Preparation method of flame retardant and droplet inhibiting polyester fiber
By adding phosphorus, nitrogen and silicon flame retardants and melt drop inhibitors to polyester fibers, and using specific process parameters and spinneret shape design, the problems of flame retardancy, melt drop resistance and spinnability are solved. Taking both issues into consideration, efficient spinning production and performance improvement are achieved.
Patent Information
- Application Number
- CN202311127587.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-04
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-09-04
AI Technical Summary
In the existing technology, flame-retardant polyester fiber cannot combine flame retardancy, droplet resistance and spinnability. Especially in the spinning process, component pressure and yarn outlet continuity are limited, making it difficult to be suitable for industrial production.
By adding phosphorus-based, nitrogen-based and silicon-based flame retardants and melt-inhibiting agents to polyester, controlling their type and addition amount, using a melt spinning process, combined with specific process parameters and spinneret hole shape design, the flame retardant is achieved. Combining flammability, drip resistance and spinnability.
The prepared flame-retardant and droplet-suppressed polyester fiber has excellent flame retardancy and droplet resistance. The spinning temperature is reduced, which improves production efficiency and reduces costs, while improving the mechanical properties and comfort of the fiber.
Smart Images

Figure HDA0004428897000000011 
Figure HDA0004428897000000012 
Figure HDA0004428897000000013
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional polyester fibers and relates to a method for preparing flame-retardant and droplet-suppressing polyester fibers. Background Art
[0002] The large-scale industrial production of polyester in China began in the 1980s. Since then, with the expansion of its application scope, the polyester industry has flourished. From 2014 to 2018, the annual output of polyester in China has reached nearly 40 million tons, and in 2022 it will reach 65 million tons, accounting for more than 80% of the total output of chemical fibers in the country. With the development of the polyester industry, the demand for polyester functionalization has become increasingly prominent. Flame retardant properties, as an important indicator for measuring fire safety, occupy a very important position in the application of polyester. According to statistics, from 2012 to 2021, a total of 1.324 million fires occurred in residential places across the country, causing about 11,634 deaths and 6,738 injuries, with direct economic losses of 7.77 billion yuan. Among them, about 20% of residential places and 50% of deaths caused by fires are related to the ignition of textiles. In the combustion process, the secondary ignition caused by molten droplets poses a great hidden danger to people's lives and property safety. With the progress of science and technology and society, people pay more and more attention to environmental issues. In addition to the requirement of high flame retardancy, environmental protection is also of great concern in the selection of flame retardants. Therefore, while improving the flame retardancy of polyester fibers, it is of great practical significance to develop and use high-efficiency, environmentally friendly and non-toxic flame retardants.
[0003] In the existing technology, there are three main ways to modify polyester fibers to be flame retardant: copolymerization, blending and finishing. While these three methods bring flame retardancy, people also put forward new requirements for the comfort and health of fabrics. The preparation of flame retardant and anti-drip polyester fibers has also become one of the important directions of research on their functional modification.
[0004] Patent CN114230720A discloses an additive with both flame retardant and anti-melting dripping functions, a preparation method and a composition thereof. The patent first prepares a core layer fluorine-containing polymer dispersion, uses the fluorine-containing polymer dispersion as a seed, adds a vinyl monomer, an initiator, a chain transfer agent, and a surfactant, heats up the polymerization, and obtains a core-shell structure polymer emulsion. After condensation, centrifugation, and drying, a core-shell structure polymer is obtained, which is sulfonated and modified, washed with deionized water to neutrality, and dried after solid-liquid separation to obtain a sulfonated core-shell polymer powder. The additive is a new type of environmentally friendly, high-efficiency flame retardant and anti-melting dripping additive with excellent flame retardant and anti-melting dripping functions, and adding 0.05 to 1.50 parts to polycarbonate, ABS and its alloys, and polyester can make its flame retardant grade reach UL-94V-0. However, the preparation process of the patent is complicated, and the additive is only available in films and plastic products, and has a great influence on the pressure of components and the continuity of silk in the spinning process, and is not suitable for the production of industrial polyester fibers. Summary of the invention
[0005] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for preparing a flame retardant and drip-suppressing polyester fiber, so as to achieve the combination of flame retardancy, drip resistance and spinnability.
[0006] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0007] The method for preparing flame-retardant and anti-melting droplet polyester fiber comprises mixing polyester, flame-retardant polyester masterbatch and anti-melting droplet agent and then performing melt spinning to obtain flame-retardant and anti-melting droplet polyester fiber;
[0008] The flame retardant polyester masterbatch is flame retardant polyester masterbatch A or flame retardant polyester masterbatch B;
[0009] The preparation process of the flame retardant polyester masterbatch A is as follows: in the process of preparing polyester, a phosphorus-based flame retardant is added to the system in the esterification stage, and a nitrogen-based flame retardant and a silicon-based flame retardant are added to the system in the polycondensation stage, so as to obtain the flame retardant polyester masterbatch A;
[0010] The preparation process of the flame retardant polyester masterbatch B is as follows: polyester and IFR (intumescent flame retardant) are melt-blended to obtain the flame retardant polyester masterbatch B;
[0011] The phosphorus flame retardant is one or more of DDP ([(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid), ODOPB (10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide), and CEPPA (2-carboxyethylphenylphosphinic acid);
[0012] The nitrogen flame retardant is one or more of MCA (melamine cyanurate), KH550 (γ-aminopropyltriethoxysilane), and hexagonal boron nitride;
[0013] The silicon-based flame retardant is one or more of silicate, silicon dioxide and POSS;
[0014] The dripping inhibitor is one or more of polytetrafluoroethylene (PTFE), polyvinylidene fluoride, tetrafluoroethylene-polyvinylidene fluoride copolymer, polyhexafluoropropylene, tetrafluoroethylene-polyhexafluoropropylene copolymer, tetrafluoroethylene-polyvinylidene fluoride-polyhexafluoropropylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, copolymer of tetrafluoroethylene and other copolymerizable olefin unsaturated monomers, sulfobutyl-β-cyclodextrin (SBE-β-CD), and potassium perfluorobutyl sulfonate;
[0015] The mass ratio of polyester, flame retardant polyester masterbatch and drip inhibitor is 65-75:15-25:2-20;
[0016] The contents of phosphorus-based flame retardant, nitrogen-based flame retardant and silicon-based flame retardant in flame-retardant polyester masterbatch A are 0.5-1wt% (preferably 0.6wt%), 1-5wt% (preferably 2-3wt%) and 0.5-1wt% (preferably 0.5-0.7wt%) respectively; the content of IFR in flame-retardant polyester masterbatch B is 5-20wt% (preferably 15wt%).
[0017] The purpose of the present invention is to solve the problem that flame retardant polyester fibers in the prior art cannot take into account flame retardancy, anti-melting dripping, and spinnability. The present invention solves the problem that flame retardant polyester fibers in the prior art cannot take into account flame retardancy, anti-melting dripping, and spinnability by controlling the types, addition amounts, and addition methods of phosphorus flame retardants, nitrogen flame retardants, silicon flame retardants, and anti-melting dripping agents. The specific principles are as follows:
[0018] The dripping inhibitor of the present invention is a sulfonic acid flame retardant or a fluorine flame retardant; when phosphorus flame retardants, nitrogen flame retardants, silicon flame retardants, and sulfonic acid flame retardants (or fluorine flame retardants) are present in the system at the same time, during the combustion process, the phosphorus flame retardant copolymerized in the molecular chain breaks first due to the weak bond energy of PO, generating P· and PO· free radicals, which can combine with flammable free radicals (such as alkane free radicals) in the air to inhibit the continuous occurrence of combustion, while the nitrogen flame retardant releases N· in the gas phase. 2 Inert gases such as sulfonic acid can further dilute the concentration of combustible gases, which is the flame retardant effect of the gas phase during combustion. In the condensed phase, the presence of sulfonic acid flame retardants can catalyze the formation of polyester into carbon, covering the surface of the polymer to isolate heat and oxygen. At the same time, silicon flame retardants or fluorine flame retardants can further enhance the strength and density of the carbon layer, and the isolation effect is further enhanced.
[0019] The present invention simultaneously adds phosphorus flame retardants, nitrogen flame retardants, silicon flame retardants, and sulfonic acid flame retardants (or fluorine flame retardants) to make the polyester have excellent flame retardant properties and anti-dripping properties. Therefore, the added amount of phosphorus flame retardants, nitrogen flame retardants, silicon flame retardants, and sulfonic acid flame retardants (or fluorine flame retardants) does not need to be too high to obtain ideal flame retardant and anti-dripping effects. The added amount of phosphorus flame retardants, nitrogen flame retardants, silicon flame retardants, and sulfonic acid flame retardants (or fluorine flame retardants) is relatively low, which is conducive to the smooth spinning.
[0020] Phosphorus-based flame retardants are reactive flame retardants that participate in the molecular chain polymerization process. Therefore, they are added during the polymerization process. The remaining flame retardants and melt drop inhibitors are mainly dispersed in the melt in the form of doping. If too much is added, it is easy to cause agglomeration and affect spinning. Multiple flame retardants can play a synergistic flame retardant role in the system, effectively reducing the amount added and promoting spinning molding.
[0021] As the preferred technical solution:
[0022] In the method for preparing the flame retardant and dripping-inhibiting polyester fiber as described above, the mass ratio of polyester, flame retardant polyester masterbatch and dripping-inhibiting agent is 75:20:5, or 70:20:10, or 65:20:15.
[0023] In the preparation method of the flame retardant and drip-suppressing polyester fiber as described above, the polyester, the flame retardant polyester masterbatch and the drip-suppressing agent are all dried before mixing, the drying temperature is 116-120°C (preferably 120°C), the drying time is about 14h, and the moisture content after drying is less than 100ppm (preferably 80-90ppm).
[0024] The method for preparing the flame-retardant and droplet-suppressing polyester fiber as described above, the steps for preparing the flame-retardant polyester masterbatch A are as follows:
[0025] Ethylene glycol and terephthalic acid are slurried and mixed, and a phosphorus-based flame retardant is added to the system;
[0026] Under nitrogen or inert gas protection, raise the system temperature from 150°C to 280°C within 30 minutes, and keep the temperature for reaction for 1.5 to 2.5 hours;
[0027] Add nitrogen-based flame retardant and silicon-based flame retardant to the system, raise the temperature to 295°C, and react for 2 to 3 hours (preferably 2.7 to 3 hours) under a vacuum degree of less than 50 Pa (preferably 30 Pa, 40 Pa) to obtain flame-retardant polyester masterbatch A.
[0028] The preparation method of the flame-retardant and droplet-suppressing polyester fiber as described above, the melt spinning process includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tension heat setting → curling → oiling → relaxation heat setting → cutting.
[0029] The preparation method of the flame retardant and droplet-suppressing polyester fiber as described above, the process parameters of melt spinning include: the temperature of each zone of the screw extruder is 265-290°C (preferably 265-288°C), the temperature of the spinning box is 275-290°C, the metering pump supply is 500-900g / min (preferably 860-880g / min), the annular air temperature is 25-30°C (preferably 26-28°C), the annular air inlet pressure is 500-800Pa (preferably 720-760Pa), the winding speed is 900-1100m / min (preferably 1000-1100m / min), the drawing temperature is 65±5°C (preferably 66-68°C), and the secondary drawing multiple is 3-4 times (preferably 3.3-3.6 times).
[0030] After the present invention adds phosphorus-based flame retardants, nitrogen-based flame retardants, silicon-based flame retardants, and melt drip inhibitors to polyester through a specific adding method, the regularity of the polyester molecular chain decreases, which in turn affects the molecular weight and molecular weight distribution, which is specifically manifested as a change in rheological properties during the melt processing, which places higher requirements on the processing temperature; the addition of the melt drip inhibitor will not only change the requirements for the filter screen in the spinneret assembly, but will also affect the crystallization properties of the molecular chain, and thus affect the annular blowing temperature and annular blowing inlet pressure. The present invention ensures that melt spinning can still proceed smoothly after adding phosphorus-based flame retardants, nitrogen-based flame retardants, silicon-based flame retardants, and melt drip inhibitors to polyester by reasonably controlling the process parameters of melt spinning.
[0031] In the method for preparing the flame retardant and droplet-suppressing polyester fiber as described above, the temperatures of zones 1 to 6 of the screw extruder correspond to 265°C, 275°C, 280°C, 285°C, 280°C, and 275°C, respectively, and the spinning manifold temperature is 275°C; or, the temperatures of zones 1 to 6 of the screw extruder correspond to 265°C, 270°C, 275°C, 280°C, 275°C, and 270°C, respectively, and the spinning manifold temperature is 270°C; or, the temperatures of zones 1 to 6 of the screw extruder correspond to 270°C, 275°C, 280°C, 285°C, 280°C, and 275°C, respectively, and the spinning manifold temperature is 275°C.
[0032] In the method for preparing flame-retardant and droplet-suppressing polyester fibers as described above, the spinneret holes in the spinneret used for spinning are one or more of the following shapes: a W-shaped, a cross-shaped, a trilobal-shaped, and a four-T-shaped (ie, four T letters are evenly distributed in the cross section).
[0033] Compared with conventional round polyester fibers, after being processed using the special-shaped process, the fibers also have better fluffiness, moisture absorption and perspiration management, and higher gloss. While giving the fibers flame retardancy and anti-melting properties, it further improves and expands its application range in clothing, home textiles, and industrial fields.
[0034] The method for preparing a flame retardant and droplet-suppressing polyester fiber as described in any of the above items, wherein the fineness of the flame retardant and droplet-suppressing polyester fiber is 0.89-22.22 dtex (preferably 1.11-22.22 dtex), the breaking strength is 5.3-6.0 cN / dtex (preferably 5.3-5.9 cN / dtex), the breaking elongation is 27.1-30.7% (preferably 27.3-29.5%), the number of curls is 10.4-11.9 / 25mm, the curl rate is 11.1-12.7%, the LOI reaches more than 30% (preferably 30.1-32%), and no droplets are generated during the combustion process.
[0035] Beneficial effects:
[0036] (1) The flame-retardant and melt-drop inhibiting polyester fiber prepared by the present invention has good flame retardancy, melt-drop resistance and spinnability by controlling the types, addition amounts and addition methods of phosphorus-based flame retardants, nitrogen-based flame retardants, silicon-based flame retardants and melt-drop inhibitors. The prepared fiber has a breaking strength of up to 5.8 cN / dtex, an elongation at break of 28.9%, an LOI of over 30%, and no melt drops are generated during combustion;
[0037] (2) Compared with the spinning process of conventional polyester fibers, the flame-retardant and melt-drop inhibiting polyester fiber can achieve good spinnability at a lower spinning temperature. The spinning temperature is reduced by 10 - 15°C. The lower spinning temperature can not only delay the thermal degradation of the melt-drop inhibitor, but also effectively improve production efficiency and reduce costs;
[0038] (3) The copolymerization-blending modification method adopted by the present invention can effectively solve the problems of the decline in the mechanical properties of fibers caused by the addition of additives and the poor hand comfort of fiber products;
[0039] (4) The profiled cross-section design of the fiber of the present invention endows the fiber with better bulkiness, moisture absorption and sweat discharge properties, and higher gloss. It can further improve the comfort of the flame-retardant and melt-drop inhibiting fiber products. Moreover, the flame-retardant and melt-drop inhibiting property of the present invention can not only reduce the secondary injury caused by the combustion of clothing to the human body, but also the profiled cross-section design improves the comfort performance of the people using flame-retardant products, expanding its application fields. Description of the Drawings
[0040] Figure 1 It is a cross-sectional schematic diagram of the flame-retardant and melt-drop inhibiting polyester fiber prepared when the spinneret hole used in the present invention is in a king shape;
[0041] Figure 2 It is a cross-sectional schematic diagram of the flame-retardant and melt-drop inhibiting polyester fiber prepared when the spinneret hole used in the present invention is in a cross shape;
[0042] Figure 3 It is a cross-sectional schematic diagram of the flame-retardant and melt-drop inhibiting polyester fiber prepared when the spinneret hole used in the present invention is in a three-leaf shape;
[0043] Figure 4 It is a cross-sectional schematic diagram of the flame-retardant and melt-drop inhibiting polyester fiber prepared when the spinneret hole used in the present invention is in a four-T shape. Detailed Embodiments
[0044] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and not to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the appended claims of the present application.
[0045] The following are the manufacturers and brands of raw materials in the examples:
[0046] IFR (intumescent flame retardant): a mixture of pentaerythritol (manufacturer: Puyang Yongan Chemical Co., Ltd., brand name 126-58-9), ammonium polyphosphate (manufacturer: Shandong Zhongli Petrochemical Technology Co., Ltd., brand name P37-N11) and melamine (manufacturer: Shanghai Yuanye Biotechnology Co., Ltd., brand name B21093) in a molar ratio of 1:1:1;
[0047] PET (polyethylene terephthalate): manufacturer is Jiangsu Shenghong Science and Trade Co., Ltd., brand number is M02;
[0048] hBN (hexagonal boron nitride): manufacturer is Ark New Materials Co., Ltd., brand name is DL-7800A;
[0049] Silicate: The manufacturer is Qingdao Bay Group Co., Ltd., the brand is SSP-32;
[0050] POSS (cage polysilsesquioxane): manufacturer is Weibai'ao (Beijing) Biotechnology Co., Ltd., brand name MA0702;
[0051] PTFE (polytetrafluoroethylene): The manufacturer is Fuzhou Taipuda New Materials Co., Ltd., the brand is TPD-405B;
[0052] PVDF (polyvinylidene fluoride): manufacturer is Shanghai Huihang New Materials Co., Ltd., brand number is 3030-15;
[0053] XR (perfluorosulfonic acid resin): the manufacturer is Huainan Kedi Chemical Technology Co., Ltd., the brand is superior;
[0054] F6 (polyhexafluoropropylene): The manufacturer is Zhejiang Juhua Co., Ltd. Fluoropolymer Factory, brand number is 6792-31-0;
[0055] FEP (tetrafluoroethylene-hexafluoropropylene copolymer): the manufacturer is Dongguan Longfeng Plastic Materials Co., Ltd., the brand is NEOFLON NP-120;
[0056] ETFE (ethylene-tetrafluoroethylene copolymer): the manufacturer is Shanghai Koraman Reagent Co., Ltd., the brand is ZY4051;
[0057] PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer): the manufacturer is Dongguan Suguang Plastic Raw Materials Co., Ltd., the brand is Generic PFA;
[0058] EPE (tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether): This substance is homemade. The specific preparation process is as follows: tetrafluoroethylene, hexafluoropropylene, perfluoroalkyl ethylene in a molar ratio of 1:1:1 and a catalyst (diisopropylamine lithium LDA) with a mass fraction of 0.1% are reacted at a temperature of 180°C and a pressure of 101 MPa for 3 hours to obtain tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether;
[0059] Sulfonbutyl-β-cyclodextrin (SBE-β-CD): manufacturer is Zibo Qianhui Biotechnology Co., Ltd., brand number is 7585-39-9;
[0060] Potassium perfluorobutanesulfonate: The manufacturer is Fujian Shaowu Jintang Anshengqi Chemical Co., Ltd., and the brand number is 29420-49-3.
[0061] The following is the test method of the performance in each embodiment:
[0062] Curl number and curl rate: measured in accordance with GB / T 14338-2022 standard.
[0063] Fineness: measured in accordance with GB / T 14336-2008.
[0064] Breaking strength: measured in accordance with GB / T 14337-2022.
[0065] Elongation at break: measured in accordance with GB / T 14337-2022.
[0066] LOI: Determined in accordance with FZ / T 50017-2011.
[0067] Moisture content: Determined in accordance with GB / T 6503-2017.
[0068] Melt dripping: During the determination of FZ / T 50017-2011, the number of times and drops of the melt dripping within one minute are calculated.
[0069] Continuous burning time: the continuous burning time of the fiber prepared in the example after combustion occurs and the fire source is removed, in seconds.
[0070] Example 1
[0071] The preparation method of flame retardant and droplet inhibiting polyester fiber comprises the following steps:
[0072] (1) Preparation of raw materials:
[0073] Phosphorus flame retardant: DDP;
[0074] Nitrogen flame retardant: MCA;
[0075] Silicon flame retardant: silicate;
[0076] Melt drip inhibitor: PTFE;
[0077] Ethylene glycol;
[0078] Terephthalic acid;
[0079] Protective gas: nitrogen or inert gas;
[0080] PET;
[0081] (2) preparing flame retardant polyester masterbatch A;
[0082] (2.1) ethylene glycol and terephthalic acid are slurried and mixed in a molar ratio of 1.2:1, and a phosphorus-based flame retardant is added to the system;
[0083] (2.2) Under the protection of protective gas, the system temperature was raised from 150°C to 280°C within 30 minutes, and then kept at this temperature for 2 hours;
[0084] (2.3) adding nitrogen-based flame retardant and silicon-based flame retardant to the system, raising the temperature to 295° C., and reacting for 2.8 hours under a vacuum degree of 40 Pa to obtain flame-retardant polyester masterbatch A;
[0085] The content of phosphorus-based flame retardant in the flame-retardant polyester masterbatch A is 0.6wt%, the content of nitrogen-based flame retardant is 2wt%, and the content of silicon-based flame retardant is 0.6wt%;
[0086] (3) Preparation of flame retardant and droplet-suppressing polyester fibers;
[0087] First, PET, flame retardant polyester masterbatch A and melt-drip inhibitor are dried at 120° C. to a moisture content of 80 ppm, and then PET, flame retardant polyester masterbatch A and melt-drip inhibitor are mixed and melt-spun to obtain flame retardant and melt-drip inhibitor polyester fibers; wherein the mass ratio of PET, flame retardant polyester masterbatch A and melt-drip inhibitor is 75:15:10;
[0088] The process of melt spinning includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tensile heat setting → curling → oiling → relaxation heat setting → cutting;
[0089] The process parameters of melt spinning include: the temperature of the first zone of the screw extruder is 265°C, the temperature of the second zone is 275°C, the temperature of the third zone is 280°C, the temperature of the fourth zone is 285°C, the temperature of the fifth zone is 280°C, the temperature of the sixth zone is 275°C, the temperature of the spinning box is 275°C, the metering pump supply is 880g / min, the temperature of the annular blowing is 27°C, the annular blowing air pressure is 760Pa, the winding speed is 1050m / min, the drafting temperature is 67°C, and the secondary drafting multiple is 3.5 times;
[0090] The spinneret holes in the spinneret used for spinning are in the shape of a king character.
[0091] The cross-section of the finally obtained flame-retardant and melt-droplet-suppressing polyester fiber is as Figure 1 shown. Its fineness is 1.56 dtex, the breaking strength is 5.8 cN / dtex, the elongation at break is 28.3%, the crimp number is 10.4 per 25 mm, the crimp ratio is 11.6%, the LOI reaches 30.1%, the continuous burning time is 30 s and no melt droplets are generated during the burning process.
[0092] Comparative Example 1
[0093] The preparation method of the flame-retardant polyester fiber is basically the same as that of Example 1, except that: in step (1), no melt-droplet suppressant is prepared; in step (3), no melt-droplet suppressant is added, and the melt-droplet suppressant is replaced by an equal mass of PET (the same as in Example 1).
[0094] The fineness of the finally obtained flame-retardant polyester fiber is 1.56 dtex, the breaking strength is 5.9 cN / dtex, the elongation at break is 27.5%, the crimp number is 11.1 per 25 mm, the crimp ratio is 12.7%, the LOI reaches 29.8%, the continuous burning time is 55 s and melt droplets are generated during the burning process.
[0095] Comparing Comparative Example 1 with Example 1, it can be seen that when preparing the flame-retardant polyester fiber in Comparative Example 1, without using a melt-droplet suppressant, it will cause the generation of molten dripping, which will in turn cause secondary ignition. This is because during the combustion process of the polymer, melting degradation occurs first, the melt fluidity increases, and the melt not only plays a role in heat conduction during the flow process, but also further promotes the degradation of the polymer. At the same time, the flammable small molecules present in the melt will also cause secondary ignition of the polymer.
[0096] Example 2
[0097] The preparation method of the flame-retardant and melt-droplet-suppressing polyester fiber is basically the same as that of Example 1, except that: the melt-droplet suppressant is sulfobutyl-β-cyclodextrin.
[0098] The fineness of the finally obtained flame-retardant and melt-droplet-suppressing polyester fiber is 1.56 dtex, the breaking strength is 5.4 cN / dtex, the elongation at break is 27.7%, the crimp number is 11.1 per 25 mm, the crimp ratio is 11.1%, the LOI reaches 31%, the continuous burning time is 48 s and no melt droplets are generated during the burning process.
[0099] Comparative Example 2
[0100] The preparation method of the flame-retardant polyester fiber is basically the same as that of Example 2, except that: in step (1), no melt-droplet suppressant is prepared; in step (3), no melt-droplet suppressant is added, and the melt-droplet suppressant is replaced by an equal mass of a silicon-based flame retardant (the same as in Example 1).
[0101] The final flame-retardant polyester fiber has a fineness of 1.56 dtex, a breaking strength of 5.6 cN / dtex, an elongation at break of 28.0%, an LOI of 30.8%, a continuous burning time of 63 s, and molten droplets are generated during the burning process.
[0102] Comparative Example 3
[0103] The method for preparing flame-retardant polyester fiber is basically the same as that in Example 2, except that: in step (1), no silicon-based flame retardant is prepared; in step (2.3), no silicon-based flame retardant is added, and the silicon-based flame retardant is replaced by an equal mass of a melt drip inhibitor (the same as in Example 2).
[0104] The final flame-retardant polyester fiber has a fineness of 1.56 dtex, a breaking strength of 5.5 cN / dtex, an elongation at break of 27.9%, an LOI of 30.9%, a continuous burning time of 77 s, and no droplets are generated during the burning process.
[0105] By comparing Example 2, Comparative Example 2 and Comparative Example 3, it can be seen that the combination of sulfonic acid flame retardant and silicon flame retardant is better than that of using them alone. This is because the presence of sulfonic acid flame retardant can catalyze PET into carbon, cover the surface of the polymer, and isolate heat and oxygen. At the same time, the silicon flame retardant can further enhance the strength and density of the carbon layer, and the insulation effect is further enhanced.
[0106] Example 3
[0107] The preparation method of the flame-retardant and drip-inhibiting polyester fiber is basically the same as that of Example 1, except that the drip-inhibiting agent is a mixture of polytetrafluoroethylene and sulfobutyl-β-cyclodextrin in a mass ratio of 1:1.
[0108] The final flame retardant and droplet-suppressing polyester fiber has a fineness of 1.56 dtex, a breaking strength of 5.9 cN / dtex, an elongation at break of 29.5%, a curl number of 11.8 / 25 mm, a curl rate of 11.8%, and an LOI of 30.8%. The flame retardant polyester fiber extinguishes itself when away from fire and no droplets are generated during the combustion process.
[0109] By comparing Example 1, Example 2 and Example 3, it can be seen that the combined use of fluorine-based flame retardants and sulfonic acid-based flame retardants is more effective than using them alone. This is because the presence of the sulfonic acid-based flame retardant can catalyze PET into carbon, cover the surface of the polymer, and isolate heat and oxygen. At the same time, the fluorine-based flame retardant can further enhance the strength and density of the carbon layer, and the insulation effect is further enhanced.
[0110] Example 4
[0111] The preparation method of flame retardant and droplet inhibiting polyester fiber comprises the following steps:
[0112] (1) Preparation of raw materials:
[0113] Phosphorus flame retardant: ODOPB;
[0114] Nitrogen flame retardant: MCA;
[0115] Silicon flame retardant: silicate;
[0116] Melting drop inhibitor: PVDF;
[0117] Ethylene glycol;
[0118] Terephthalic acid;
[0119] Protective gas: nitrogen or inert gas;
[0120] PET;
[0121] (2) preparing flame retardant polyester masterbatch A;
[0122] (2.1) ethylene glycol and terephthalic acid are slurried and mixed in a molar ratio of 1.2:1, and a phosphorus-based flame retardant is added to the system;
[0123] (2.2) Under the protection of protective gas, the system temperature was raised from 150°C to 280°C within 30 minutes, and then kept at this temperature for 2 hours;
[0124] (2.3) adding nitrogen-based flame retardant and silicon-based flame retardant to the system, raising the temperature to 295° C., and reacting for 2.8 hours under a vacuum degree of 40 Pa to obtain flame-retardant polyester masterbatch A;
[0125] The content of phosphorus-based flame retardant in the flame-retardant polyester masterbatch A is 0.6wt%, the content of nitrogen-based flame retardant is 2wt%, and the content of silicon-based flame retardant is 0.6wt%;
[0126] (3) Preparation of flame retardant and droplet-suppressing polyester fibers;
[0127] First, PET, flame retardant polyester masterbatch A and melt-drip inhibitor are dried at 120° C. to a moisture content of 80 ppm, and then PET, flame retardant polyester masterbatch A and melt-drip inhibitor are mixed and melt-spun to obtain flame retardant and melt-drip inhibitor polyester fibers; wherein the mass ratio of PET, flame retardant polyester masterbatch A and melt-drip inhibitor is 75:20:5;
[0128] The process of melt spinning includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tensile heat setting → curling → oiling → relaxation heat setting → cutting;
[0129] The process parameters of melt spinning include: the temperature of the first zone of the screw extruder is 265°C, the temperature of the second zone is 275°C, the temperature of the third zone is 280°C, the temperature of the fourth zone is 285°C, the temperature of the fifth zone is 280°C, the temperature of the sixth zone is 275°C, the temperature of the spinning box is 275°C, the metering pump supply is 880g / min, the annular air temperature is 28°C, the annular air inlet pressure is 720Pa, the winding speed is 1100m / min, the drafting temperature is 68°C, and the secondary drafting multiple is 3.3 times;
[0130] The spinneret holes in the spinneret used for spinning are cross-shaped.
[0131] The cross section of the flame retardant and droplet-inhibiting polyester fiber finally obtained is as follows: Figure 2 As shown, its fineness is 1.89 dtex, breaking strength is 5.5 cN / dtex, breaking elongation is 27.9%, the number of crimps is 11.9 / 25mm, the crimp rate is 12.3%, the LOI reaches 30.6%, and no droplets are generated during the combustion process.
[0132] Example 5
[0133] The preparation method of flame retardant and droplet inhibiting polyester fiber comprises the following steps:
[0134] (1) Preparation of raw materials:
[0135] IFR;
[0136] Melt drip inhibitor: FEP;
[0137] Protective gas: nitrogen or inert gas;
[0138] PET;
[0139] (2) preparing flame retardant polyester masterbatch B;
[0140] The flame retardant polyester masterbatch B is obtained by melt blending PET and IFR;
[0141] The content of IFR in the prepared flame retardant polyester masterbatch B is 15wt%;
[0142] (3) Preparation of flame retardant and droplet-suppressing polyester fibers;
[0143] First, PET, flame retardant polyester masterbatch B and melt drip inhibitor are dried at 120° C. to a moisture content of 90 ppm, and then PET, flame retardant polyester masterbatch B and melt drip inhibitor are mixed and melt-spun to obtain flame retardant and melt drip inhibitor polyester fiber; wherein the mass ratio of PET, flame retardant polyester masterbatch B and melt drip inhibitor is 70:20:10;
[0144] The process of melt spinning includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tensile heat setting → curling → oiling → relaxation heat setting → cutting;
[0145] The process parameters of melt spinning include: the temperature of the first zone of the screw extruder is 265°C, the temperature of the second zone is 270°C, the temperature of the third zone is 275°C, the temperature of the fourth zone is 280°C, the temperature of the fifth zone is 275°C, the temperature of the sixth zone is 270°C, the temperature of the spinning box is 270°C, the metering pump supply is 870g / min, the temperature of the annular blowing is 26°C, the annular blowing air pressure is 750Pa, the winding speed is 1000m / min, the drawing temperature is 66°C, and the secondary drawing multiple is 3.6 times;
[0146] The spinneret holes in the spinneret used for spinning are trilobal.
[0147] The cross section of the flame retardant and droplet-inhibiting polyester fiber finally obtained is as follows: Figure 3 As shown, its fineness is 2.22dtex, breaking strength is 5.5cN / dtex, breaking elongation is 27.8%, the number of crimps is 11.2 / 25mm, the crimp rate is 12.6%, the LOI reaches 32%, and no droplets are generated during the combustion process.
[0148] Example 6
[0149] The preparation method of flame retardant and droplet inhibiting polyester fiber comprises the following steps:
[0150] (1) Preparation of raw materials:
[0151] IFR;
[0152] Melt drop inhibitor: F6;
[0153] Protective gas: nitrogen or inert gas;
[0154] PET;
[0155] (2) preparing flame retardant polyester masterbatch B;
[0156] The flame retardant polyester masterbatch B is obtained by melt blending PET and IFR;
[0157] The content of IFR in the prepared flame retardant polyester masterbatch B is 15wt%;
[0158] (3) Preparation of flame retardant and droplet-suppressing polyester fibers;
[0159] First, PET, flame retardant polyester masterbatch B and melt drip inhibitor are dried at 120° C. to a moisture content of 85 ppm, and then PET, flame retardant polyester masterbatch B and melt drip inhibitor are mixed and melt-spun to obtain flame retardant and melt drip inhibitor polyester fibers; wherein the mass ratio of PET, flame retardant polyester masterbatch B and melt drip inhibitor is 65:20:15;
[0160] The process of melt spinning includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tensile heat setting → curling → oiling → relaxation heat setting → cutting;
[0161] The process parameters of melt spinning include: the temperature of the first zone of the screw extruder is 270°C, the temperature of the second zone is 275°C, the temperature of the third zone is 280°C, the temperature of the fourth zone is 285°C, the temperature of the fifth zone is 280°C, the temperature of the sixth zone is 275°C, the temperature of the spinning box is 275°C, the metering pump supply is 860g / min, the temperature of the annular blowing is 27°C, the annular blowing air pressure is 740Pa, the winding speed is 1100m / min, the drafting temperature is 68°C, and the secondary drafting multiple is 3.4 times;
[0162] The spinneret holes in the spinneret used for spinning are four-T shaped.
[0163] The cross section of the flame retardant and droplet-inhibiting polyester fiber finally obtained is as follows: Figure 4 As shown, its fineness is 3.33 dtex, breaking strength is 5.3 cN / dtex, breaking elongation is 27.4%, the number of crimps is 11.2 / 25 mm, the crimp rate is 12.6%, the LOI reaches 31.8%, and no droplets are generated during the combustion process.
[0164] Example 7
[0165] The preparation method of flame retardant and droplet inhibiting polyester fiber comprises the following steps:
[0166] (1) Preparation of raw materials:
[0167] Phosphorus flame retardant: CEPPA;
[0168] Nitrogen flame retardant: KH550;
[0169] Silicon flame retardant: POSS;
[0170] Melt drip inhibitor: FEP;
[0171] Ethylene glycol;
[0172] Terephthalic acid;
[0173] Protective gas: nitrogen or inert gas;
[0174] PET;
[0175] (2) preparing flame retardant polyester masterbatch A;
[0176] (2.1) ethylene glycol and terephthalic acid are slurried and mixed in a molar ratio of 1.2:1, and a phosphorus-based flame retardant is added to the system;
[0177] (2.2) Under the protection of protective gas, the system temperature was raised from 150°C to 280°C within 30 minutes, and then kept at this temperature for 2 hours;
[0178] (2.3) Adding nitrogen-based flame retardant and silicon-based flame retardant to the system, raising the temperature to 295° C., and reacting for 3 h under a vacuum degree of 40 Pa to obtain flame-retardant polyester masterbatch A;
[0179] The content of phosphorus-based flame retardant in the flame-retardant polyester masterbatch A is 0.6wt%, the content of nitrogen-based flame retardant is 2wt%, and the content of silicon-based flame retardant is 0.6wt%;
[0180] (3) Preparation of flame retardant and droplet-suppressing polyester fibers;
[0181] First, PET, flame retardant polyester masterbatch A and melt-drip inhibitor are dried at 120° C. to a moisture content of 80 ppm, and then PET, flame retardant polyester masterbatch A and melt-drip inhibitor are mixed and melt-spun to obtain flame retardant and melt-drip inhibitor polyester fibers; wherein the mass ratio of PET, flame retardant polyester masterbatch A and melt-drip inhibitor is 75:15:10;
[0182] The process of melt spinning includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tensile heat setting → curling → oiling → relaxation heat setting → cutting;
[0183] The process parameters of melt spinning include: the temperature of the first zone of the screw extruder is 268°C, the temperature of the second zone is 278°C, the temperature of the third zone is 283°C, the temperature of the fourth zone is 288°C, the temperature of the fifth zone is 283°C, the temperature of the sixth zone is 278°C, the temperature of the spinning box is 278°C, the metering pump supply is 870g / min, the temperature of the annular blowing is 27°C, the annular blowing air pressure is 760Pa, the winding speed is 1050m / min, the drafting temperature is 67°C, and the secondary drafting multiple is 3.5 times;
[0184] The spinneret holes in the spinneret used for spinning are cross-shaped.
[0185] The final flame retardant and droplet-suppressing polyester fiber has a fineness of 11.11 dtex, a breaking strength of 5.3 cN / dtex, an elongation at break of 27.5%, a curl number of 11.2 / 25 mm, a curl rate of 12.6%, an LOI of 31.9%, and no droplets are generated during the combustion process.
[0186] Example 8
[0187] The preparation method of flame retardant and droplet inhibiting polyester fiber comprises the following steps:
[0188] (1) Preparation of raw materials:
[0189] Phosphorus flame retardant: DDP;
[0190] Nitrogen flame retardant: hBN;
[0191] Silicon flame retardant: POSS;
[0192] Melt drip inhibitor: PFA;
[0193] Ethylene glycol;
[0194] Terephthalic acid;
[0195] Protective gas: nitrogen or inert gas;
[0196] PET;
[0197] (2) preparing flame retardant polyester masterbatch A;
[0198] (2.1) ethylene glycol and terephthalic acid in a molar ratio of 1.2:1 are slurried and mixed, and a phosphorus-based flame retardant is added to the system;
[0199] (2.2) Under the protection of protective gas, the system temperature was raised from 150°C to 280°C within 30 minutes, and then kept at this temperature for 2 hours;
[0200] (2.3) adding nitrogen-based flame retardant and silicon-based flame retardant to the system, raising the temperature to 295° C., and reacting for 2.8 hours under a vacuum degree of 30 Pa to obtain flame-retardant polyester masterbatch A;
[0201] The content of phosphorus-based flame retardant in the flame-retardant polyester masterbatch A is 0.6wt%, the content of nitrogen-based flame retardant is 3wt%, and the content of silicon-based flame retardant is 0.7wt%;
[0202] (3) Preparation of flame retardant and droplet-suppressing polyester fibers;
[0203] First, PET, flame retardant polyester masterbatch A and melt drip inhibitor are dried at 120° C. to a moisture content of 90 ppm, and then PET, flame retardant polyester masterbatch A and melt drip inhibitor are mixed and melt-spun to obtain flame retardant and melt drip inhibitor polyester fibers; wherein the mass ratio of PET, flame retardant polyester masterbatch A and melt drip inhibitor is 70:15:15;
[0204] The process of melt spinning includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tensile heat setting → curling → oiling → relaxation heat setting → cutting;
[0205] The process parameters of melt spinning include: the temperature of the first zone of the screw extruder is 266°C, the temperature of the second zone is 276°C, the temperature of the third zone is 281°C, the temperature of the fourth zone is 286°C, the temperature of the fifth zone is 281°C, the temperature of the sixth zone is 276°C, the temperature of the spinning box is 276°C, the metering pump supply is 860g / min, the temperature of the annular blowing is 28°C, the annular blowing air pressure is 760Pa, the winding speed is 1000m / min, the drawing temperature is 66°C, and the secondary drawing multiple is 3.6 times;
[0206] The spinneret holes in the spinneret used for spinning are trilobal.
[0207] The final flame retardant and droplet-suppressing polyester fiber has a fineness of 13.32 dtex, a breaking strength of 5.3 cN / dtex, an elongation at break of 27.5%, a curl number of 11.1 / 25 mm, a curl rate of 11.7%, an LOI of 32.1%, and no droplets are generated during the combustion process.
[0208] Example 9
[0209] The preparation method of flame retardant and droplet inhibiting polyester fiber comprises the following steps:
[0210] (1) Preparation of raw materials:
[0211] IFR;
[0212] Melt drip inhibitor: PFA;
[0213] Protective gas: nitrogen or inert gas;
[0214] PET;
[0215] (2) preparing flame retardant polyester masterbatch B;
[0216] The flame retardant polyester masterbatch B is obtained by melt blending PET and IFR;
[0217] The content of IFR in the prepared flame retardant polyester masterbatch B is 15wt%;
[0218] (3) Preparation of flame retardant and droplet-suppressing polyester fibers;
[0219] First, PET, flame retardant polyester masterbatch B and melt drip inhibitor are dried at 120° C. to a moisture content of 85 ppm, and then PET, flame retardant polyester masterbatch B and melt drip inhibitor are mixed and melt-spun to obtain flame retardant and melt drip inhibitor polyester fibers; wherein the mass ratio of PET, flame retardant polyester masterbatch B and melt drip inhibitor is 65:15:20;
[0220] The process of melt spinning includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tensile heat setting → curling → oiling → relaxation heat setting → cutting;
[0221] The process parameters of melt spinning include: the temperature of the first zone of the screw extruder is 265°C, the temperature of the second zone is 275°C, the temperature of the third zone is 280°C, the temperature of the fourth zone is 285°C, the temperature of the fifth zone is 280°C, the temperature of the sixth zone is 275°C, the temperature of the spinning box is 275°C, the metering pump supply is 880g / min, the annular air temperature is 26°C, the annular air inlet pressure is 720Pa, the winding speed is 1100m / min, the drafting temperature is 68°C, and the secondary drafting multiple is 3.4 times;
[0222] The spinneret holes in the spinneret used for spinning are four-T shaped.
[0223] The final flame retardant and droplet-suppressing polyester fiber has a fineness of 1.89 dtex, a breaking strength of 5.5 cN / dtex, an elongation at break of 28.7%, a curl number of 11.1 / 25 mm, a curl rate of 11.7%, an LOI of 30.6%, and no droplets are generated during the combustion process.
[0224] Example 10
[0225] The preparation method of flame retardant and droplet inhibiting polyester fiber comprises the following steps:
[0226] (1) Preparation of raw materials:
[0227] IFR;
[0228] Melt drip inhibitor: EPE;
[0229] Protective gas: nitrogen or inert gas;
[0230] PET;
[0231] (2) preparing flame retardant polyester masterbatch B;
[0232] The flame retardant polyester masterbatch B is obtained by melt blending PET and IFR;
[0233] The content of IFR in the prepared flame retardant polyester masterbatch B is 15wt%;
[0234] (3) Preparation of flame retardant and droplet-suppressing polyester fibers;
[0235] First, PET, flame retardant polyester masterbatch B and melt drip inhibitor are dried at 120° C. to a moisture content of 80 ppm, and then PET, flame retardant polyester masterbatch B and melt drip inhibitor are mixed and melt-spun to obtain flame retardant and melt drip inhibitor polyester fibers; wherein the mass ratio of PET, flame retardant polyester masterbatch B and melt drip inhibitor is 65:25:10;
[0236] The process of melt spinning includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tensile heat setting → curling → oiling → relaxation heat setting → cutting;
[0237] The process parameters of melt spinning include: the temperature of the first zone of the screw extruder is 268°C, the temperature of the second zone is 278°C, the temperature of the third zone is 283°C, the temperature of the fourth zone is 288°C, the temperature of the fifth zone is 283°C, the temperature of the sixth zone is 278°C, the temperature of the spinning box is 278°C, the metering pump supply is 870g / min, the temperature of the annular blowing is 27°C, the annular blowing air pressure is 750Pa, the winding speed is 1050m / min, the drafting temperature is 67°C, and the secondary drafting multiple is 3.5 times;
[0238] The spinneret holes in the spinneret used for spinning are cross-shaped.
[0239] The final flame retardant and droplet-suppressing polyester fiber has a fineness of 2.22 dtex, a breaking strength of 5.5 cN / dtex, an elongation at break of 28.6%, a curl number of 10.9 / 25 mm, a curl rate of 12.2%, an LOI of 31.4%, and no droplets are generated during the combustion process.
[0240] Embodiment 11
[0241] The preparation method of flame retardant and droplet inhibiting polyester fiber comprises the following steps:
[0242] (1) Preparation of raw materials:
[0243] Phosphorus flame retardant: DDP;
[0244] Nitrogen flame retardant: KH550;
[0245] Silicon flame retardant: POSS;
[0246] Melting drop inhibitor: potassium perfluorobutanesulfonate;
[0247] Ethylene glycol;
[0248] Terephthalic acid;
[0249] Protective gas: nitrogen or inert gas;
[0250] PET;
[0251] (2) preparing flame retardant polyester masterbatch A;
[0252] (2.1) ethylene glycol and terephthalic acid are slurried and mixed in a molar ratio of 1.2:1, and a phosphorus-based flame retardant is added to the system;
[0253] (2.2) Under the protection of protective gas, the system temperature was raised from 150°C to 280°C within 30 minutes, and then kept at this temperature for 2 hours;
[0254] (2.3) adding nitrogen-based flame retardant and silicon-based flame retardant to the system, raising the temperature to 295° C., and reacting for 2.9 hours under a vacuum degree of 30 Pa to obtain flame-retardant polyester masterbatch A;
[0255] The content of phosphorus-based flame retardant in the flame-retardant polyester masterbatch A is 0.6wt%, the content of nitrogen-based flame retardant is 3wt%, and the content of silicon-based flame retardant is 0.7wt%;
[0256] (3) Preparation of flame retardant and droplet-suppressing polyester fibers;
[0257] First, PET, flame retardant polyester masterbatch A and melt drip inhibitor are dried at 120° C. to a moisture content of 90 ppm, and then PET, flame retardant polyester masterbatch A and melt drip inhibitor are mixed and melt-spun to obtain flame retardant and melt drip inhibitor polyester fibers; wherein the mass ratio of PET, flame retardant polyester masterbatch A and melt drip inhibitor is 70:15:15;
[0258] The process of melt spinning includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tensile heat setting → curling → oiling → relaxation heat setting → cutting;
[0259] The process parameters of melt spinning include: the temperature of the first zone of the screw extruder is 266°C, the temperature of the second zone is 276°C, the temperature of the third zone is 281°C, the temperature of the fourth zone is 286°C, the temperature of the fifth zone is 281°C, the temperature of the sixth zone is 276°C, the temperature of the spinning box is 276°C, the metering pump supply is 860g / min, the temperature of the annular air is 27°C, the annular air inlet pressure is 740Pa, the winding speed is 1000m / min, the drafting temperature is 68°C, and the secondary drafting multiple is 3.5 times;
[0260] The spinneret holes in the spinneret used for spinning are cross-shaped.
[0261] The final flame retardant and droplet-suppressing polyester fiber has a fineness of 22.22 dtex, a breaking strength of 5.3 cN / dtex, an elongation at break of 27.3%, a curl number of 11.7 / 25 mm, a curl rate of 11.9%, an LOI of 31.2%, and no droplets are generated during the combustion process.
[0262] Example 12
[0263] The preparation method of flame retardant and droplet inhibiting polyester fiber comprises the following steps:
[0264] (1) Preparation of raw materials:
[0265] Phosphorus flame retardant: a mixture of DDP and ODOPB in a mass ratio of 1:1;
[0266] Nitrogen flame retardant: a mixture of MCA and KH550 in a mass ratio of 1:1;
[0267] Silicon flame retardant: a mixture of silicate and silicon dioxide in a mass ratio of 1:1;
[0268] Melting drop inhibitor: a mixture of polytetrafluoroethylene and sulfobutyl-β-cyclodextrin in a mass ratio of 1:1;
[0269] Ethylene glycol;
[0270] Terephthalic acid;
[0271] Protective gas: nitrogen or inert gas;
[0272] PET;
[0273] (2) preparing flame retardant polyester masterbatch A;
[0274] (2.1) ethylene glycol and terephthalic acid in a molar ratio of 1.2:1 are slurried and mixed, and a phosphorus-based flame retardant is added to the system;
[0275] (2.2) Under the protection of protective gas, the system temperature was raised from 150°C to 280°C within 30 minutes, and then kept at this temperature for 2 hours;
[0276] (2.3) Adding nitrogen-based flame retardant and silicon-based flame retardant to the system, raising the temperature to 295° C., and reacting for 3 h under a vacuum degree of 40 Pa to obtain flame-retardant polyester masterbatch A;
[0277] The content of phosphorus-based flame retardant in the flame-retardant polyester masterbatch A is 0.6wt%, the content of nitrogen-based flame retardant is 2.5wt%, and the content of silicon-based flame retardant is 0.5wt%;
[0278] (3) Preparation of flame retardant and droplet-suppressing polyester fibers;
[0279] First, PET, flame retardant polyester masterbatch A and melt-drip inhibitor are dried at 120° C. to a moisture content of 85 ppm, and then PET, flame retardant polyester masterbatch A and melt-drip inhibitor are mixed and melt-spun to obtain flame retardant and melt-drip inhibitor polyester fibers; wherein the mass ratio of PET, flame retardant polyester masterbatch A and melt-drip inhibitor is 65:15:20;
[0280] The process of melt spinning includes: screw extruder melt extrusion → spinning → annular air cooling → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tensile heat setting → curling → oiling → relaxation heat setting → cutting;
[0281] The process parameters of melt spinning include: the temperature of the first zone of the screw extruder is 265°C, the temperature of the second zone is 275°C, the temperature of the third zone is 280°C, the temperature of the fourth zone is 285°C, the temperature of the fifth zone is 280°C, the temperature of the sixth zone is 275°C, the temperature of the spinning box is 275°C, the metering pump supply is 870g / min, the annular air temperature is 26°C, the annular air inlet pressure is 760Pa, the winding speed is 1100m / min, the drafting temperature is 67°C, and the secondary drafting multiple is 3.3 times;
[0282] The spinneret holes used for spinning are in the shape of a Chinese character and a cross with a number ratio of 1:1.
[0283] The final flame retardant and droplet-suppressing polyester fiber has a fineness of 11.11 dtex, a breaking strength of 5.3 cN / dtex, an elongation at break of 27.4%, a curl number of 11.9 / 25 mm, a curl rate of 11.6%, an LOI of 30.9%, and no droplets are generated during the combustion process.
[0284] Example 13
[0285] The method for preparing flame-retardant and drip-suppressing polyester fiber is basically the same as that in Example 12, except that the drip-suppressing agent used in step (3) is XR.
[0286] The final flame retardant and droplet-suppressing polyester fiber has a fineness of 11.12 dtex, a breaking strength of 5.4 cN / dtex, an elongation at break of 27.1%, a curl number of 10.8 / 25 mm, a curl rate of 12%, an LOI of 30.7%, and no droplets are generated during the combustion process.
[0287] Embodiment 14
[0288] The method for preparing flame-retardant and drip-suppressing polyester fiber is basically the same as that in Example 12, except that the drip-suppressing agent used in step (3) is ETFE.
[0289] The final flame retardant and droplet-suppressing polyester fiber has a fineness of 11.11 dtex, a breaking strength of 5.4 cN / dtex, an elongation at break of 27.6%, a curl number of 11.1 / 25 mm, a curl rate of 12.7%, an LOI of 30.6%, and no droplets are generated during the combustion process.
[0290] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.
Claims
1. A method for preparing flame retardant and droplet-suppressing polyester fiber, characterized in that: The polyester, the flame retardant polyester masterbatch and the dripping inhibitor are mixed and then melt-spinned to obtain the flame retardant and dripping inhibitor polyester fiber; The preparation steps of flame retardant polyester masterbatch are as follows: (1) ethylene glycol and terephthalic acid are slurried and mixed, and a phosphorus-based flame retardant is added to the system; (2) Under the protection of nitrogen or inert gas, the system temperature is raised from 150°C to 280°C within 30 minutes, and the temperature is kept for reaction for 1.5 to 2.5 hours; (3) adding a nitrogen-based flame retardant and a silicon-based flame retardant to the system, raising the temperature to 295° C., and reacting for 2 to 3 hours under a vacuum degree of less than 50 Pa to obtain a flame-retardant polyester masterbatch; The phosphorus flame retardant is one or more of DDP and CEPPA; The nitrogen flame retardant is one or more of MCA, KH550 and hexagonal boron nitride; The silicon-based flame retardant is one or more of silicate, silicon dioxide and POSS; The dripping inhibitor is one or more of polytetrafluoroethylene, polyvinylidene fluoride, tetrafluoroethylene-polyvinylidene fluoride copolymer, polyhexafluoropropylene, tetrafluoroethylene-polyhexafluoropropylene copolymer, tetrafluoroethylene-polyvinylidene fluoride-polyhexafluoropropylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, copolymer of tetrafluoroethylene and other copolymerizable olefin unsaturated monomers, sulfobutyl-β-cyclodextrin, and potassium perfluorobutyl sulfonate; The mass ratio of polyester, flame retardant polyester masterbatch and drip inhibitor is 65-75:15-25:2-20; The contents of phosphorus-based flame retardant, nitrogen-based flame retardant and silicon-based flame retardant in the flame-retardant polyester masterbatch are 0.5-1wt%, 1-5wt% and 0.5-1wt% respectively.
2. The method for preparing flame retardant and drip-suppressing polyester fiber according to claim 1, characterized in that: The mass ratio of polyester, flame retardant polyester masterbatch and drip inhibitor is 75:20:5, or 70:20:10, or 65:20:
15.
3. The method for preparing the flame retardant and droplet-suppressing polyester fiber according to claim 1, characterized in that: The polyester, flame retardant polyester masterbatch and drip inhibitor are all dried before mixing, the drying temperature is 116-120°C, and the moisture content after drying is less than 100ppm.
4. The method for preparing the flame retardant and dripping-suppressing polyester fiber according to claim 1, characterized in that: The process flow of melt spinning includes: melt extrusion by screw extruder → spinning → cooling by annular air blowing → winding → forming to obtain raw yarn → raw yarn bundling → two-stage drawing → tension heat setting → curling → oiling → relaxation heat setting → cutting.
5. The method for preparing the flame retardant and dripping-suppressing polyester fiber according to claim 4, characterized in that: The process parameters of melt spinning include: temperature of each zone of the screw extruder is 265-290°C, temperature of the spinning box is 275-290°C, supply of the metering pump is 500-900g / min, temperature of the annular air is 25-30°C, inlet pressure of the annular air is 500-800Pa, winding speed is 900-1100m / min, drawing temperature is 65±5°C, and secondary drawing multiple is 3-4 times.
6. The method for preparing the flame retardant and droplet-suppressing polyester fiber according to claim 5, characterized in that: The temperatures of zones 1 to 6 of the screw extruder correspond to 265°C, 275°C, 280°C, 285°C, 280°C, and 275°C, respectively, and the spinning box temperature is 275°C; alternatively, the temperatures of zones 1 to 6 of the screw extruder correspond to 265°C, 270°C, 275°C, 280°C, 275°C, and 270°C, respectively, and the spinning box temperature is 270°C; alternatively, the temperatures of zones 1 to 6 of the screw extruder correspond to 270°C, 275°C, 280°C, 285°C, 280°C, and 275°C, respectively, and the spinning box temperature is 275°C.
7. The method for preparing the flame retardant and droplet-suppressing polyester fiber according to claim 4, characterized in that: The spinneret holes in the spinneret used for spinning are one or more of the following shapes: a W-shaped, a cross-shaped, a trilobal-shaped, and a quad-T-shaped.
8. The method for preparing the flame retardant and dripping-suppressing polyester fiber according to any one of claims 1 to 7, characterized in that: The flame retardant and droplet-suppressing polyester fiber has a fineness of 0.89-22.22 dtex, a breaking strength of 5.3-6.0 cN / dtex, a breaking elongation of 27.1-30.7%, a crimp number of 10.4-11.9 / 25mm, a crimp rate of 11.1-12.7%, an LOI of more than 30%, and no droplets are generated during the combustion process.
Citation Information
Patent Citations
Additive with flame-retardant and anti-dripping functions as well as preparation method and composition thereof
CN114230720A
Antifouling, flame retardant and anti-dripping polyester fibers and preparation method thereof
CN104451938A
Preparation method of environmentally-friendly flame-retardant polyester bulked continuous filament
CN105133085A
Flame-resistant polyester fiber and preparation method thereof
CN105463610A
Modified inflaming retarding polyethylene glycol terephthalate system and preparation method thereof