UiO-66 Material, Preparation Method, and Its Application in Synergistic Removal of Organic Pollutants by Thermotropic Adsorption and Photocatalysis

UiO-66 material without regulators was synthesized by solvothermal method. By utilizing the optimal adsorption temperature of its volcanic performance curve, the problem of the photocatalyst's adsorption capacity decreasing with increasing temperature was solved, and the effect of efficient thermal adsorption and photocatalytic synergistic removal of organic pollutants was achieved.

CN117186428BActive Publication Date: 2026-11-17SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311059036.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-22
Publication Date
2026-11-17
Estimated Expiration
2043-08-22

AI Technical Summary

Technical Problem

Existing photocatalysts exhibit reduced adsorption capacity at elevated temperatures, affecting catalytic efficiency and hindering the effective removal of volatile organic compounds.

Method used

UiO-66 material without regulators was synthesized by a solvothermal method. By controlling the ratio of metal source, organic ligand and solvent and stirring time, highly crystalline UiO-66 material was formed. The optimal adsorption temperature of its volcanic performance curve was used to perform synergistic removal of organic pollutants through thermal adsorption and photocatalysis.

Benefits of technology

Within the optimal adsorption temperature range, UiO-66 material can efficiently adsorb and degrade organic pollutants, improve photocatalytic efficiency, and increase adsorption capacity as temperature rises, achieving a highly efficient synergistic removal effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117186428B_ABST
    Figure CN117186428B_ABST
Patent Text Reader

Abstract

This invention discloses a solvothermal synthesis method for UiO-66 material without the use of a regulator. The method includes: dissolving a metal source and terephthalic acid in DMF and stirring for a period of time to obtain a precursor solution; placing the precursor solution in a reaction vessel and maintaining it at 120-180°C for 24-48 hours; washing and drying the reaction product to obtain the UiO-66 material. The UiO-66 material is a catalyst whose performance exhibits a volcanic-like variation trend with temperature, which is of great significance for photocatalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photocatalysis, and more particularly to a UiO-66 material, its preparation method, and its application in the synergistic removal of organic pollutants by thermal adsorption and photocatalysis. Background Technology

[0002] Today, people spend over 80% of their time indoors. The continuous release of volatile organic compounds (VOCs) from interior decoration, building materials (such as adhesives and paints), and furniture poses a significant threat to human health. VOC removal methods are mainly divided into three categories: combustion treatment of waste gas; adsorption of VOCs using adsorbents; and catalytic oxidation. Among these, photocatalytic oxidation (PCO) is considered a promising method for eliminating indoor VOCs due to its mild reaction conditions (ambient temperature and pressure), low energy consumption, and lack of equipment dependence.

[0003] Metal-organic frameworks (MOFs) are porous crystalline nanomaterials composed of inorganic units (metal ions or metal clusters) linked by polymeric organic ligands. MOFs are characterized by large specific surface area, high porosity, and easily tunable pore structure and chemical composition, and are widely used in molecular adsorption and separation, catalysis, and other fields.

[0004] Currently, to enable photocatalysts to be more widely used in daily life, researchers are working to adjust the light absorption range of catalysts and improve their catalytic efficiency under visible light. It is well known that light inevitably releases heat, thus increasing the temperature of the catalyst. The catalyst's adsorption capacity for VOCs decreases with increasing temperature. The adsorption process is a key step in gas-phase catalysis and has a significant impact on catalytic efficiency. Specifically, in photocatalytic reactions, light continuously releases heat, raising the temperature of the reaction system to its highest achievable temperature, and this temperature increase affects the reaction's progress. Current understanding is that increased temperature causes the VOCs adsorbed in the catalyst to desorb. Therefore, the heat generated by light raises the catalyst's temperature, which inevitably reduces the catalyst's adsorption and degradation performance for VOCs. Summary of the Invention

[0005] In response to the problems raised in the background art, the present invention provides a UiO-66 material and its preparation method, as well as its application in the synergistic removal of organic pollutants by thermo-induced adsorption and photocatalysis. The UiO-66 material is a catalyst whose performance and temperature exhibit a volcanic-like variation trend, which is of great significance to photocatalysis.

[0006] A volcano-shaped curve refers to a curve where the vertical axis (reaction efficiency or adsorption performance) initially increases and then decreases with increasing horizontal axis (temperature). Catalysts exhibiting this volcano-shaped performance-temperature trend have an optimal adsorption temperature (or optimal reaction temperature). The heat generated by sunlight increases the temperature of the reaction system, and this temperature range falls precisely in the first half of the volcano-shaped curve (adsorption performance increases with temperature). The highest temperature reached by the reaction system is precisely the highest point of the volcano-shaped curve (the optimal temperature for the catalyst reaction). This allows the catalyst to efficiently adsorb and degrade VOCs.

[0007] In a first aspect, the present invention provides a method for solvothermal synthesis of UiO-66 material without the use of a regulator. The method comprises: dissolving a metal source and terephthalic acid in DMF and stirring for a period of time to obtain a precursor solution; placing the precursor solution in a reaction vessel and maintaining it at 120-180°C for 24-48 hours; washing and drying the reaction product to obtain the UiO-66 material.

[0008] Preferably, the metal source is one of zirconium chloride and hafnium chloride.

[0009] Preferably, the ratio of metal source, terephthalic acid and DMF in the precursor solution is 0.1-1.0 mmol: 0.1-1.0 mmol: 50-100 mL.

[0010] Preferably, the stirring time is 1-3 hours.

[0011] Secondly, the present invention provides a UiO-66 material obtained by any of the preparation methods described above. The UiO-66 material is a polymer formed by coordination between a metal center and the organic ligand terephthalic acid.

[0012] Preferably, the metal center is zirconium or hafnium.

[0013] Preferably, the UiO-66 material is composed of stacked grains with a cubic crystal structure, and the grain size is 60-120 nm.

[0014] Thirdly, the present invention provides the application of the UiO-66 material described in any of the above claims in the synergistic removal of organic pollutants by thermal adsorption and photocatalysis.

[0015] Preferably, the organic pollutant is an organic pollutant containing a benzene ring.

[0016] Preferably, the optimal adsorption temperature of the UiO-66 material is 20-40℃, and more preferably 30℃. Attached Figure Description

[0017] Figure 1This is the XRD pattern of UiO-66(Zr) prepared in Example 1.

[0018] Figure 2 This is a SEM image of UiO-66(Zr) prepared in Example 1.

[0019] Figure 3 The temperature changes in the reaction chamber under light and heating conditions are shown in Examples 2 and 3.

[0020] Figure 4 Examples 2 and 3 show the changes in toluene concentration under light and heating conditions.

[0021] Figure 5 This is the toluene concentration change curve of UiO-66 used four times consecutively in Example 2.

[0022] Figure 6 This is the curve showing the change in toluene concentration with temperature in Example 4.

[0023] Figure 7 The adsorption amount of UiO-66(Zr) prepared in Example 1 on toluene at different temperatures was measured by adsorption isotherms.

[0024] Figure 8 This is the change in toluene concentration under heating conditions after different MOFs in Example 3 have been saturated with adsorption.

[0025] Figure 9 The images show the ESR (·OH concentration) spectra of UiO-66(Zr) before and after toluene adsorption prepared in Example 1. This indicates that UiO-66(Zr) adsorption of toluene is beneficial for the generation of free radicals, thus promoting photocatalysis.

[0026] Figure 10 These are the toluene adsorption isotherms of UiO-66(Zr) at different temperatures. This indicates that 30℃ is the optimal adsorption temperature for UiO-66(Zr). Detailed Implementation

[0027] The present invention is further illustrated by the following embodiments. It should be understood that the following embodiments are for illustrative purposes only and are not intended to limit the present invention. Unless otherwise specified, all percentage contents refer to mass percentage contents.

[0028] Existing techniques typically employ modifiers in the preparation of UiO-66 materials. However, the introduction of modifiers often introduces defects into the structure of UiO-66 materials. Therefore, this invention provides a method for the solvothermal synthesis of UiO-66 materials without the use of modifiers.

[0029] A precursor solution is obtained by dissolving a metal salt and terephthalic acid (BDC) in DMF and stirring for a period of time. The metal source includes, but is not limited to, zirconium chloride and hafnium chloride. Taking zirconium chloride as an example, in DMF, zirconium chloride first forms a zirconium-oxygen cluster, and then coordinates with BDC to form the three-dimensional framework structure of UiO-66 material.

[0030] The ratio of metal source, terephthalic acid, and DMF in the precursor solution is 0.1-1.0 mmol: 0.1-1.0 mmol: 50-100 mL. Lower metal source concentrations result in easier acquisition of highly crystalline UiO-66 material, but also affect the yield. By controlling the metal source concentration at the aforementioned level, both highly crystalline UiO-66 material and a suitable product quantity can be obtained.

[0031] The stirring time is 1-3 hours. By appropriately extending the stirring time, it is beneficial for the metal source and the organic ligand BDC to have more complete contact coordination, which promotes better synthesis of UiO-66 material in the subsequent solvothermal reaction.

[0032] The precursor solution was placed in a reaction vessel and kept at 120-180℃ for 24-48 hours. Shortening the reaction time, for example, controlling the synthesis time to 18 hours, resulted in a wider XRD diffraction peak and poorer crystallinity of the obtained UiO-66 material.

[0033] A high-pressure reactor is preferred. A high-pressure reactor provides a better nucleation environment for crystallization. Under suitable high-pressure conditions, the coordination and binding of ligands with the metal matrix are facilitated, resulting in a higher degree of crystallinity and greater stability of the prepared UiO-66 material compared to that synthesized under normal pressure. In a specific embodiment, the reactor is a reactor with a stainless steel outer liner and a polytetrafluoroethylene inner liner. The working pressure of the reactor does not exceed 3 MPa, and the volume does not exceed 80%.

[0034] In some technical solutions, the volume of DMF occupies 50% of the reactor volume. This is beneficial for controlling the reaction pressure.

[0035] The reaction product was washed and dried to obtain the UiO-66 material. Drying removes residual DMF from the product. The drying temperature and time can be selected according to actual needs. For example, vacuum drying at 100°C for 12 hours.

[0036] Taking the synthesis of UiO-66(Zr) material as an example: ZrCl4 (1.0 mmol) and H2BDC (1.0 mmol) were dissolved in DMF (50 mL) and stirred for 2 hours to obtain a precursor solution. The precursor solution was then placed in a reaction vessel and kept at 120 °C for 24 hours. The precipitate was washed with DMF and ethanol respectively, and dried under vacuum at 80 °C for 8 hours to obtain the UiO-66(Zr) material.

[0037] The morphology of UiO-66 materials can be controlled using modifiers such as acetic acid. For example, adding a modifier can promote crystal nucleus growth, resulting in larger crystal sizes of the obtained UiO-66 material, yielding complete octahedrons (leaning towards hexahedrons). However, because the crystal size increases, the specific surface area of ​​the UiO-66 material increases, leading to more defects. This invention proposes a solvothermal method for synthesizing UiO-66 material without using a modifier. Without introducing a modifier, the crystal nucleation process is more pronounced, meaning that many UiO-66 particles with smaller crystal sizes will be formed. This invention can prepare well-crystallized UiO-66 material without the need for additional modifiers such as carboxylic acids to control the morphology.

[0038] The present invention also provides a UiO-66 material obtained by the above preparation method, wherein the UiO-66 material is a polymer formed by coordination between a metal center and an organic ligand terephthalic acid. For example, the UiO-66(Zr) synthesized in the examples is a polymer formed by coordination between a metal center Zr and an organic ligand terephthalic acid (BDC).

[0039] In some technical solutions, the metal center is Zr or Hf. The metal center, acting as a Lewis acidic site, can better adsorb catalytic Lewis basic gases (such as toluene). Furthermore, the ligand terephthalic acid of UiO-66 can better adsorb toluene through π-π interactions of the benzene ring.

[0040] The UiO-66 material is composed of stacked grains with a cubic crystal structure, and the grain size is 60-120 nm. The UiO-66 material has a large specific surface area, well-developed channels, and an adjustable pore size structure. In some technical solutions, UiO-66 is a microporous material with a pore size of less than 2 nm.

[0041] This invention also proposes the application of the UiO-66 material described in any of the above claims in the synergistic removal of organic pollutants by thermotropic adsorption and photocatalysis. In particular, the organic pollutants are benzene-ring-containing organic pollutants. The interaction between the benzene-ring-containing ligands and benzene-ring-containing VOCs in the UiO-66 material is the cause of the thermotropic adsorption phenomenon; that is, thermotropic adsorption occurs when both contain benzene rings.

[0042] In summary, the UiO-66 material prepared by this invention exhibits thermo-induced adsorption, with 30°C being the optimal adsorption temperature within the range of 20-40°C. Maintaining the catalyst at approximately 30°C ensures continuous and efficient adsorption and degradation of toluene. Furthermore, photocatalytic reactions are conducted at room temperature (20-25°C), where light exposure increases the catalyst temperature, leading to increased toluene adsorption and improved photocatalytic efficiency.

[0043] The UiO-66 material described in this invention exhibits thermo-induced adsorption, meaning that illumination can raise the catalyst's temperature, thereby further enhancing its photocatalytic efficiency. The UiO-66 of this invention exhibits an optimal temperature for toluene adsorption, which happens to be the highest temperature achievable under experimental illumination. Furthermore, below 30°C, the adsorption capacity of UiO-66 for toluene increases with increasing temperature, demonstrating practicality. Photocatalysis raises the reaction system temperature, which is precisely what favors increasing the amount of toluene adsorbed by UiO-66, thus contributing to the photocatalytic reaction.

[0044] Furthermore, the adsorption performance, or reaction efficiency, is negatively correlated with temperature. Experiments showed that the current light conditions allowed the reaction system to reach a maximum temperature of around 30°C, which is precisely the optimal temperature for UiO-66 to adsorb toluene. The adsorption capacity and temperature of UiO-66 also closely match the volcano-shaped adsorption curve.

[0045] The following examples further illustrate the present invention in detail. It should also be understood that the following examples are only for further explanation of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention are within the scope of protection of the present invention. The specific process parameters, etc., in the following examples are merely examples within a suitable range; that is, those skilled in the art can make appropriate selections within the appropriate range based on the description herein, and are not intended to be limited to the specific values ​​in the examples below.

[0046] Example 1

[0047] ZrCl4 (1.0 mmol) and terephthalic acid (1.0 mmol) were dissolved in N,N-dimethylformamide (50 mL), sonicated until dissolved, and stirred for 2 hours (600 r / min). The solution was then placed in a 100 mL high-pressure reactor and placed in an oven, with the reaction temperature and time controlled at 125 °C and 24 h, respectively. After the reaction was completed and the reaction solution was cooled to room temperature, the reaction product was separated from the reaction solution by centrifugation and washing with DMF and ethanol several times, respectively. After vacuum drying in an oven (80 °C for 8 hours), it was ground to obtain UiO-66(Zr).

[0048] Figure 1This is the XRD pattern of UiO-66(Zr) prepared in this embodiment. As shown in the figure, the UiO-66(Zr) prepared in this embodiment exhibits obvious characteristic peaks between 5-50°, which corresponds to UiO-66.

[0049] Figure 2 This is a SEM image of the UiO-66(Zr) prepared in this embodiment. It can be seen that the prepared UiO-66 exhibits a cubic structure.

[0050] Example 2

[0051] 30 mg of UiO-66 (Zr) prepared in Example 1 above was weighed and dispersed in 5 mL of ethanol. After ball milling for 8 hours, the mixture was coated onto a 15 cm × 7 cm glass plate and dried to obtain a UiO-66 coating. The obtained UiO-66 coating was placed in a reaction chamber, where a thermometer was used to record the real-time temperature. Adsorption was carried out in the dark at room temperature (22 °C). After adsorption saturation, the light source (250 W xenon lamp + 400 nm filter) was turned on, with the light source 30 cm away from the catalyst, to measure the changes in reaction chamber temperature and toluene concentration under illumination.

[0052] Example 3

[0053] 30 mg of UiO-66 prepared in Example 1 was weighed and dispersed in 5 mL of ethanol. After ball milling for 8 hours, the mixture was coated onto a 15 cm × 7 cm glass plate and dried to obtain a UiO-66 coating. The obtained UiO-66 coating was placed in a reaction chamber, where a thermometer recorded the real-time temperature. Adsorption was carried out in a dark environment at room temperature (20 °C). After adsorption saturation, the heating stage under the reaction chamber was turned on to simulate the temperature of the reaction chamber under light, in order to measure the changes in reaction chamber temperature and toluene concentration under heating conditions.

[0054] Figure 3 This represents the temperature changes in the reaction chamber under both illumination and heating conditions. It can be seen that the temperature change trend under heating conditions is close to that under actual illumination, and the temperature values ​​are similar, indicating that heating conditions can effectively simulate real-time temperature changes under illumination conditions.

[0055] Figure 4 The data represents the change in toluene concentration under light and heating conditions. It can be seen that under light conditions, the toluene removal efficiency of UiO-66 is 90%. However, UiO-66 itself has very weak light absorption under visible light, which leads to its generally low adsorption performance. The inventors speculate that temperature also has a certain impact on the toluene removal efficiency of UiO-66.

[0056] Remove the light source and use a heating platform to simulate the real-time temperature changes of the reaction chamber under light. Figure 3The results showed that the temperature changes in the reaction chamber were similar under both heating and light irradiation conditions. The results also revealed that the toluene removal efficiency of UiO-66 was 70% under heating conditions, indicating that the 90% toluene removal efficiency under light irradiation was due to both the temperature effect (70%) and the photocatalytic reaction (20%). This invention is the first to discover that temperature causes a decrease in the toluene concentration of UiO-66, a very rare phenomenon and the focus of this research. Increasing the temperature causes UiO-66 to adsorb more toluene, leading to a decrease in the toluene concentration. In other words, temperature affects the ability of UiO-66 to adsorb toluene.

[0057] Figure 5 The figures show the toluene concentration change curves after four consecutive uses of UiO-66 under the conditions of Example 2. After discovering the excellent toluene removal efficiency of UiO-66 under light irradiation, the experiment was repeated four times under the light irradiation conditions of Example 2, demonstrating the repeatability and stability of the synergistic removal of toluene by UiO-66 through thermal adsorption and photocatalysis.

[0058] Example 4

[0059] Weigh 30 mg of UiO-66 prepared in Example 1 above, disperse it in 5 mL of ethanol, ball mill it for 8 hours, coat it onto a 15 cm × 7 cm glass plate, and dry it to obtain a UiO-66 coating. Place the obtained UiO-66 coating in a reaction chamber, where a thermometer records the real-time temperature. Adsorption is carried out in a dark environment at room temperature of 20°C. After adsorption saturation, turn on the heating platform under the reaction chamber, and when the temperature rises to about 29°C, circulate water to cool the reaction chamber.

[0060] Figure 6 This is the curve showing the change in toluene concentration with temperature in Example 4. From the aforementioned... Figure 4 It can be seen that increasing the temperature decreases the toluene concentration, indicating that UiO-66 increases the adsorption capacity of toluene. And from... Figure 6 Further observation shows that increasing the temperature decreases the toluene concentration, while decreasing the temperature increases it, indicating a reduction in the toluene adsorption capacity of UiO-66. This demonstrates that the toluene adsorption capacity of UiO-66 is affected by temperature and is related to temperature changes. Furthermore, a simple cooling process can desorb toluene from UiO-66 (a C / C0 greater than 1 indicates that toluene has desorbed, resulting in a toluene concentration in the reaction chamber higher than the equilibrium value C0).

[0061] Figure 7 This represents the adsorption capacity of UiO-66(Zr) for toluene at different temperatures. Specifically, it's the adsorption capacity calculated based on adsorption isotherms at different temperatures. It can be seen that 30℃ is the optimal adsorption temperature for UiO-66(Zr), and this has been proven. Figure 6 The authenticity.

[0062] Example 5

[0063] Hafnium chloride was substituted for zirconium chloride, and UiO-66(Hf) was prepared using the same steps. 30 mg of UiO-66(Hf) was weighed and dispersed in 5 mL of ethanol. After ball milling for 8 hours, the mixture was coated onto a 15 cm × 7 cm glass plate and dried to obtain a UiO-66 coating. The obtained UiO-66 coating was placed in a reaction chamber, where a thermometer recorded the real-time temperature. Adsorption was performed in the dark at room temperature (20 °C). After adsorption saturation, the heating platform under the reaction chamber was turned on to simulate the temperature under light.

[0064] Comparative Example 1

[0065] MOF-801 was prepared using the same procedure, replacing terephthalic acid with fumaric acid. 30 mg of MOF-801 was weighed and dispersed in 5 mL of ethanol. After ball milling for 8 hours, the dispersed material was coated onto a 15 cm × 7 cm glass plate and dried to obtain a UiO-66 coating. The obtained UiO-66 coating was placed in a reaction chamber, where a thermometer recorded the real-time temperature. Adsorption was performed in the dark at room temperature (20°C). After adsorption saturation, the heating stage under the reaction chamber was turned on to simulate the temperature under light.

[0066] Figure 8 This section describes the change in toluene concentration under heating conditions after different MOFs have reached adsorption saturation. After different MOFs reached adsorption saturation, heating was performed, and it was found that the toluene concentration decreased in Uio-66(Zr) and Uio-66(Hf) under heating conditions, indicating that they exhibit thermo-induced adsorption. However, MOF-801 (with Zr as the metal center and fumaric acid as the organic ligand, which does not contain a benzene ring) did not exhibit thermo-induced adsorption; instead, toluene continuously desorbed from MOF-801 upon heating (a common phenomenon consistent with the previously mentioned decrease in adsorption capacity of common catalysts upon increasing temperature). This suggests that thermo-induced adsorption is related to the organic ligands of the MOF. The ligands for Uio-66(Zr) and Uio-66(Hf) are both terephthalic acid, containing a benzene ring structure, and are unrelated to the metal center.

Claims

1. Application of UiO-66 material for synergistic removal of volatile organic pollutants toluene by using heat-induced adsorption and photocatalysis, characterized in that, The photocatalytic reaction was carried out at room temperature (20-25℃). Irradiation increased the temperature of the UiO-66 catalyst, leading to increased toluene adsorption and improved photocatalytic efficiency. By maintaining the UiO-66 catalyst at 30℃, it continuously and efficiently adsorbed and degraded toluene. The UiO-66 material is a polymer formed by coordination between a metal center and the organic ligand terephthalic acid. The UiO-66 material was synthesized via a solvothermal method without the use of a regulator. The synthesis method included the following steps: dissolving a metal source and terephthalic acid in DMF and stirring for a period of time to obtain a precursor solution; placing the precursor solution in a reaction vessel and maintaining it at 120-180℃ for 24-48 hours. The reaction product was washed and dried to obtain the UiO-66 material; the ratio of metal source, terephthalic acid and DMF in the precursor solution was 0.1-1.0 mmol: 0.1-1.0 mmol: 50-100 mL.

2. Use according to claim 1, characterized in that, The UiO-66 material is a cubic crystal structure with a grain size of 60-120 nm.

3. Use according to claim 1, characterized in that, The metal source is either zirconium chloride or hafnium chloride.

4. Use according to claim 1, characterized in that, The stirring time is 1-3 hours.

Citation Information

Patent Citations

  • Metal-organic framework UiO-66 adsorbent and modified material thereof

    CN108671892A

  • A method for preparing high-yield UiO-66 metal-organic framework materials and their applications

    CN114933709A