A 18MND5 steel plate for nuclear power injection box and its production method

By optimizing the production process of 18MND5 steel plates, the problem of insufficient thickness and tensile strength of existing nuclear power plant safety box steel plates has been solved, the mechanical properties have been significantly improved, and the high-strength requirements of the emergency cooling system of nuclear power plants have been met.

CN117165852BActive Publication Date: 2024-10-25NANJING IRON & STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202311095147.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-29
Publication Date
2024-10-25
Estimated Expiration
2043-08-29

AI Technical Summary

Technical Problem

The existing steel plates used for safety boxes in nuclear power plants have narrow thickness and width, and poor tensile strength at room temperature and 150°C, making it difficult to meet the high-strength requirements of the emergency cooling system of nuclear power plants.

Method used

The production method of 18MND5 steel plate is adopted, including converter smelting, LF+RH out-of-furnace refining, dynamic light pressure continuous casting, electromagnetic stirring technology, one-step high-temperature and high-pressure rolling, offline quenching + tempering heat treatment, optimizing the chemical composition and organizational structure, and improving Hardenability and temper embrittlement resistance of steel plates.

Benefits of technology

Produce 18MND5 steel plate with excellent mechanical properties. The yield strength and tensile strength are significantly improved. The high temperature tensile strength at 150℃ is ≥620MPa. The transverse impact energy at 0℃ is ≥200J. It has excellent welding performance and is suitable for the high and low temperatures of the safety box of nuclear power plants. environment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses an 18MND5 steel plate for nuclear power injection box and a production method thereof; it belongs to the technical field of steel production; its chemical composition is as follows: C, Mn, P, S, Si, Cr, Mo, Ni, V, Nb, Ti, Alt, Cu, N, H, As, Sn, Co, and the rest is Fe and impurities; its steps are as follows: smelting, heating, rolling, cooling and heat treatment process. The present invention adopts converter smelting + LF / RH furnace refining, which makes up for the process operation shortcomings of reduction deoxidation, alloying, and inclusion sedation and floating; in addition, the present invention adopts large thick continuous casting billets, and the steel quality of the billet rolled steel plate is more uniform and stable; the steel plate produced by the present invention has excellent and stable mechanical properties, and the performance after PWHT also meets the requirements, the flaw detection is qualified, the steel plate composition is uniform, the welding performance is excellent, the comprehensive mechanical properties are excellent, it has high compressive strength, low temperature toughness, and excellent creep resistance, and can realize the economic and mass production of steel plates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel production, and relates to a steel plate and a production method thereof, and specifically to an 18MND5 steel plate for a nuclear power injection box and a production method thereof. Background Art

[0002] At present, the safety injection system (RIS) of nuclear power plants is used to complete the emergency cooling function of the core when a loss of water accident occurs in the coolant system of the nuclear reactor or a pipeline rupture occurs in the main steam system. The injection tank is a medium-pressure safety injection system that stores boric water (C B -2100ppm) container,

[0003] The nuclear power technology injection boxes currently in use are usually AP1000 and CAP1400 third-generation nuclear power technology injection boxes. Their disadvantages are that the steel plates are relatively thin, the width is relatively narrow, and the requirements for tensile strength at room temperature and 150°C are generally poor. Therefore, it is worth considering how to solve the above problems. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide an 18MND5 steel plate for nuclear power injection box with excellent mechanical properties;

[0005] Another object of the present invention is to provide a method for producing 18MND5 steel plates for nuclear power injection boxes.

[0006] Technical solution: The 18MND5 steel plate for a nuclear power injection box of the present invention has the following chemical compositions and weight percentages: C: 0.16%-0.20%, Mn: 1.35%-1.60%, P≤0.008%, S≤0.005%, Si: 0.15%-0.30%, Cr≤0.10%, Mo: 0.45%-0.55%, Ni: 0.60%-0.80%, V≤0.05%, Nb≤0.02%, Ti≤0.03%, Alt: 0.02%-0.04%, Cu≤0.10%, N≤0.006%, H≤0.006%, As≤0.01%, Sn≤0.05%, Co≤0.10%, and the rest is Fe and impurities;

[0007] The thickness of the steel plate is 30-150 mm, and the structure of the steel plate is mainly bainite;

[0008] The production method includes smelting, continuous casting, heating, rolling, cooling after rolling and heat treatment processes, and the specific steps are as follows:

[0009] Smelting process: molten iron pretreatment, converter smelting, LF+RH refining outside the furnace;

[0010] Continuous casting process: dynamic soft reduction and electromagnetic stirring technology are adopted, and the center segregation of continuous casting billet is C0.5 level;

[0011] Heating process: After the ingot is cooled for ≥48h, it is heated in a step-beam heating furnace;

[0012] Rolling process: Taking advantage of the large rolling force of the 5M rolling mill, a one-stage high-temperature and high-reduction rolling process is adopted, with the starting rolling temperature ≥1000℃ and the maximum single-pass reduction rate of 20% to 25%, so that the rolling deformation can effectively penetrate into the core;

[0013] Cooling process: the rolled steel plate is air-cooled on a cooling bed, and then slowly cooled by stacking;

[0014] Heat treatment process: The steel plate adopts offline quenching + tempering process. The holding time of the quenching process is 1.5min / mm×t+40min, t is the thickness of the steel plate; the holding time of the tempering process is 2.0min / mm×t+80min, t is the thickness of the steel plate;

[0015] Wherein, the heating coefficient in the heating process is ≥10.0min / cm, and the heating temperature is 1180°C to 1220°C;

[0016] The first-stage rolling has a starting rolling temperature of ≥1000°C;

[0017] In the heat treatment process, the normalizing temperature is 900±10°C and the tempering temperature is 680±20°C.

[0018] The invention adopts the method of controlling the content of C, Mn, Ni and Mo elements of the steel according to the standard upper limit in order to ensure the hardenability of the steel plate and the stability of the quenched and tempered structure of the steel plate; C in the heat-treated structure of the steel mainly exists in the form of FeC cementite compound; FeC cementite in the quenched and tempered heat-treated steel is uniformly and finely dispersed, and becomes a phase for improving the room temperature and 150 DEG C tensile strength of the steel plate; Mn, Ni and Mo are both solid solution strengthening elements and prevent the diffusion and movement of elements in the metastable state structure phase of the steel plate, thereby improving the hardenability of the steel, the stability of the tempered structure, and the body strength and 150 DEG C tensile performance of the steel; and the design without Nb, V and Ti microalloy components ensures that the actual grain size of the steel plate is uniform, and at the same time reduces the precipitation of microalloy element carbides caused by metal phase change to generate local stress, thereby improving the stainless steel surfacing quality on the surface of the steel plate.

[0019] Beneficial effects: Compared with the prior art, the present invention has the following characteristics: 1. The converter smelting + LF / RH refining outside the furnace is adopted. Compared with electric furnace steelmaking, the process operation shortcomings of reduction deoxidation, alloying, and inclusion calming and floating are made up, and the purity of steel and the control of other harmful impurity elements have surpassed the production process of electric furnace steelmaking; 2. The large thick continuous casting billet (460mm) is adopted. Compared with the steel plate rolled from the steel ingot, the steel plate rolled from the casting billet has higher uniformity and stability, higher yield rate and lower cost; 3. The mechanical properties are excellent. The chemical composition is optimized in the present invention, and the content of C, Mn, Ni and Mo elements is added according to the standard upper limit, which can improve The hardenability and temper embrittlement resistance of the steel ensure the mechanical properties of the steel plate in medium and high temperature environments; 4. The steel plate produced by the present invention has excellent and stable mechanical properties, the yield strength is distributed between 530MPa and 630MPa, the tensile strength is distributed between 650MPa and 710MPa, the high-temperature tensile tensile strength at 150°C is ≥620Mpa, the impact energy of the lateral impact at 0°C is ≥200J, the performance after PWHT also meets the requirements, the flaw detection is qualified, the steel plate has uniform composition, excellent welding performance, excellent comprehensive mechanical properties, high compressive strength, low-temperature toughness, and excellent creep resistance, and can realize economical and mass production of steel plates. DETAILED DESCRIPTION

[0020] The present invention will be further described below in conjunction with the embodiments.

[0021] Example 1

[0022] The present embodiment provides an 18MND5 steel plate for a nuclear power injection box, which has a thickness of 88 mm and a composition content (wt): C: 0.18%, Mn: 1.45%, P: 0.005%, S: 0.001%, Si: 0.17%, Cr: 0.02%, Mo: 0.49%, Ni: 0.65%, V: 0.003%, Nb: 0.003%, Ti: 0.011%, Alt: 0.027%, Cu: 0.02%, N: 0.0030%, As: 0.006%, Sn: 0.002%, Co: 0.001%, and the rest is Fe and impurities.

[0023] The production method of the steel plate comprises the following steps:

[0024] Steelmaking process: hot metal pretreatment, converter smelting, LF+RH refining outside the furnace;

[0025] Continuous casting process: dynamic soft reduction and electromagnetic stirring technology are used, the center segregation of the continuous casting billet is C0.5 level, and the thickness of the billet is 320mm;

[0026] Heating process: The billet is cooled for 65 hours and then heated in a heating furnace with a heating coefficient of 11.1 min / cm and a heating temperature of 1198°C.

[0027] Rolling process: One-stage rolling process is adopted, the starting rolling temperature is 1090℃, the final rolling temperature is 970℃, and the rolling passes are 13;

[0028] Cooling process: the rolled steel plate is air-cooled on a cooling bed; then it is stacked and cooled offline, with a stacking temperature of ≥300°C and a stacking cooling time of 52h;

[0029] Heat treatment process: After the steel plate is trimmed, it is quenched and tempered, the quenching temperature is 909℃, the total time in the furnace is 174min, and it is water-cooled after it is taken out of the furnace; the tempering temperature is 683℃, the total time in the furnace is 256min, and it is air-cooled after it is taken out of the furnace;

[0030] NDT process: The steel plate is inspected and accepted according to the NDT requirements of EN 10160S3E4 and the NDT is qualified.

[0031] The mechanical properties are: yield strength 568MPa, tensile strength 700MPa, elongation after break 22%, high temperature tensile strength at 150℃ 670MPa, lateral impact energy Akv at 0℃: 248J, 238J, 228J, average 238J; yield strength after 615℃ PWHT 555MPa, tensile strength 668MPa, elongation after break 25%, high temperature tensile strength at 150℃ 660MPa, lateral impact energy Akv at 0℃: 265J, 256J, 241J, average 254J.

[0032] Example 2

[0033] The present embodiment provides an 18MND5 steel plate for a nuclear power injection box, with a thickness of 105 mm and a composition content (wt): C: 0.18%, Mn: 1.45%, P: 0.005%, S: 0.001%, Si: 0.17%, Cr: 0.02%, Mo: 0.49%, Ni: 0.65%, V: 0.003%, Nb: 0.003%, Ti: 0.011%, Alt: 0.027%, Cu: 0.02%, N: 0.0030%, As: 0.006%, Sn: 0.002%, Co: 0.001%, and the rest are Fe and impurities.

[0034] The production method of the steel plate comprises the following steps:

[0035] Steelmaking process: hot metal pretreatment, converter smelting, LF+RH refining outside the furnace;

[0036] Continuous casting process: dynamic soft reduction and electromagnetic stirring technology are used, the center segregation of the continuous casting billet is C0.5 level, and the thickness of the billet is 320mm;

[0037] Heating process: The billet is cooled for 65 hours and then heated in a heating furnace with a heating coefficient of 11.1 min / cm and a heating temperature of 1197°C.

[0038] Rolling process: One-stage rolling process is adopted, the starting rolling temperature is 1080℃, the final rolling temperature is 990℃, and the rolling passes are 11;

[0039] Cooling process: the steel plate after rolling is air-cooled on the cooling bed; then it is stacked and cooled offline, the stacking temperature is ≥300℃, and the stacking time is 61h;

[0040] Heat treatment process: After the steel plate is trimmed, it is quenched and tempered, the quenching temperature is 905℃, the total time in the furnace is 198min, and it is water-cooled after it is taken out of the furnace; the tempering temperature is 688℃, the total time in the furnace is 291min, and it is air-cooled after it is taken out of the furnace;

[0041] NDT process: The steel plate is inspected and accepted according to the NDT requirements of EN 10160S3E4 and the NDT is qualified.

[0042] The mechanical properties are: yield strength 565MPa, tensile strength 695MPa, elongation at break 21%, high temperature tensile strength at 150℃ 655MPa, lateral impact energy Akv at 0℃: 211J, 218J, 215J, average 215J; yield strength after 615℃ PWHT 530MPa, tensile strength 665MPa, elongation 24%, high temperature tensile strength at 150℃ 630MPa, lateral impact energy Akv at 0℃: 252J, 253J, 246J, average 250J.

[0043] In summary, the present invention adopts a composition design with composite additions of Mn, Ni, and Mo elements, strict control of elements such as P and S, continuous casting electromagnetic stirring and continuous casting billet C-type segregation precise control technology, high-temperature heating, and one-stage rolling to produce 18MND5 steel plates for nuclear power injection boxes with excellent performance. The 88mm and 105mm specifications of 18MND5 steel plates meet the current requirements for steel plates for nuclear power technology injection boxes. The steel plate structure is bainite, and the flaw detection meets the requirements of EN 10160S3E4. The yield strength of the steel plate is distributed between 530MPa and 630MPa, the tensile strength is distributed between 650MPa and 710MPa, the high-temperature tensile strength at 150℃ is ≥620Mpa, and the transverse impact energy at 0℃ is ≥200J. The performance after PWHT also meets the requirements and is qualified in flaw detection. The steel plate has uniform composition, excellent welding performance, excellent comprehensive mechanical properties, high compressive strength, low-temperature toughness, and excellent creep resistance, which can realize economical and mass production of steel plates.

Claims

1. A 18MND5 steel plate for nuclear power injection box, characterized in that: The thickness is 88mm, and its chemical composition and weight percentage are: C: 0.18%, Mn: 1.45%, P: 0.005%, S: 0.001%, Si: 0.17%, Cr: 0.02%, Mo: 0.49%, Ni: 0.65%, V: 0.003%, Nb: 0.003%, Ti: 0.011%, Alt: 0.027%, Cu: 0.02%, N: 0.0030%, As: 0.006%, Sn: 0.002%, Co: 0.001%, the rest are Fe and impurities; The production method comprises the following steps: Steelmaking process: hot metal pretreatment, converter smelting, LF+RH refining outside the furnace; Continuous casting process: dynamic soft reduction and electromagnetic stirring technology are used, the center segregation of the continuous casting billet is C0.5 level, and the thickness of the billet is 320mm; Heating process: The billet is cooled for 65 hours and then heated in a heating furnace with a heating coefficient of 11.1 min / cm and a heating temperature of 1198°C. Rolling process: One-stage rolling process is adopted, the starting rolling temperature is 1090℃, the final rolling temperature is 970℃, and the rolling passes are 13; Cooling process: the rolled steel plate is air-cooled on a cooling bed; then it is stacked and cooled offline, with a stacking temperature of ≥300°C and a stacking cooling time of 52h; Heat treatment process: After the steel plate is trimmed, it is quenched and tempered, the quenching temperature is 909℃, the total time in the furnace is 174min, and it is water-cooled after it is taken out of the furnace; the tempering temperature is 683℃, the total time in the furnace is 256min, and it is air-cooled after it is taken out of the furnace; Flaw detection process: The steel plate is inspected and accepted according to the flaw detection requirements of EN 10160 S3E4, and the flaw detection is qualified; The mechanical properties are: yield strength 568MPa, tensile strength 700MPa, elongation after break 22%, high temperature tensile strength at 150℃ 670MPa, lateral impact energy Akv at 0℃: 248J, 238J, 228J, average 238J; yield strength after 615℃ PWHT 555MPa, tensile strength 668MPa, elongation after break 25%, high temperature tensile strength at 150℃ 660MPa, lateral impact energy Akv at 0℃: 265J, 256J, 241J, average 254J.

2. A 18MND5 steel plate for nuclear power injection box, characterized in that: The thickness is 105mm, and its chemical composition and weight percentage are: C: 0.18%, Mn: 1.45%, P: 0.005%, S: 0.001%, Si: 0.17%, Cr: 0.02%, Mo: 0.49%, Ni: 0.65%, V: 0.003%, Nb: 0.003%, Ti: 0.011%, Alt: 0.027%, Cu: 0.02%, N: 0.0030%, As: 0.006%, Sn: 0.002%, Co: 0.001%, the rest are Fe and impurities; The production method comprises the following steps: Steelmaking process: hot metal pretreatment, converter smelting, LF+RH refining outside the furnace; Continuous casting process: dynamic soft reduction and electromagnetic stirring technology are used, the center segregation of the continuous casting billet is C0.5 level, and the thickness of the billet is 320mm; Heating process: The billet is cooled for 65 hours and then heated in a heating furnace with a heating coefficient of 11.1 min / cm and a heating temperature of 1197°C. Rolling process: One-stage rolling process is adopted, the starting rolling temperature is 1080℃, the final rolling temperature is 990℃, and the rolling passes are 11; Cooling process: the steel plate after rolling is air-cooled on the cooling bed; then it is stacked and cooled offline, the stacking temperature is ≥300℃, and the stacking time is 61h; Heat treatment process: After the steel plate is trimmed, it is quenched and tempered, the quenching temperature is 905℃, the total time in the furnace is 198min, and it is water-cooled after it is taken out of the furnace; the tempering temperature is 688℃, the total time in the furnace is 291min, and it is air-cooled after it is taken out of the furnace; Flaw detection process: The steel plate is inspected and accepted according to the flaw detection requirements of EN 10160 S3E4, and the flaw detection is qualified; The mechanical properties are: yield strength 565MPa, tensile strength 695MPa, elongation after break 21%, high temperature tensile strength at 150℃ 655MPa, lateral impact energy Akv at 0℃: 211J, 218J, 215J, average 215J; yield strength after 615℃ PWHT 530MPa, tensile strength 665MPa, elongation after break 24%, high temperature tensile strength at 150℃ 630MPa, lateral impact energy Akv at 0℃: 252J, 253J, 246J, average 250J.

Citation Information

Cited By

  • Preparation method of high-temperature-resistant die welding nuclear power steel 18MND5

    CN121737402A