

4. A method for preparing an organic cathode material, characterized in that, The method includes the following steps: 2,5-Dichloro-1,4-benzoquinone and 1,3-phenylenediamine were dissolved in reaction solvent B, and then heated under inert gas protection to carry out a condensation reaction. After the reaction was completed, the mixture was filtered to obtain a filter cake. The filter cake was washed with a washing solvent and then dried to obtain the organic cathode material. The structural formula of this organic cathode material is: Where n is a natural number greater than or equal to 1.

5. The method for preparing the organic cathode material according to claim 4, characterized in that, The method specifically includes the following steps: According to the ratio of 1.1 g to 2.2 g of 1,3-phenylenediamine dissolved in 5 mL to 150 mL of reaction solvent B, 2,5-dichloro-1,4-benzoquinone and 1,3-phenylenediamine were dissolved in reaction solvent B and reacted at 20 °C to 150 °C for 1 h to 48 h under inert gas protection. After the reaction was completed and cooled, the mixture was filtered to obtain a filter cake. The filter cake was washed with washing solvent and dried to obtain a black solid powder, which is the organic cathode material.

6. The method for preparing the organic cathode material according to claim 5, characterized in that, The reaction solvent B is methanol, ethanol, isopropanol, n-butanol, pyridine, N,N-dimethylformamide, or N-methylpyrrolidone.

7. The method for preparing the organic cathode material according to claim 1 or 4, characterized in that, The washing solvent is one or more of methanol, ethanol, isopropanol, n-butanol, N,N-dimethylformamide, and water.

Citation Information

Patent Citations

  • Porous carbon coated ternary positive electrode material as well as preparation method and application thereof

    CN116344761A