A dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating and preparation method thereof
By using nano-scale and micron-scale binary doped ultra-high-temperature ceramic powders to prepare gradient porosity coatings in nuclear power plant equipment, the problem of high-temperature fatigue and thermal insulation performance compatibility of materials has been solved, and efficient thermal insulation and wear resistance have been achieved. , extending equipment service life and reducing design and construction costs.
Patent Information
- Application Number
- CN202311268423.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-09-28
AI Technical Summary
When the existing technology increases the service temperature of nuclear power plant equipment, the high-temperature fatigue and high-temperature creep properties of the materials decrease, resulting in lower allowable limits and shortened service life. In addition, the thermal insulation performance and mechanical properties of the thermal insulation materials are incompatible, resulting in design difficulties. Large and high cost.
Nano-scale and micron-scale dual-component doped ultra-high-temperature ceramic powders are used to prepare dense outer layers and loose inner layers on both sides to form a microstructure with gradient porosity. Dual-component doped gradient porous materials are prepared through vacuum hot-pressing sintering and grinding and polishing. Ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating.
The load-bearing, heat-insulating and wear-resistant properties of the coating are achieved, the mechanical properties and heat-insulating properties of the material are improved, the service life is extended, and the design and construction costs are reduced.
Smart Images

Figure CN117263712B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ultra-high temperature heat-insulating, pressure-resistant and wear-resistant coating materials and their preparation, and specifically relates to a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating and its preparation method. Background Art
[0002] The development of the nuclear power industry is an important measure to effectively improve my country's energy supply structure, reduce the emission of pollutants from the power industry, and mitigate the global greenhouse effect. It plays an important role in ensuring national energy security and economic security. With the continuous updating of nuclear power reactor types, the relevant design parameters of nuclear power plants are constantly improving, especially the service temperature of nuclear power plants. The service temperature of the fourth-generation reactors currently recognized internationally has generally exceeded 500°C. Under long-term high-temperature service, the high-temperature fatigue and high-temperature creep properties of materials will decrease significantly, resulting in a sharp decrease in their allowable limits and a shortened service life. In order to ensure the safety and reliability of nuclear-grade components, the requirements can only be met during the design process by increasing the thickness of the bracket, changing the layout plan, or even replacing high-performance materials. Not only is the design improvement difficult, but the cost is also extremely high, resulting in a waste of manpower and material resources.
[0003] The design temperature of the reactor body and energy conversion system of the air-cooled micro reactor is as high as 600℃, which is much higher than the long-term safe operation limit of concrete of 70℃. In order to ensure the pressure bearing capacity of the concrete structure, the support system of the pressure vessel needs to be cooled. There are two commonly used methods: (1) lengthen the distance between the reactor body and the concrete, and let the temperature transferred from the support system to the concrete reach below 70℃ through natural heat dissipation of the support system; (2) use an independent support cooling system to cool the support system to ensure that the concrete temperature at the support position can meet the specification requirements under any working conditions. However, both of the above methods still have various shortcomings: the first method mentioned above will not only increase the size of the reactor body, but also be unfavorable for the seismic analysis of the reactor body and the energy conversion system; the second method mentioned above uses a separate support cooling system, which will not only cause unnecessary heat loss of the reactor body, but also increase the design difficulty and construction cost.
[0004] At present, the research on thermal insulation materials has gradually become a development direction. The thermal insulation performance of materials is usually achieved by increasing the porosity, but the increase in porosity will lead to the loss of mechanical properties and antioxidant properties of the material. Therefore, how to make all aspects of performance compatible is the key to the development and application of thermal insulation materials. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating in view of the deficiencies of the above-mentioned prior art. The method uses nano-scale dual-doped ultra-high temperature ceramic powder and micron-scale dual-doped ultra-high temperature ceramic powder to prepare the dense outer layers on both sides of the coating and the loose inner layer in the middle, forming a gradient porosity and obtaining a microstructure with a loose interior and a dense exterior, giving full play to the advantages of each layer of ultra-high temperature ceramic material, so that the coating has the characteristics of load-bearing, heat insulation and wear resistance at the same time, solving the problem that the thermal insulation performance and mechanical properties of the material are difficult to be compatible.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating, characterized in that the method comprises the following steps:
[0007] Step 1: Powder selection: select nano-scale dual-element doped ultra-high temperature ceramic powder as the outer layer powder, and select micron-scale dual-element doped ultra-high temperature ceramic powder as the inner layer powder;
[0008] Step 2, powder preparation: according to the composition system of the outer layer powder and the inner layer powder selected in step 1, raw materials are selected respectively, mixed evenly by a powder mixer, and then dried to obtain the outer layer powder and the inner layer powder respectively;
[0009] Step 3, filling powder: laying carbon paper on the inner side of the mold barrel of the graphite mold and the surface of the lower graphite press head, selecting the outer layer powder obtained in step 2 to fill in the graphite mold, and compacting it with the upper graphite press head, then selecting the inner layer powder obtained in step 2 to fill in the compacted outer layer powder in batches, and compacting it with the upper graphite press head, continuing to select the outer layer powder obtained in step 2 to fill in the compacted inner layer powder, and compacting it with the upper graphite press head, then laying carbon paper on the upper surface of the compacted outer layer powder of the upper layer and placing the upper graphite press head, and wrapping carbon felt on the outer surface of the graphite mold to obtain a graphite mold filled with powder;
[0010] Step 4: Pre-pressing: pre-pressing the graphite mold filled with powder obtained in step 3 by applying a compressive stress of 10 MPa to 30 MPa;
[0011] Step 5, sintering: placing the graphite mold pre-pressed in step 3 in a vacuum environment, then applying a compressive stress of 30 MPa to 60 MPa and sintering, and obtaining a sintered body after demolding;
[0012] Step 6, grinding and polishing: Use a 60-400 mesh diamond grinding wheel to roughly grind the outer side of the sintered body obtained in step 5 to remove the outer carbon paper, and then use metallographic sandpaper to grind and polish until the surface reaches a mirror effect, thereby obtaining a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating.
[0013] The present invention uses nano-scale and micron-scale dual-doped ultra-high temperature ceramic powders as outer and inner layer powders respectively, and then fills the powder in the manner of outer layer powder-inner layer powder-outer layer powder. After pre-pressing, hot pressing and sintering are performed under a vacuum environment. After demolding, the dual-doped gradient porous ultra-high temperature ceramic coating with a structure of outer layers on both sides and mixed inner layers is obtained by grinding and polishing. In the preparation process, ultra-high temperature ceramic powder is first used as the raw material for preparing the coating to ensure the heat resistance of the coating; then, according to the influence of powder particle size on ceramic grain size, porosity and performance, nano-level dual-element doped ultra-high temperature ceramic powder is used to prepare a dense outer layer with small porosity, high strength and good wear resistance on both sides, and micron-level dual-element doped ultra-high temperature ceramic powder is used to prepare a loose inner layer with large internal porosity, good strength and good thermal insulation performance, thereby forming a gradient porosity and obtaining a microstructure with loose interior and dense exterior, giving full play to the advantages of each layer of ultra-high temperature ceramic material, namely the wear-resistant and anti-oxidation properties of the outer layer and the thermal insulation properties of the inner layer, so that the coating has the characteristics of load-bearing, heat-insulating and wear-resistant at the same time, realizing the load-bearing-heat-insulating-wear-resistant integrated design and preparation of materials and structures.
[0014] Generally, the present invention limits the thickness of the outer layer and the inner layer on both sides of the coating according to the thickness requirement or the anti-oxidation performance requirement of the target product coating. Generally, the thickness of the outer layer on both sides is 0.1 mm to 1 mm.
[0015] The above-mentioned method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating is characterized in that the mass purity of the nano-scale dual-doped ultra-high temperature ceramic powder in step one is more than 99%, and the particle size is 30nm to 100nm; the mass purity of the micron-scale dual-doped ultra-high temperature ceramic powder is more than 99%, and the particle size is 1μm to 5μm. Generally, the smaller the particle size of the above two powders and the smaller the porosity formed, the better the mechanical properties of the corresponding structure, the better the wear resistance, the lower the thermal insulation performance, and the higher the price; the larger the particle size and the larger the porosity formed, the lower the mechanical properties of the corresponding structure, the lower the wear resistance, the better the thermal insulation performance, and the lower the price; comprehensively considering the performance requirements of the inner layer and the outer layers on both sides of the coating and cost control, powders of the above-mentioned particle sizes are selected respectively.
[0016] The above-mentioned method for preparing a binary doped gradient porous ultra-high temperature ceramic thermal insulation, pressure-resistant and wear-resistant coating is characterized in that the binary component system of the nano-scale binary doped ultra-high temperature ceramic powder in step one is: ZrO2-SiC, ZrB2-SiC, ZrC-SiC, NbB2-SiC, NbC-SiC, HfB2-SiC, HfC-SiC, TaB2-SiC or TaC-SiC; the binary component system of the micron-scale binary doped ultra-high temperature ceramic powder is: ZrO2-SiC, ZrB2-SiC, ZrC-SiC, NbB2-SiC, NbC-SiC, HfB2-SiC, HfC-SiC, TaB2-SiC or TaC-SiC. The outer layer and inner layer powders of the present invention are both made of dual-element doped ultra-high temperature ceramic powder. By controlling the main component of the powder to be ZrO2, ZrB2, ZrC, NbB2, NbC, HfB2, HfC, TaB2 or TaC, it is ensured that it belongs to the category of ultra-high temperature ceramic powder, thereby ensuring the heat resistance of the coating. At the same time, SiC is used as a sintering aid to play a modifying function, effectively eliminating the grain size defects of the main component during the sintering process, thereby greatly improving the mechanical properties of the material.
[0017] The above-mentioned method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating is characterized in that the dual-component system of the nano-scale dual-doped ultra-high temperature ceramic powder and the micron-scale dual-doped ultra-high temperature ceramic powder in step 1 is the same. The present invention reduces the thermal adaptation stress of each layer in the coating by selecting the same dual-component system as the components of the outer layer and the inner layer on both sides of the coating, thereby improving the stability of the coating structure.
[0018] The above-mentioned method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating is characterized in that the dual component system of the nano-scale dual-doped ultra-high temperature ceramic powder and the micron-scale dual-doped ultra-high temperature ceramic powder in step 1 is ZrC-SiC. The raw materials of this preferred dual component system are easy to obtain, cost-effective, and widely used.
[0019] The above-mentioned method for preparing a binary doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating is characterized in that the binary component system of the nano-scale binary doped ultra-high temperature ceramic powder and the micron-scale binary doped ultra-high temperature ceramic powder is ZrC-20% SiC, ZrC-15% SiC, ZrC-10% SiC or ZrC-5% SiC in volume percentage.
[0020] The above-mentioned method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating is characterized in that the mixing time in step 2 is 24 hours, and the drying temperature is 150°C and the time is 24 hours.
[0021] The above-mentioned method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating is characterized in that the sintering process described in step five is: first heating to 1000°C for 10 minutes and keeping warm for 5 minutes, then continuing to heat to 1750°C for 10 minutes and keeping warm for 20 minutes, and then cooling to 150°C in the furnace and taking out.
[0022] In addition, the present invention also discloses a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating prepared by the above method.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] 1. The present invention adopts nano-scale dual-element doped ultra-high temperature ceramic powder to prepare a dense outer layer with small porosity on both sides, high strength and good wear resistance, and simultaneously adopts micron-scale dual-element doped ultra-high temperature ceramic powder to prepare a loose inner layer with large internal porosity, good strength and good thermal insulation performance, forming a gradient porosity and obtaining a microstructure with loose interior and dense exterior, giving full play to the advantages of each layer of ultra-high temperature ceramic material, so that the coating has the characteristics of load-bearing, heat insulation and wear resistance at the same time, and is suitable for thermal insulation materials for nuclear power.
[0025] 2. The present invention controls the particle size of the dual-doped ultra-high temperature ceramic powder for preparing the outer layers and the inner layers on both sides, and then controls the porosity of the outer layers and the inner layers on both sides, thereby adjusting the mechanical properties, wear resistance and thermal insulation properties of the coating to meet the application requirements of different occasions. It is flexible, convenient and easy to implement.
[0026] 3. The present invention selects the same binary component system as the components of the outer layer and the inner layer on both sides of the coating to reduce the thermal adaptation stress of each layer in the coating and improve the stability of the coating structure.
[0027] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The present invention is a flow chart of the preparation process of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating.
[0029] Figure 2 It is a schematic diagram of the powder filling process of the present invention.
[0030] Figure 3 This is a physical picture of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating prepared in Example 1 of the present invention.
[0031] Figure 4 This is a compressive strain-compressive stress curve of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating prepared in Example 1 of the present invention.
[0032] Figure 5 This is a test chart of the thermal insulation performance of the dual-doped gradient porous ultra-high temperature ceramic thermal insulation, pressure-resistant and wear-resistant coating prepared in Example 1 of the present invention.
[0033] Figure 6 This is a physical picture of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating prepared in Example 2 of the present invention.
[0034] Figure 7a This is a scanning electron microscope image of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating prepared in Example 2 of the present invention.
[0035] Figure 7b for Figure 7a SEM images of the middle and outer layers.
[0036] Figure 7c for Figure 7a SEM image of the middle inner layer.
[0037] Figure 8 This is a curve chart showing the relationship between the compressive strength and oxidation time of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0038] Example 1
[0039] like Figure 1 As shown, this embodiment includes the following steps:
[0040] Step 1, powder selection: select a nano-scale dual-element doped ultra-high temperature ceramic powder with a mass purity of 99.9% and a particle size of 30nm to 100nm as the outer layer powder, and select a micron-scale dual-element doped ultra-high temperature ceramic powder with a mass purity of 99.9% and a particle size of 1μm to 5μm as the inner layer powder; the binary component system of the nano-scale dual-element doped ultra-high temperature ceramic powder is ZrC-15% SiC by volume percentage, wherein the particle size of the ZrC powder is 100nm, and the particle size of the SiC powder is 30nm; the binary component system of the micron-scale dual-element doped ultra-high temperature ceramic powder is ZrC-15% SiC by volume percentage, wherein the particle size of the ZrC powder is 5μm, and the particle size of the SiC powder is 2μm;
[0041] Step 2, powder preparation: according to the composition system of the outer layer powder and the inner layer powder selected in step 1, respectively select raw materials and use a powder mixer to mix them evenly for 24 hours and dry them at 150° C. for 24 hours to obtain outer layer powder and inner layer powder respectively;
[0042] Step 3: Fill with powder: Figure 2As shown, a carbon paper with a thickness of 0.02 mm is laid on the inner side of the mold barrel of the graphite mold and the surface of the lower graphite pressure head, the outer layer powder obtained in step 2 is selected to be filled into the graphite mold, and the upper graphite pressure head is used to compact it, and then the inner layer powder obtained in step 2 is selected to be filled in the compacted outer layer powder in batches, and the upper graphite pressure head is used to compact it, and the outer layer powder obtained in step 2 is continuously selected to be filled in the compacted inner layer powder, and the upper graphite pressure head is used to compact it, and then the carbon paper is laid on the upper surface of the compacted outer layer powder of the upper layer and the upper graphite pressure head is placed, and the carbon felt is wrapped on the outer surface of the graphite mold to obtain a graphite mold filled with powder;
[0043] Step 4: Pre-pressing: pre-pressing the graphite mold filled with powder obtained in step 3 by applying a compressive stress of 20 MPa;
[0044] Step 5, sintering: the graphite mold pre-pressed in step 3 is placed in a vacuum environment, and then loaded with a compressive stress of 40 MPa and sintered, first heated to 1000°C for 10 minutes and kept warm for 5 minutes, then continued to heat to 1750°C for 10 minutes and kept warm for 20 minutes, cooled to 150°C with the furnace and taken out, and the sintered body was obtained after demolding;
[0045] Step 6, grinding and polishing: Use 100 mesh and 400 mesh diamond grinding discs to roughly grind the outer side of the sintered body obtained in step 5 to remove the outer carbon paper, and then use metallographic sandpaper to grind and polish until the surface reaches a mirror effect, thereby obtaining a dual-element doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating, such as Figure 3 As shown; the outer layer single-side thickness of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating is 0.3mm, the inner layer thickness is 2.4mm, and the total thickness is 3mm.
[0046] Figure 4 This is a compressive strain-compressive stress curve of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating prepared in this embodiment. Figure 4 It can be seen that the compressive strength of the coating is as high as 810 MPa.
[0047] Figure 5 This is a test chart of the thermal insulation performance of the dual-doped gradient porous ultra-high temperature ceramic thermal insulation, pressure-resistant and wear-resistant coating prepared in this embodiment. The coating thickness is 3 mm. When the single-side coating is heated to 600°C (the heater is about 780°C), the back temperature is about 400°C, and the test time is 548700s. Then a K-type thermocouple is used to measure the temperature, and the insulation temperature is about 220°C, indicating that the coating has excellent thermal insulation performance.
[0048] Samples 1 to 4 were selected from the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating prepared in this embodiment, and the wear resistance of each sample was tested respectively: the test conditions were temperature 530°C, load 20MPa, stroke ±5mm, friction time 2h, and the grinding material was Q235 stainless steel. The results are shown in Table 1 below.
[0049] Table 1
[0050]
[0051] It can be seen from Table 1 that the wear amount of the unoxidized sample 1 at a frequency of 10 Hz is 1.8 mg, the wear amount of the sample 2 oxidized for 7 days at a frequency of 10 Hz is 2.4 mg, the wear amount of the unoxidized sample 3 at a frequency of 20 Hz is 14.0 mg, and the wear amount of the sample 4 oxidized for 7 days at a frequency of 20 Hz is 26.4 mg, indicating that the dual-doped gradient porous ultra-high temperature ceramic thermal insulation, pressure-resistant and wear-resistant coating prepared in this embodiment has excellent wear resistance.
[0052] The binary component system of the nano-scale binary doped ultra-high temperature ceramic powder in this embodiment can also be replaced by ZrO2-SiC, ZrB2-SiC, NbB2-SiC, NbC-SiC, HfB2-SiC, HfC-SiC, TaB2-SiC or TaC-SiC; the binary component system of the micron-scale binary doped ultra-high temperature ceramic powder can also be replaced by: ZrO2-SiC, ZrB2-SiC, NbB2-SiC, NbC-SiC, HfB2-SiC, HfC-SiC, TaB2-SiC or TaC-SiC.
[0053] Example 2
[0054] like Figure 1 As shown, this embodiment includes the following steps:
[0055] Step 1, powder selection: select nano-scale dual-element doped ultra-high temperature ceramic powder with a mass purity of 99.9% and a particle size of 30nm to 100nm as the outer layer powder, and select micron-scale dual-element doped ultra-high temperature ceramic powder with a mass purity of 99.9% and a particle size of 1μm to 5μm as the inner layer powder; the binary component system of the nano-scale dual-element doped ultra-high temperature ceramic powder is ZrB2-15% SiC by volume percentage, wherein the particle size of the ZrB2 powder is 100nm, and the particle size of the SiC powder is 30nm; the binary component system of the micron-scale dual-element doped ultra-high temperature ceramic powder is ZrB2-15% SiC by volume percentage, wherein the particle size of the ZrB2 powder is 5μm, and the particle size of the SiC powder is 2μm;
[0056] Step 2, powder preparation: according to the composition system of the outer layer powder and the inner layer powder selected in step 1, respectively select raw materials and use a powder mixer to mix them evenly for 24 hours and dry them at 150° C. for 24 hours to obtain outer layer powder and inner layer powder respectively;
[0057] Step 3: Fill with powder: Figure 2 As shown, a carbon paper with a thickness of 0.02 mm is laid on the inner side of the mold barrel of the graphite mold and the surface of the lower graphite pressure head, the outer layer powder obtained in step 2 is selected to be filled into the graphite mold, and the upper graphite pressure head is used to compact it, and then the inner layer powder obtained in step 2 is selected to be filled in the compacted outer layer powder in batches, and the upper graphite pressure head is used to compact it, and the outer layer powder obtained in step 2 is continuously selected to be filled in the compacted inner layer powder, and the upper graphite pressure head is used to compact it, and then the carbon paper is laid on the upper surface of the compacted outer layer powder of the upper layer and the upper graphite pressure head is placed, and the carbon felt is wrapped on the outer surface of the graphite mold to obtain a graphite mold filled with powder;
[0058] Step 4: Pre-pressing: pre-pressing the graphite mold filled with powder obtained in step 3 by applying a compressive stress of 20 MPa;
[0059] Step 5, sintering: the graphite mold pre-pressed in step 3 is placed in a vacuum environment, and then loaded with a compressive stress of 40 MPa and sintered, first heated to 1000°C for 10 minutes and kept warm for 5 minutes, then continued to heat to 1750°C for 10 minutes and kept warm for 20 minutes, cooled to 150°C with the furnace and taken out, and the sintered body was obtained after demolding;
[0060] Step 6, grinding and polishing: Use 100 mesh and 400 mesh diamond grinding discs to roughly grind the outer side of the sintered body obtained in step 5 to remove the outer carbon paper, and then use metallographic sandpaper to grind and polish until the surface reaches a mirror effect, thereby obtaining a dual-element doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating, such as Figure 6 As shown; the outer layer single-side thickness of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating is 0.68 mm, the inner layer thickness is 8.64 mm, and the total thickness is 10 mm.
[0061] Figure 7a to Figure 7c The scanning electron microscope images of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating and its outer and inner layers prepared in this embodiment are shown in FIG. Figure 7a to Figure 7c It can be seen that the coating is divided into inner and outer layers, and the grain size of the outer layer is smaller, while the grain size of the inner layer is larger.
[0062] Figure 8The relationship between the compressive strength and oxidation time of the dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating prepared in this embodiment is shown in the graph, wherein the experimental conditions for oxidation are oxidation for 0 days, 1 day, 7 days, 15 days and 30 days, room temperature or high temperature (530°C for 15 min), displacement loading, and a loading rate of 0.2 mm / min. Figure 8 It can be seen that with the increase of oxidation time, the compressive strength of the coating at room temperature increases parabolically, and with the increase of oxidation time, the compressive strength of the coating at high temperature changes little, indicating that the coating has high strength at both room temperature and high temperature and has excellent load-bearing properties.
[0063] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating, characterized in that: The method comprises the following steps: Step 1, powder selection: select nano-scale dual-element doped ultra-high temperature ceramic powder as the outer layer powder, and select micron-scale dual-element doped ultra-high temperature ceramic powder as the inner layer powder; the dual component system of the nano-scale dual-element doped ultra-high temperature ceramic powder is: ZrO2-SiC, ZrB2-SiC, ZrC-SiC, NbB2-SiC, NbC-SiC, HfB2-SiC, HfC-SiC, TaB2-SiC or TaC-SiC; the dual component system of the micron-scale dual-element doped ultra-high temperature ceramic powder is: ZrO2-SiC, ZrB2-SiC, ZrC-SiC, NbB2-SiC, NbC-SiC, HfB2-SiC, HfC-SiC, TaB2-SiC or TaC-SiC; the nano-scale dual-element doped ultra-high temperature ceramic powder has the same dual component system as the micron-scale dual-element doped ultra-high temperature ceramic powder; Step 2, powder preparation: according to the composition system of the outer layer powder and the inner layer powder selected in step 1, raw materials are selected respectively, mixed evenly by a powder mixer, and then dried to obtain the outer layer powder and the inner layer powder respectively; Step 3, filling powder: laying carbon paper on the inner side of the mold barrel of the graphite mold and the surface of the lower graphite press head, selecting the outer layer powder obtained in step 2 to fill in the graphite mold, and compacting it with the upper graphite press head, then selecting the inner layer powder obtained in step 2 to fill in the compacted outer layer powder in batches, and compacting it with the upper graphite press head, continuing to select the outer layer powder obtained in step 2 to fill in the compacted inner layer powder, and compacting it with the upper graphite press head, then laying carbon paper on the upper surface of the compacted outer layer powder of the upper layer and placing the upper graphite press head, and wrapping carbon felt on the outer surface of the graphite mold to obtain a graphite mold filled with powder; Step 4: Pre-pressing: pre-pressing the graphite mold filled with powder obtained in step 3 by applying a compressive stress of 10MPa to 30MPa; Step 5, sintering: placing the graphite mold pre-pressed in step 3 in a vacuum environment, then applying a compressive stress of 30MPa to 60MPa and sintering, and obtaining a sintered body after demolding; Step 6, grinding and polishing: Use a 60-400 mesh diamond grinding wheel to roughly grind the outer side of the sintered body obtained in step 5 to remove the outer carbon paper, and then use metallographic sandpaper to grind and polish until the surface reaches a mirror effect, thereby obtaining a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating.
2. The method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating according to claim 1, characterized in that: The mass purity of the nano-scale dual-element doped ultra-high temperature ceramic powder in step 1 is above 99%, and the particle size is 30nm~100nm; the mass purity of the micron-scale dual-element doped ultra-high temperature ceramic powder is above 99%, and the particle size is 1μm~5μm.
3. The method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating according to claim 1, characterized in that: The binary component systems of the nano-scale binary doped ultra-high temperature ceramic powder and the micron-scale binary doped ultra-high temperature ceramic powder in step 1 are both ZrC-SiC.
4. The method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating according to claim 1, characterized in that: The binary component system of the nano-scale binary doped ultra-high temperature ceramic powder and the micron-scale binary doped ultra-high temperature ceramic powder is ZrC-20%SiC, ZrC-15%SiC, ZrC-10%SiC or ZrC-5%SiC in terms of volume percentage.
5. The method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating according to claim 1, characterized in that: The mixing time in step 2 is 24 hours, and the drying temperature is 150° C. for 24 hours.
6. The method for preparing a dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating according to claim 1, characterized in that: The sintering process in step 5 is: firstly, heating to 1000°C for 10 minutes and keeping the temperature for 5 minutes, then heating to 1750°C for 10 minutes and keeping the temperature for 20 minutes, and then taking out after cooling to 150°C in the furnace.
7. A dual-doped gradient porous ultra-high temperature ceramic heat-insulating, pressure-resistant and wear-resistant coating prepared by the method according to any one of claims 1 to 6.