Low-corrosion chip photoresist stripping liquid as well as preparation method and application thereof
By using a combination of amine compounds, amide solvents, hydroxylated naphthoquinone and quinone salts in the photoresist stripping solution, the corrosion of semiconductor chip materials by the photoresist stripping solution is solved. Problem, more efficient glue removal and longer life-long chip cleaning effect are achieved.
Patent Information
- Application Number
- CN202410775848.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-11-08
AI Technical Summary
The existing photoresist stripping liquid is prone to corrode the semiconductor chip material when removing the photoresist, affecting the chip quality and reliability.
Using low-corrosion chip photoresist stripping liquid, including amine compounds, amide solvents, hydroxylated naphthoquinone and quinone salts, the combination of these components forms a protective film and reduces electrochemical corrosion, effectively inhibiting the corrosion of metal electrodes. .
While ensuring the glue removal effect, it significantly reduces the corrosion of metal electrodes, extends the chip life, and improves the cleaning quality of semiconductor chips.
Smart Images

Figure CN118915405A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to photoresist stripping liquid technology, in particular to a low-corrosion chip photoresist stripping liquid, a preparation method and application thereof. Background Art
[0002] In semiconductor manufacturing, photoresist stripping is a key process in chip manufacturing. Incomplete photoresist stripping may lead to the scrapping of the entire batch of chips. Therefore, the surface state of the chip and the degree of removal of contaminants are one of the most important factors affecting the chip yield and device quality and reliability. The selection and use of photoresist stripping liquid directly affects the quality and efficiency of chip manufacturing.
[0003] At present, photoresist stripping liquid is mainly composed of polar organic solvents, strong alkali and / or water, etc. The photoresist on the semiconductor chip is removed by immersing the semiconductor chip in the photoresist stripping liquid or washing the semiconductor chip with the photoresist stripping liquid. In this process, the chip material may be corroded due to the removal of the photoresist. Therefore, a photoresist stripping liquid with excellent photoresist removal effect and capable of minimizing the corrosion of the chip material is needed. Summary of the invention
[0004] The purpose of the present invention is to provide a low-corrosion chip photoresist stripping solution to address the problem that the current photoresist stripping solution corrodes chip materials. The low-corrosion chip photoresist stripping solution has low corrosion to chip materials and can be used for cleaning photoresists in semiconductor manufacturing.
[0005] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising", etc. and similar meanings, as well as closed-ended "composed of", "composed of", etc. and similar meanings.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a low-corrosion chip photoresist stripping solution, comprising the following components in weight proportions:
[0007] 5-15 parts of amine compounds;
[0008] 60-80 parts of amide solvent;
[0009] 4-10 parts of hydroxylated naphthoquinone;
[0010] Quinone salt 0.1-0.5 parts.
[0011] Furthermore, the amine compound is one or more of alcohol amine, aromatic amine and aliphatic amine.
[0012] Furthermore, the alcoholamine is one or more of monoethanolamine, methylmonoethanolamine, diethanolamine, triethanolamine, n-propanolamine, isopropanolamine, 2-(diethylamino)ethanol, ethyldiethanolamine, diglycolamine and isomers of the above alcoholamines.
[0013] Furthermore, the alcoholamine is preferably a mixture of methyl monoethanolamine and monoethanolamine.
[0014] Furthermore, the alcoholamine is more preferably a mixture of methylmonoethanolamine and monoethanolamine in a mass ratio of 1-3:1.
[0015] Furthermore, the alcoholamine is most preferably a mixture of methyl monoethanolamine and monoethanolamine in a mass ratio of 2:1.
[0016] Furthermore, the aromatic amine is one or more of aniline, o-phenylenediamine, p-toluidine, benzidine and diphenylamine.
[0017] Furthermore, the fatty amine is one or more of methylamine, ethylamine, propylamine, isopropylamine, butylamine, dimethylamine, diethylamine and trimethylamine.
[0018] Furthermore, the amine compound is 10-13 parts.
[0019] Furthermore, the amide solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, N-methylformamide, N-propylformamide, N,N-diethylacetamide, N-methyl-2-pyrrolylformamide, N-ethyl-2-pyrrolylformamide, N-propyl-2-pyrrolylformamide and N-ethylformamide.
[0020] Furthermore, the amide solvent is 65-78 parts.
[0021] Furthermore, the hydroxylated naphthoquinone is one or more of 2-hydroxy-1,4-naphthoquinone, 5,8-dihydroxy-1,4-naphthoquinone, 2,3-dichloro-5,8-dihydroxy-1,4-naphthoquinone and 5-hydroxy-p-naphthoquinone.
[0022] Furthermore, the hydroxylated naphthoquinone is preferably 2-hydroxy-1,4-naphthoquinone.
[0023] Furthermore, the hydroxylated naphthoquinone is 6-8 parts.
[0024] Furthermore, the quinone salt is one or more of tetrahydroxy-p-benzoquinone disodium salt, 2,6-dichloro-N-(p-hydroxyphenyl)-p-benzoquinone imine sodium salt, pyrroloquinoline benzoquinone sodium salt, 1,2-naphthoquinone-4-sulfonate sodium, anthraquinone-1,8-disulfonate dipotassium and anthraquinone-2,6-disulfonate disodium.
[0025] Furthermore, the quinone salt is preferably tetrahydroxy-p-benzoquinone disodium salt.
[0026] Furthermore, the quinone salt is 0.2-0.5 parts.
[0027] Another object of the present invention is to disclose a method for preparing a low-corrosion chip photoresist stripping solution, comprising the following steps:
[0028] Hydroxylated naphthoquinone and quinone salt are added to an amide solvent and mixed evenly, and then an amine compound is added and mixed evenly to prepare a low-corrosion chip photoresist stripping solution.
[0029] Another object of the present invention is to disclose the application of a low-corrosion chip photoresist stripping solution in the field of cleaning semiconductor chips.
[0030] Further, the semiconductor chip is cleaned using a low-corrosion chip photoresist stripping solution, comprising the following steps:
[0031] Step 1: Immerse the semiconductor chip in a low-corrosion chip photoresist stripping solution;
[0032] Step 2: Rinse the soaked semiconductor chip in ultrapure water to complete the cleaning of the semiconductor chip.
[0033] Furthermore, the soaking temperature in step 1 is 80-95°C.
[0034] Furthermore, the soaking time in step 1 is 10-40 minutes.
[0035] Furthermore, in step 2, the semiconductor chip after immersion is rinsed in ultrapure water at least twice.
[0036] The low-corrosion chip photoresist stripping solution, preparation method and application thereof of the present invention have the following advantages compared with the prior art:
[0037] (1) The present invention uses a combination of hydroxylated naphthoquinone and quinone salts. On the one hand, the lone pair electrons of a large number of O atoms in hydroxylated naphthoquinone will form coordination bonds with the 2p orbital of metal atoms to undergo chemical adsorption, thereby preventing the corrosive medium from contacting the metal surface. On the other hand, the large π bonds in hydroxylated naphthoquinone and quinone salts will also form coordination bonds with the 2p orbital of metal atoms, further enhancing chemical adsorption. At the same time, the anions generated by the ionization of quinone salts will be adsorbed in the anode region, preventing the metal from losing electrons at the anode, thereby further reducing metal corrosion. In addition, since the carbonyl functional groups in the structures of hydroxylated naphthoquinone and quinone salts are redox active centers, they have good electrochemical activity and are excellent carriers for electron transfer. Therefore, the two can be synergistically reduced in the cathode region of the electrochemical reaction, thereby reducing the electrochemical corrosion of the metal.
[0038] (2) The amine compounds used in the present invention have strong alkalinity and can decompose the molecular chains in the photoresist into small molecules, effectively removing the photoresist that has been ashed after etching. Compared with NaOH and KOH, the amine compounds themselves have amine groups, which have a corrosion inhibition effect on metals such as Al and Ni, greatly reducing the corrosion of metal electrodes. At the same time, the amine compounds are soluble in amide solvents, and the two together accelerate the stripping and dissolution of the photoresist. Using a variety of amine compounds as a combination has the effect of enhancing the dissolution of photoresist and increasing the lifespan.
[0039] (3) The amide solvent used in the present invention is a strong polar solvent, which can effectively swell and soften the photoresist, so that the molecular chain disentangles the resin layer and swells, further accelerating the dissolution of the photoresist, so that the amine compound can contact the photoresist in a larger range and react with it to dissolve the photoresist.
[0040] In summary, the low-corrosion chip photoresist stripping solution of the present invention not only ensures the degumming ability, but also forms a protective film on the metal surface through the synergistic effect of hydroxylated naphthoquinone and quinone salts, and reduces electrochemical corrosion as a redox center, thereby having a good protective effect on Al and Ni metal electrodes, effectively inhibiting their corrosion and prolonging their life. The low-corrosion chip photoresist stripping solution of the present invention has very good application prospects and large-scale industrial promotion potential in the field of semiconductor chip cleaning. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is a 500-fold magnified image of an Al chip that has not been immersed in photoresist stripping solution under a microscope;
[0042] Figure 2 This is a 500-fold magnified image of a Ni chip that has not been immersed in photoresist stripping solution under a microscope;
[0043] Figure 3 This is a picture of an Al chip after being immersed in the photoresist stripping solution prepared in Example 1, magnified 500 times under a microscope;
[0044] Figure 4 This is a picture of a Ni chip after being immersed in the photoresist stripping solution prepared in Example 1, magnified 500 times under a microscope;
[0045] Figure 5 This is a picture of the Al chip magnified 500 times under a microscope after being treated with the photoresist stripping solution prepared in Comparative Example 1;
[0046] Figure 6 This is a picture of the Ni chip magnified 500 times under a microscope after being treated with the photoresist stripping solution prepared in Comparative Example 1. DETAILED DESCRIPTION
[0047] The present invention is further described below with reference to embodiments.
[0048] Examples 1-6
[0049] The present embodiments 1-6 disclose a variety of low-corrosion chip photoresist stripping solutions, the components and weight ratios of which are shown in Table 1, and the preparation methods thereof are as follows:
[0050] Step 1: Weigh each component separately;
[0051] Step 2: Add hydroxylated naphthoquinone and quinone salt into an amide solvent, stir evenly, then add an amine compound, stir evenly, and prepare a low-corrosion chip photoresist stripping solution.
[0052] Table 1 Components and weight ratios of low-corrosion chip photoresist stripping solutions of Examples 1-6
[0053]
[0054] Comparative Examples 1-3
[0055] Comparative Examples 1-3 disclose a variety of chip photoresist stripping solutions, the components and weight ratios of which are shown in Table 2, and the preparation methods thereof are the same as those of Example 1.
[0056] Table 2 Comparative Examples 1-3 Chip Photoresist Stripping Solution Components and Weight Ratios
[0057]
[0058] The various properties of the above embodiments or comparative examples are tested below.
[0059] The test method for performance 1 corrosion is:
[0060] The sample coated with 5μm thick positive photoresist was immersed in 85℃ photoresist stripping solution for 30min, taken out and rinsed with ultrapure water for 5min, then dried with nitrogen, and the chip surface was observed with a metallographic microscope. Ultrapure water is ultrapure water with a resistance of at least 18MΩ.
[0061] Figure 1 This is a 500-fold magnified image of an Al chip that has not been immersed in photoresist stripping solution under a microscope; Figure 2 This is a 500-fold magnified image of a Ni chip that has not been immersed in photoresist stripping solution under a microscope; Figure 3 This is a picture of an Al chip after being immersed in the photoresist stripping solution prepared in Example 1, magnified 500 times under a microscope; Figure 4 This is a picture of a Ni chip after being immersed in the photoresist stripping solution prepared in Example 1, magnified 500 times under a microscope; Figure 5This is a picture of the Al chip magnified 500 times under a microscope after being treated with the photoresist stripping solution prepared in Comparative Example 1; Figure 6 This is a picture of the Ni chip magnified 500 times under a microscope after being treated with the photoresist stripping solution prepared in Comparative Example 1.
[0062] by Figure 1 and Figure 2 As a basis for comparison. Figure 3 and Figure 4 It can be seen that there is basically no corrosion on the Al and Ni chips after being cleaned with the chip photoresist stripping solution prepared in Example 1 of the present invention. Figure 5 and Figure 6 It can be seen that the Al and Ni chips cleaned with the chip photoresist stripping solution prepared in Comparative Example 1 have been corroded.
[0063] Performance 2 The test method for metal corrosion rate is:
[0064] The four-probe method was used to test the corrosion rate of different photoresist stripping solutions on metal.
[0065] The specific test method is: immerse 2cm×2cm Al and Ni sheets in photoresist stripping solution at 85°C for 30 minutes respectively.
[0066] Then the thickness of Al and Ni sheets before and after immersion in photoresist stripping solution was measured by four-probe method, and their corrosion rates were calculated ( Right now Minutes, also known as "etching rate"), thereby examining the corrosion rate of different photoresist stripping solutions on metals.
[0067] Table 3 Test data
[0068]
[0069] Based on Table 3, it can be seen that the metal corrosion rate of the embodiment of the present invention at the degumming temperature of 85°C is
[0070] In Comparative Examples 1-3, the metal corrosion rate at the degumming temperature of 85°C is
[0071]
[0072] It can be seen that the photoresist stripping solution provided in the embodiment of the present invention has a good protective effect on the photoresist and metal electrodes such as Al and Ni, and can effectively inhibit the corrosion of different metals.
[0073] From the comparison between the embodiments of the present invention and comparative examples 1-3, it can be seen that: when hydroxylated naphthoquinone and quinone salts are present in the stripping solution at the same time, the two can exert an unexpected synergistic effect, thereby achieving excellent anti-corrosion effect; when hydroxylated naphthoquinone is not added in comparative example 1, a protective layer cannot be formed on the metal surface, resulting in an increase in the metal corrosion rate; quinone salts are not added in comparative example 2, resulting in an increase in the metal corrosion rate; compared with embodiment 1, comparative example 3 uses disodium ethylenediaminetetraacetic acid instead of quinone salts. Due to the lack of quinone structure, it does not further serve as a redox center together with hydroxylated naphthoquinone to reduce electrochemical corrosion, resulting in an increase in the metal corrosion rate.
[0074] In summary, the present invention provides a type of low-corrosion chip photoresist stripping solution, which exerts an unexpected low-corrosion effect through the selection and combination of specific components such as hydroxylated naphthoquinone, quinone salts and amine compounds, and amide solvents.
[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A low-corrosion chip photoresist stripping solution, characterized in that: The composition includes the following components in weight ratio: 5-15 parts of amine compounds; 60-80 parts of amide solvent; 4-10 parts of hydroxylated naphthoquinone; Quinone salt 0.1-0.5 parts.
2. The low-corrosion chip photoresist stripping solution according to claim 1, characterized in that: The amine compound is one or more of alcohol amine, aromatic amine and aliphatic amine.
3. The low-corrosion chip photoresist stripping solution according to claim 1, characterized in that: The amide solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, N-methylformamide, N-propylformamide, N,N-diethylacetamide, N-methyl-2-pyrrolylformamide, N-ethyl-2-pyrrolylformamide, N-propyl-2-pyrrolylformamide and N-ethylformamide.
4. The low-corrosion chip photoresist stripping solution according to claim 1, characterized in that: The hydroxylated naphthoquinone is one or more of 2-hydroxy-1,4-naphthoquinone, 5,8-dihydroxy-1,4-naphthoquinone, 2,3-dichloro-5,8-dihydroxy-1,4-naphthoquinone and 5-hydroxy-p-naphthoquinone.
5. The low-corrosion chip photoresist stripping solution according to claim 1, characterized in that: The quinone salt is one or more of tetrahydroxy-p-benzoquinone disodium salt, 2,6-dichloro-N-(p-hydroxyphenyl)-p-benzoquinone imine sodium salt, pyrroloquinoline benzoquinone sodium salt, 1,2-naphthoquinone-4-sulfonate sodium, anthraquinone-1,8-disulfonate dipotassium and anthraquinone-2,6-disulfonate disodium.
6. A method for preparing the low-corrosion chip photoresist stripping solution according to any one of claims 1 to 5, comprising the following steps: Hydroxylated naphthoquinone and quinone salt are added to an amide solvent and mixed evenly, and then an amine compound is added and mixed evenly to prepare a low-corrosion chip photoresist stripping solution.
7. Use of the low-corrosion chip photoresist stripping solution according to any one of claims 1 to 5 in the field of cleaning semiconductor chips.
8. The use according to claim 7, characterized in that: The method of cleaning a semiconductor chip using a low-corrosion chip photoresist stripping solution comprises the following steps: Step 1: Immerse the semiconductor chip in a low-corrosion chip photoresist stripping solution; Step 2: Rinse the soaked semiconductor chip in ultrapure water to complete the cleaning of the semiconductor chip.
9. The use according to claim 8, characterized in that: Step 1: The soaking temperature is 80-95°C.
10. The use according to claim 8, characterized in that: Step 1: Soaking time is 10-40 minutes.
Citation Information
Cited By
Photoresist stripping liquid as well as preparation method and application thereof
CN120669493A