Acid and alkali resistant polyimide film for new energy batteries and its preparation process

Through acid and alkali treatment and vacuum impregnation process of modified graphene and silicon carbide, a polyimide film with excellent acid and alkali resistance is prepared, which solves the problem of insufficient acid and alkali resistance of the film in the existing technology and significantly improves the Electrochemical performance and life of new energy batteries.

CN117210004BActive Publication Date: 2024-10-25SUZHOU GOLDEN KEY AUTOMATION EQUIP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311327679.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-13
Publication Date
2024-10-25
Estimated Expiration
2043-10-13

AI Technical Summary

Technical Problem

The polyimide film prepared by the existing technology has poor acid and alkali resistance in new energy batteries, which affects the battery life and performance.

Method used

Modified graphene and silicon carbide are used to prepare acid and alkali-resistant polyimide films for new energy batteries through specific acid-base treatment and vacuum impregnation processes, adding diamine monomers, dianhydride monomers and methyltriethoxy groups Silane, forming a thin film with excellent acid and alkali resistance.

Benefits of technology

Significantly improve the acid and alkali resistance and dielectric constant of the polyimide film, enhance the electrochemical performance of new energy batteries, extend battery life and improve reprocessing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117210004B_ABST
    Figure CN117210004B_ABST
Patent Text Reader

Abstract

The invention discloses an acid- and alkali-resistant polyimide film for new energy batteries and a preparation process thereof, and relates to the technical field of lithium batteries. The film is made of the following ingredients: graphene, silicon carbide, sodium stearate, diamine monomer, dianhydride monomer, and methyltriethoxysilane. The polyimide film prepared by the invention has excellent acid and alkali resistance and also has a suitable dielectric constant, and can be better applied to new energy batteries, thereby improving the electrochemical performance of new energy batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of new energy batteries, in particular to an acid- and alkali-resistant polyimide film for new energy batteries and a preparation process thereof. Background Art

[0002] Polyimide materials have excellent heat resistance, good mechanical properties, and outstanding dielectric properties. Therefore, they can be widely used in aerospace, precision instruments, electronic packaging, new energy batteries and other fields. In the production process of new energy batteries, polyimide films are needed. However, the acid and alkali resistance of polyimide films prepared by existing technologies is relatively general, which greatly affects the lifespan of the films when working in new energy batteries, and thus directly affects the working performance of new energy batteries.

[0003] Therefore, the prior art needs to be further improved. Summary of the invention

[0004] The purpose of the present invention is to provide an acid- and alkali-resistant polyimide film for new energy batteries to solve the deficiencies in the prior art.

[0005] The technical solution adopted by the present invention is as follows:

[0006] The acid-base resistant polyimide film for new energy batteries is made of the following ingredients by weight: 3-5 parts of graphene, 3-5 parts of silicon carbide, 1.2-1.6 parts of sodium stearate, 10-20 parts of diamine monomer, 9.5-19 parts of dianhydride monomer, and 2-3 parts of methyltriethoxysilane;

[0007] Among them, graphene and silicon carbide have been modified.

[0008] As a further technical solution: the graphene and silicon carbide modification treatment method includes:

[0009] (1) First, nitric acid and sulfuric acid are added to deionized water respectively, and stirred to mix evenly to prepare a mixed acid solution;

[0010] (2) adding sodium hydroxide to deionized water, stirring and mixing to prepare a sodium hydroxide solution;

[0011] (3) adding graphene and silicon carbide to a sodium hydroxide solution, stirring and treating for 40 minutes in a 90° C. water bath, then filtering, washing to neutrality, and drying to obtain a pretreated mixture;

[0012] (4) adding the pretreated mixed material and the mixed acid solution obtained in the above step (3) into a vacuum impregnation reactor in sequence;

[0013] (5) adjusting the temperature in the vacuum impregnation reactor to 56° C., stirring for 30 min, then adjusting the temperature to 76° C., stirring for 30 min, and finally adjusting the temperature to 90° C., stirring for 2 hours, and standing for 30 min;

[0014] (6) Discharge the vacuum impregnation reactor in step (5), filter, wash with deionized water until neutral, and dry in vacuum.

[0015] As a further technical solution: the mass fraction of nitric acid in the mixed acid solution in step (1) is 5-5.5%;

[0016] The mass fraction of the sulfuric acid is 2.5%.

[0017] As a further technical solution: the mass fraction of the sodium hydroxide solution in step (2) is 10%.

[0018] As a further technical solution: in step (3), the mixing ratio of graphene and sodium hydroxide solution is 12g:90mL.

[0019] As a further technical solution: the mixing ratio of the pretreated mixture and the mixed acid solution in step (4) is 10g:120-130mL.

[0020] As a further technical solution: the vacuum degree in the vacuum impregnation reactor in step (5) is 3-5Pa.

[0021] As a further technical solution: the vacuum drying temperature in step (6) is 55°C;

[0022] The vacuum drying time was 2 hours.

[0023] As a further technical solution: the diamine monomer is: 4,4'-diaminodiphenyl ether and 4,4'-diaminodiphenyl sulfide are mixed in a mass ratio of 2:1;

[0024] The dianhydride monomer is prepared by mixing 3,3',4,4'-benzophenone tetracarboxylic dianhydride and 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride in a mass ratio of 1:1.

[0025] The preparation process of acid-alkali resistant polyimide film for new energy batteries includes the following steps:

[0026] (1) Weighing the following materials in parts by weight: graphene, silicon carbide, sodium stearate, diamine monomer, dianhydride monomer, and methyltriethoxysilane;

[0027] (2) adding the modified graphene and silicon carbide to N,N-dimethylacetamide, stirring for 10 minutes, and then ultrasonically treating for 5 minutes to obtain a dispersion;

[0028] (3) Sodium stearate and diamine monomer are added to the dispersion in sequence, and reflux reaction is carried out for 20 hours. Then, dianhydride monomer and methyltriethoxysilane are added respectively, and stirring reaction is continued for 10 hours. Then, coating is carried out to form a film, and then a thermal imidization reaction is carried out to form a finished product, which is then cut.

[0029] Beneficial effects:

[0030] The polyimide film prepared by the present invention has excellent acid resistance and alkali resistance, and also has a suitable dielectric constant, and can be better applied to new energy batteries, thereby improving the electrochemical performance of new energy batteries.

[0031] In the preparation process of polyimide film, the performance of polyimide film can be greatly improved by modifying graphene and silicon carbide, especially the acid and alkali resistance can be significantly improved. In addition, in the film formation process, the different internal structures can promote the interaction between polyamic acid molecules. At the same time, the solvent can promote the polyamic acid molecules to aggregate more closely, thereby greatly reducing the distance between polyamic acid molecules, which in turn leads to the film being able to effectively resist the penetration of acidic and alkaline solutions.

[0032] By introducing the joint action of multiple components, the effect of asymmetric structure can be introduced into the main chain of polyimide, which is manifested as: reducing the chain spacing of polyimide, reducing the main chain stacking, improving the acid and alkali resistance of polyimide film, improving the flexibility of polyimide film, significantly improving the mechanical properties, inhibiting the charge transfer effect, and greatly improving the reprocessing performance of polyimide film. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a histogram of dielectric constants of the embodiments. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0035] The following are specific embodiments:

[0036] Example 1

[0037] The acid-base resistant polyimide film for new energy batteries is made of the following ingredients by weight: 3 parts of graphene, 3 parts of silicon carbide, 1.2 parts of sodium stearate, 10 parts of diamine monomer, 9.5 parts of dianhydride monomer, and 2 parts of methyltriethoxysilane;

[0038] Among them, graphene and silicon carbide have been modified.

[0039] The modification methods of graphene and silicon carbide include:

[0040] (1) First, nitric acid and sulfuric acid are added to deionized water respectively, and stirred to mix evenly to prepare a mixed acid solution; the mass fraction of nitric acid in the mixed acid solution is 5%;

[0041] The mass fraction of the sulfuric acid is 2.5%.

[0042] (2) Add sodium hydroxide to deionized water, stir and mix well to prepare a sodium hydroxide solution; the mass fraction of the sodium hydroxide solution is 10%.

[0043] (3) Adding graphene and silicon carbide to a sodium hydroxide solution, stirring for 40 minutes in a 90° C. water bath, then filtering, washing to neutrality, and drying to obtain a pretreated mixture; the mixing ratio of graphene to sodium hydroxide solution is 12 g:90 mL.

[0044] (4) The pretreated mixture and the mixed acid solution obtained in the above step (3) are added into the vacuum impregnation reactor in sequence; the mixing ratio of the pretreated mixture and the mixed acid solution is 10 g:120 mL.

[0045] (5) The temperature in the vacuum impregnation reactor was adjusted to 56° C., stirred for 30 min, then adjusted to 76° C., stirred for 30 min, and finally adjusted to 90° C., stirred for 2 hours, and allowed to stand for 30 min; the vacuum degree in the vacuum impregnation reactor was 3 Pa.

[0046] (6) Discharge the vacuum impregnation reactor in step (5), filter, wash with deionized water until neutral, and vacuum dry; the vacuum drying temperature is 55° C.;

[0047] The vacuum drying time was 2 hours.

[0048] The diamine monomer is a mixture of 4,4'-diaminodiphenyl ether and 4,4'-diaminodiphenyl sulfide in a mass ratio of 2:1;

[0049] The dianhydride monomer is prepared by mixing 3,3',4,4'-benzophenone tetracarboxylic dianhydride and 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride in a mass ratio of 1:1.

[0050] The preparation process of acid-alkali resistant polyimide film for new energy batteries includes the following steps:

[0051] (1) Weighing the following materials in parts by weight: graphene, silicon carbide, sodium stearate, diamine monomer, dianhydride monomer, and methyltriethoxysilane;

[0052] (2) adding the modified graphene and silicon carbide to N,N-dimethylacetamide, stirring for 10 minutes, and then ultrasonically treating for 5 minutes to obtain a dispersion;

[0053] (3) Sodium stearate and diamine monomer are added to the dispersion in sequence, and reflux reaction is carried out for 20 hours. Then, dianhydride monomer and methyltriethoxysilane are added respectively, and stirring reaction is continued for 10 hours. Then, coating is carried out to form a film, and then a thermal imidization reaction is carried out to form a finished product, which is then cut.

[0054] Example 2

[0055] The acid- and alkali-resistant polyimide film for new energy batteries is made of the following ingredients by weight: 3.5 parts of graphene, 3.5 parts of silicon carbide, 1.4 parts of sodium stearate, 12 parts of diamine monomer, 11.4 parts of dianhydride monomer, and 2.5 parts of methyltriethoxysilane;

[0056] Among them, graphene and silicon carbide have been modified.

[0057] The modification methods of graphene and silicon carbide include:

[0058] (1) First, nitric acid and sulfuric acid are added to deionized water respectively, and stirred to mix evenly to prepare a mixed acid solution; the mass fraction of nitric acid in the mixed acid solution is 5.2%;

[0059] The mass fraction of the sulfuric acid is 2.5%.

[0060] (2) Add sodium hydroxide to deionized water, stir and mix well to prepare a sodium hydroxide solution; the mass fraction of the sodium hydroxide solution is 10%.

[0061] (3) Adding graphene and silicon carbide to a sodium hydroxide solution, stirring for 40 minutes in a 90° C. water bath, then filtering, washing to neutrality, and drying to obtain a pretreated mixture; the mixing ratio of graphene to sodium hydroxide solution is 12 g:90 mL.

[0062] (4) The pretreated mixture and the mixed acid solution obtained in the above step (3) are added into the vacuum impregnation reactor in sequence; the mixing ratio of the pretreated mixture and the mixed acid solution is 10 g:125 mL.

[0063] (5) The temperature in the vacuum impregnation reactor was adjusted to 56° C., stirred for 30 min, then adjusted to 76° C., stirred for 30 min, and finally adjusted to 90° C., stirred for 2 hours, and allowed to stand for 30 min; the vacuum degree in the vacuum impregnation reactor was 3.5 Pa.

[0064] (6) Discharge the vacuum impregnation reactor in step (5), filter, wash with deionized water until neutral, and vacuum dry; the vacuum drying temperature is 55° C.;

[0065] The vacuum drying time was 2 hours.

[0066] The diamine monomer is a mixture of 4,4'-diaminodiphenyl ether and 4,4'-diaminodiphenyl sulfide in a mass ratio of 2:1;

[0067] The dianhydride monomer is prepared by mixing 3,3',4,4'-benzophenone tetracarboxylic dianhydride and 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride in a mass ratio of 1:1.

[0068] The preparation process of acid-alkali resistant polyimide film for new energy batteries includes the following steps:

[0069] (1) Weighing the following materials in parts by weight: graphene, silicon carbide, sodium stearate, diamine monomer, dianhydride monomer, and methyltriethoxysilane;

[0070] (2) adding the modified graphene and silicon carbide to N,N-dimethylacetamide, stirring for 10 minutes, and then ultrasonically treating for 5 minutes to obtain a dispersion;

[0071] (3) Sodium stearate and diamine monomer are added to the dispersion in sequence, and reflux reaction is carried out for 20 hours. Then, dianhydride monomer and methyltriethoxysilane are added respectively, and stirring reaction is continued for 10 hours. Then, coating is carried out to form a film, and then a thermal imidization reaction is carried out to form a finished product, which is then cut.

[0072] Example 3

[0073] The acid-base resistant polyimide film for new energy batteries is made of the following ingredients by weight: 4 parts of graphene, 4 parts of silicon carbide, 1.5 parts of sodium stearate, 15 parts of diamine monomer, 14.25 parts of dianhydride monomer, and 2.8 parts of methyltriethoxysilane;

[0074] Among them, graphene and silicon carbide have been modified.

[0075] The modification methods of graphene and silicon carbide include:

[0076] (1) First, nitric acid and sulfuric acid are added to deionized water respectively, and stirred to mix evenly to prepare a mixed acid solution; the mass fraction of nitric acid in the mixed acid solution is 5.3%;

[0077] The mass fraction of the sulfuric acid is 2.5%.

[0078] (2) Add sodium hydroxide to deionized water, stir and mix well to prepare a sodium hydroxide solution; the mass fraction of the sodium hydroxide solution is 10%.

[0079] (3) Adding graphene and silicon carbide to a sodium hydroxide solution, stirring for 40 minutes in a 90° C. water bath, then filtering, washing to neutrality, and drying to obtain a pretreated mixture; the mixing ratio of graphene to sodium hydroxide solution is 12 g:90 mL.

[0080] (4) The pretreated mixture and the mixed acid solution obtained in the above step (3) are added into the vacuum impregnation reactor in sequence; the mixing ratio of the pretreated mixture and the mixed acid solution is 10 g:125 mL.

[0081] (5) The temperature in the vacuum impregnation reactor was adjusted to 56° C., stirred for 30 min, then adjusted to 76° C., stirred for 30 min, and finally adjusted to 90° C., stirred for 2 hours, and allowed to stand for 30 min; the vacuum degree in the vacuum impregnation reactor was 4 Pa.

[0082] (6) Discharge the vacuum impregnation reactor in step (5), filter, wash with deionized water until neutral, and vacuum dry; the vacuum drying temperature is 55° C.;

[0083] The vacuum drying time was 2 hours.

[0084] The diamine monomer is a mixture of 4,4'-diaminodiphenyl ether and 4,4'-diaminodiphenyl sulfide in a mass ratio of 2:1;

[0085] The dianhydride monomer is prepared by mixing 3,3',4,4'-benzophenone tetracarboxylic dianhydride and 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride in a mass ratio of 1:1.

[0086] The preparation process of acid-alkali resistant polyimide film for new energy batteries includes the following steps:

[0087] (1) Weighing the following materials in parts by weight: graphene, silicon carbide, sodium stearate, diamine monomer, dianhydride monomer, and methyltriethoxysilane;

[0088] (2) adding the modified graphene and silicon carbide to N,N-dimethylacetamide, stirring for 10 minutes, and then ultrasonically treating for 5 minutes to obtain a dispersion;

[0089] (3) Sodium stearate and diamine monomer are added to the dispersion in sequence, and reflux reaction is carried out for 20 hours. Then, dianhydride monomer and methyltriethoxysilane are added respectively, and stirring reaction is continued for 10 hours. Then, coating is carried out to form a film, and then a thermal imidization reaction is carried out to form a finished product, which is then cut.

[0090] Example 4

[0091] The acid- and alkali-resistant polyimide film for new energy batteries is made of the following ingredients by weight: 5 parts of graphene, 5 parts of silicon carbide, 1.6 parts of sodium stearate, 20 parts of diamine monomer, 19 parts of dianhydride monomer, and 3 parts of methyltriethoxysilane;

[0092] Among them, graphene and silicon carbide have been modified.

[0093] The modification methods of graphene and silicon carbide include:

[0094] (1) First, nitric acid and sulfuric acid are added to deionized water respectively, and stirred to mix evenly to prepare a mixed acid solution; the mass fraction of nitric acid in the mixed acid solution is 5.5%;

[0095] The mass fraction of the sulfuric acid is 2.5%.

[0096] (2) Add sodium hydroxide to deionized water, stir and mix well to prepare a sodium hydroxide solution; the mass fraction of the sodium hydroxide solution is 10%.

[0097] (3) Adding graphene and silicon carbide to a sodium hydroxide solution, stirring for 40 minutes in a 90° C. water bath, then filtering, washing to neutrality, and drying to obtain a pretreated mixture; the mixing ratio of graphene to sodium hydroxide solution is 12 g:90 mL.

[0098] (4) The pretreated mixture and the mixed acid solution obtained in the above step (3) are added into the vacuum impregnation reactor in sequence; the mixing ratio of the pretreated mixture and the mixed acid solution is 10 g:130 mL.

[0099] (5) The temperature in the vacuum impregnation reactor was adjusted to 56° C., stirred for 30 min, then adjusted to 76° C., stirred for 30 min, and finally adjusted to 90° C., stirred for 2 hours, and allowed to stand for 30 min; the vacuum degree in the vacuum impregnation reactor was 5 Pa.

[0100] (6) Discharge the vacuum impregnation reactor in step (5), filter, wash with deionized water until neutral, and vacuum dry; the vacuum drying temperature is 55° C.;

[0101] The vacuum drying time was 2 hours.

[0102] The diamine monomer is a mixture of 4,4'-diaminodiphenyl ether and 4,4'-diaminodiphenyl sulfide in a mass ratio of 2:1;

[0103] The dianhydride monomer is prepared by mixing 3,3',4,4'-benzophenone tetracarboxylic dianhydride and 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride in a mass ratio of 1:1.

[0104] The preparation process of acid-alkali resistant polyimide film for new energy batteries includes the following steps:

[0105] (1) Weighing the following materials in parts by weight: graphene, silicon carbide, sodium stearate, diamine monomer, dianhydride monomer, and methyltriethoxysilane;

[0106] (2) adding the modified graphene and silicon carbide to N,N-dimethylacetamide, stirring for 10 minutes, and then ultrasonically treating for 5 minutes to obtain a dispersion;

[0107] (3) Sodium stearate and diamine monomer are added to the dispersion in sequence, and reflux reaction is carried out for 20 hours. Then, dianhydride monomer and methyltriethoxysilane are added respectively, and stirring reaction is continued for 10 hours. Then, coating is carried out to form a film, and then a thermal imidization reaction is carried out to form a finished product, which is then cut.

[0108] Comparative Example 1:

[0109] Based on Example 1, graphene is not added and the rest of the technical solutions remain unchanged.

[0110] Comparative Example 2:

[0111] Based on Example 1, silicon carbide is not added and the rest of the technical solutions remain unchanged.

[0112] Comparative Example 3:

[0113] Based on Example 1, graphene and silicon carbide are not modified, and the rest of the technical solutions remain unchanged.

[0114] test

[0115] This paper uses a precision impedance analyzer to test the dielectric spectrum of the embodiment and comparative film:

[0116] Table 1

[0117] Dielectric constant Example 1 2.51 Example 2 2.63 Example 3 2.58 Example 4 2.50

[0118] It can be seen from Table 1 that the acid- and alkali-resistant polyimide film for new energy batteries prepared in the present invention has a more suitable dielectric constant.

[0119] The samples of the embodiment were tested according to the national standard GB / T1040.3-2006 "Determination of tensile properties of plastics":

[0120] Table 2

[0121] Tensile strength MPa Example 1 165 Example 2 169 Example 3 166 Example 4 161 Comparative Example 1 132 Comparative Example 2 127 Comparative Example 3 105

[0122] It can be seen from Table 2 that the acid- and alkali-resistant polyimide film for new energy batteries prepared in the present invention has excellent mechanical properties.

[0123] Acid resistance test:

[0124] The samples of the embodiment and the comparative example were added to a sulfuric acid solution with a mass fraction of 10% respectively, and soaked for 120 hours at room temperature. Then, they were taken out, cleaned and dried, and the mass before and after were compared to calculate the mass loss rate:

[0125] Table 3

[0126] Acid resistance mass loss rate % Example 1 0.055 Example 2 0.046 Example 3 0.042 Example 4 0.053 Comparative Example 1 0.128 Comparative Example 2 0.164 Comparative Example 3 0.355

[0127] It can be seen from Table 3 that the acid- and alkali-resistant polyimide film for new energy batteries prepared in the present invention has excellent acid resistance.

[0128] Alkali resistance test:

[0129] The samples of the embodiment and the comparative example were added to a sodium hydroxide solution with a mass fraction of 10% respectively, and soaked for 120 hours at room temperature. Then, they were taken out, cleaned and dried, and the mass before and after were compared to calculate the mass loss rate:

[0130] Table 4

[0131]

[0132]

[0133] It can be seen from Table 4 that the acid- and alkali-resistant polyimide film for new energy batteries prepared in the present invention has excellent alkali resistance.

[0134] Figure 1 2 is a histogram of dielectric constants of the embodiment.

[0135] The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.

Claims

1. Acid and alkali resistant polyimide film for new energy batteries, characterized by: It is made of the following ingredients by weight: 3-5 parts of graphene, 3-5 parts of silicon carbide, 1.2-1.6 parts of sodium stearate, 10-20 parts of diamine monomer, 9.5-19 parts of dianhydride monomer, and 2-3 parts of methyltriethoxysilane; The diamine monomer is a mixture of 4,4'-diaminodiphenyl ether and 4,4'-diaminodiphenyl sulfide in a mass ratio of 2:1; The dianhydride monomer is a mixture of 3,3',4,4'-benzophenone tetracarboxylic dianhydride and 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride in a mass ratio of 1:1; Among them, graphene and silicon carbide have been modified; The graphene and silicon carbide modification treatment method comprises: (1) First, nitric acid and sulfuric acid are added to deionized water respectively, and stirred to mix evenly to prepare a mixed acid solution; (2) adding sodium hydroxide to deionized water, stirring and mixing to prepare a sodium hydroxide solution; (3) adding graphene and silicon carbide to a sodium hydroxide solution, stirring and treating for 40 minutes in a 90° C. water bath, then filtering, washing to neutrality, and drying to obtain a pretreated mixture; (4) adding the pretreated mixed material and the mixed acid solution obtained in the above step (3) into the vacuum impregnation reactor in sequence; (5) adjusting the temperature in the vacuum impregnation reactor to 56° C., stirring for 30 min, then adjusting the temperature to 76° C., stirring for 30 min, and finally adjusting the temperature to 90° C., stirring for 2 hours, and standing for 30 min; (6) discharging the material from the vacuum impregnation reactor in step (5), filtering, washing with deionized water until neutral, and vacuum drying; The mass fraction of nitric acid in the mixed acid solution in step (1) is 5-5.5%; The mass fraction of sulfuric acid is 2.5%; The mass fraction of the sodium hydroxide solution in step (2) is 10%; The mixing ratio of graphene and sodium hydroxide solution in step (3) is 12 g:90 mL; The mixing ratio of the pre-treated mixed material and the mixed acid solution in step (4) is 10 g: 120-130 mL; The vacuum degree in the vacuum impregnation reactor in step (5) is 3-5 Pa; The vacuum drying temperature in step (6) is 55°C; The vacuum drying time was 2 hours.

2. The process for preparing the acid- and alkali-resistant polyimide film for new energy batteries according to claim 1, characterized in that: The following steps are involved: (1) Weighing the following materials in parts by weight: graphene, silicon carbide, sodium stearate, diamine monomer, dianhydride monomer, and methyltriethoxysilane; (2) adding the modified graphene and silicon carbide to N,N-dimethylacetamide, stirring for 10 minutes, and then ultrasonically treating for 5 minutes to obtain a dispersion; (3) Sodium stearate and diamine monomer are added to the dispersion in sequence, and reflux reaction is carried out for 20 hours. Then, dianhydride monomer and methyltriethoxysilane are added respectively, and stirring reaction is continued for 10 hours. Then, coating is carried out to form a film, and then a thermal imidization reaction is carried out to form a finished product, which is then cut.

Citation Information

Patent Citations

  • Polyimide film with improved alkali resistance and preparation method thereof

    CN113817196A

  • Acid and alkali resistant polyimide film for new energy battery and preparation process of acid and alkali resistant polyimide film

    CN116063847A

  • Modified polyimide copolymer and polyamic acid copolymer

    JP1990045529A

  • KR20190085315A