Anti-shedding pencil topcoat and preparation method thereof

By using epoxy resin, silicone microspheres modified layered sodium silicate and nanowood powder, the problem of easy peeling of pencil topcoat is solved, the effect of waterproof, adhesion and anti-falling is achieved, and the pencil is improved Safety and service life.

CN117264454BActive Publication Date: 2024-12-03ZHEJIANG ANYI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311373747.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-23
Publication Date
2024-12-03
Estimated Expiration
2043-10-23

AI Technical Summary

Technical Problem

The NC paint used in the production process of existing pencil topcoats has solvent volatility problems, which affects the environment and operator safety. It is easy to crack and peel off the topcoat due to friction and hand sweat oil stains during use, which affects the appearance and may cause accidental ingestion or stabbing.

Method used

Using epoxy resin E51, silicone microsphere modified layered sodium silicate, acrylic acid and other additives, it is used to combine γ-methacryloyloxypropyltrimethoxysilane and tetramethylammonium clathrate polybis Silicone polymerization microspheres were prepared by hydrolysis and polymerization of semisiloxane, and reacted with layered sodium silicate to form a modified layered sodium silicate, combining nanowood powder to form a rough structure, improving the waterproofness, adhesion and Anti-falling performance.

Benefits of technology

The pencil topcoat has been realized, with strong adhesion and anti-falling effects, reducing the hydrophobicity and cracking risks of topcoat, and improving safety and service life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an anti-shedding pencil topcoat and a preparation method thereof, and relates to the field of pencil coatings. The invention firstly utilizes γ-methacryloxypropyltrimethoxysilane and tetramethylammonium cage-shaped polysilsesquioxane to hydrolyze and condense into micrometer-level organosilicon microspheres, which are loaded on the surface of layered sodium silicate and form a micro-nano rough structure with nano-wood powder to improve the waterproof effect of the topcoat, and then, the topcoat is made with epoxy resin, acrylic acid, etc., which has good adhesion to pencil wood, and before the topcoat is sprayed, the pencil wood is first subjected to amino treatment to enhance the adhesion between the pencil and the topcoat, and after spraying, ultraviolet light is used for curing to polymerize the microspheres, acrylic acid, etc. to form a polypropylene structure, and further enhance the waterproofness of the pencil topcoat.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pencil coatings, in particular to an anti-shedding pencil topcoat and a preparation method thereof. Background Art

[0002] Pencils are used a lot as daily stationery for students. While we pay attention to the healthy growth of children's body and mind, we should also provide children with a safe environment from the outside. As the thing that children touch most in daily life, the safety of pencils is worthy of every parent's attention.

[0003] In addition to the lead core, the outer layer of the pencil should also be taken seriously. Among them, the decorative coating currently mainly uses NC coating, which has the advantages of good decorative effect, simple construction and quick drying. However, NC coating has obvious problems in terms of safety: 1. A large amount of solvents are volatilized during the production process, and these solvents include esters, ketones, alcohol ethers, etc., which are harmful to the environment and operators; 2. Safety during customer use: Children are the main consumer of pencils, their physical development is not yet complete, and they have the habit of "holding in the mouth", which increases the safety requirements. At the same time, the topcoat of the pencil is prone to cracking and peeling due to long-term holding friction and erosion by hand sweat and oil stains. The peeling of the outer layer of the pencil not only affects the beauty of the pencil, but also may cause students to accidentally eat the topcoat. After the topcoat is peeled off, the pencil is exposed as wood, and there is also the risk of wood thorns piercing students' fingers. The present invention innovates an anti-shedding pencil topcoat and a preparation method thereof, aiming to solve the above problems. Summary of the invention

[0004] The invention aims to provide an anti-shedding pencil topcoat and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: an anti-shedding pencil topcoat, which comprises epoxy resin E51, organic silicon microsphere modified layered sodium silicate, acrylic acid, and other additives.

[0006] Furthermore, the organosilicon microsphere modified layered sodium silicate is prepared by hydrolyzing and polymerizing γ-methacryloxypropyltrimethoxysilane and tetramethylammonium cage-shaped polysilsesquioxane to obtain organosilicon polymer microspheres, which are then reacted with layered sodium silicate.

[0007] Further, a method for preparing an anti-shedding pencil topcoat comprises the following preparation steps:

[0008] (1) 1-3 parts of γ-methacryloxypropyltrimethoxysilane and 1-3 parts of tetramethylammonium cage-shaped polysilsesquioxane are mixed with 10 parts of deionized water, hydrochloric acid is added to a pH value of 4-6, and the mixture is reacted at 25° C. for 5 hours, and then ammonia water is added to a solution pH of 6-11, and then the temperature is raised to 30° C., and the reaction is continued for 3 hours, filtered, washed, and dried at 150° C. for 10 hours to obtain silicone polymer microspheres with a particle size of 1-15 μm;

[0009] (2) 30-40 parts of deionized water and 10-20 parts of layered silicate were stirred at 500-600 r / min for 2-3 minutes, then placed in a constant temperature water bath at 80° C., stirred at 500-600 r / min for 30 minutes, and 5-10 parts of an organosilicon microsphere solution were added, wherein the mass ratio of organosilicon polymer microspheres to deionized water in the organosilicon microsphere solution was 1:10-2:10, reacted at 80° C. for 3 hours, allowed to stand for 12 hours, filtered, the solid was taken, washed 2-4 times, and dried at a vacuum degree of -0.098 MPa and 70° C. for 5 hours to obtain organosilicon microsphere modified layered sodium silicate;

[0010] (3) Add 30 parts of acrylic acid to 10-100 parts of weak alkaline aqueous solution, stir at 2000-3000 r / min for 10-60 min, add 5-10 parts of organosilicon microsphere modified layered sodium silicate, 1-2 parts of photoinitiator, 0.1-0.5 parts of defoamer, 5-10 parts of wood powder with a particle size of 100-300 nm, continue stirring for 20-40 min, add 30 parts of epoxy resin E51, continue stirring for 1-2 h, and obtain an anti-shedding pencil topcoat.

[0011] Furthermore, the washing in step (1) is to wash the filtered solid with deionized water and ethanol three times respectively.

[0012] Furthermore, the washing in step (2) is performed using 80° C. hot deionized water.

[0013] Furthermore, the weak alkaline solution in step (3) is prepared by adding lysine to deionized water until the pH of the solution is 7-9.

[0014] Furthermore, the photoinitiator in step (3) is dialkoxyacetophenone.

[0015] Furthermore, the defoaming agent in step (3) is a mixture of one or more of tributyl phosphate, emulsified silicone oil, polyoxypropylene glycerol ether or ether defoaming agents.

[0016] Further, a method for spraying using the anti-shedding pencil topcoat comprises the following steps:

[0017] a. Prepare an ethanol aqueous solution with a concentration of 95% using anhydrous ethanol and ultrapure water, then add N1-[(4-vinylphenylmethyl]-N2-3-(triethoxysilyl)propyl]-1,2-ethylenediamine to a mass fraction of 2%-8%, and mix ultrasonically at 20kHz for 1h to prepare a siloxane coupling agent solution; at room temperature, spray the siloxane coupling agent solution on the surface of the pencil, place it in an oven at 103°C, and dry it to constant weight to obtain a pre-modified pencil;

[0018] b. Spray the anti-shedding pencil topcoat evenly on the pre-modified pencil with a thickness of 100 μm and use a 700W high-pressure mercury lamp with an illumination of 1.1 mW / cm 2 Curing for 60-100 seconds.

[0019] Furthermore, the spraying in step a is repeated 3 times, each spraying amount is 0.3-0.5 mL / min, and the spraying time is 8-15 min.

[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0021] The invention utilizes N1-[(4-vinylphenylmethyl]-N2-3-(triethoxysilyl)propyl]-1,2-ethylenediamine and layered sodium silicate for modification, polymerizes organic silicon microspheres and acrylic acid light curing, and nano-wood powder to form a rough structure to achieve waterproof, strong adhesion, and anti-shedding effects.

[0022] Firstly, the invention uses N1-[(4-vinylphenylmethyl]-N2-3-(triethoxysilyl)propyl]-1,2-ethylenediamine to perform amino treatment on pencil wood, so that the surface of the pencil raw material wood is rich in a large number of amino groups and is weakly alkaline, which is bonded with the carboxyl group in the epoxy resin to form a double bond that is not easy to break. The formed double bond is bonded with acrylic acid, so that the cohesion of the coating is further improved and it is not easy to crack and fall off. Furthermore, layered sodium silicate is used as a structural frame, which can not only form a physical filling effect in the pores of the pencil wood, but also chemically react with the alcohol hydroxyl group on the surface of the wood to form a silicon-oxygen bond. At the same time, the silicate is bonded with the active group in the epoxy resin E51, and serves as a linker to improve the adhesion between the coating and the pencil wood.

[0023] Secondly, γ-methacryloxypropyltrimethoxysilane and tetramethylammonium cage-shaped polysilsesquioxane are hydrolyzed and condensed to polymerize into micron-sized silicone microspheres, which can reduce the surface energy and improve the hydrophobicity of the topcoat, so that the pencil is not easily penetrated by sweat or other moisture to cause cracking and falling off when used; at the same time, nano-scale wood powder and silicone microspheres are used to form a micro-nano rough structure, so that the hydrophobicity of the coating surface is further improved, thereby improving the anti-falling performance of the topcoat; and during the curing process, γ-methacryloxypropyltrimethoxysilane and acrylic Acid and N1-[(4-vinylphenylmethyl]-N2-3-(triethoxysilyl)propyl]-1,2-ethylenediamine are bonded to form a polypropylene structure with a hydrophobic long carbon chain, which improves the waterproof performance of the topcoat; at the same time, acrylic acid reacts and grafts with the epoxy group contained in the epoxy resin to enhance the adhesion of the coating and achieve an anti-shedding effect; in addition, the ammonium group in the tetramethylammonium cage-shaped polysilsesquioxane is ion-exchanged with the sodium ion in the layered sodium silicate to modify it, so that the silicone microspheres are strongly combined with the layered silicate, thereby improving the anti-shedding performance of the coating. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0025] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of an anti-shedding pencil topcoat prepared in the following examples are as follows:

[0026] Peel resistance: Refer to GB / T 9286, use a grid knife to cut the coating surface into a grid pattern perpendicular to each other, with a scratch width of 2mm; stick 3M tape tightly to the grid pattern surface, peel it off at 180° and observe the peeling of the coating grid.

[0027] Hydrophobicity: The topcoat is based on the sessile drop test technique and the contact angle of the drop is measured using a surface contact angle meter.

[0028] Example 1

[0029] (1) Mix 1 part of γ-methacryloxypropyltrimethoxysilane and 1 part of tetramethylammonium cage-shaped polysilsesquioxane with 10 parts of deionized water, add hydrochloric acid to a pH value of 4, react at 25° C. for 5 hours, add ammonia water to a solution pH of 6, then heat to 30° C., continue to react for 3 hours, filter, take the solid, wash it with deionized water and ethanol three times respectively, and dry it at 150° C. for 10 hours to obtain silicone polymer microspheres with a particle size of 1 μm;

[0030] (2) 30 parts of deionized water and 10 parts of layered silicate were stirred at 500 r / min for 2 min, then placed in a constant temperature water bath at 80°C and stirred at 500 r / min for 30 min, 5 parts of an organosilicon microsphere solution were added, the mass ratio of organosilicon polymer microspheres to deionized water in the organosilicon microsphere solution was 1:10, reacted at 80°C for 3 h, allowed to stand for 12 h, filtered, the solid was taken, washed twice with 80°C hot deionized water, and dried at a vacuum degree of -0.098 MPa and 70°C for 5 h to obtain organosilicon microsphere modified layered sodium silicate;

[0031] (3) adding lysine to deionized water until the pH of the solution is 7 to prepare a weak alkaline aqueous solution; adding 30 parts of acrylic acid to 10 parts of the weak alkaline aqueous solution, stirring at 2000 r / min for 10 minutes, adding 5 parts of organosilicon microsphere modified layered sodium silicate, 1 part of dialkoxyacetophenone photoinitiator, 0.1 part of tributyl phosphate defoamer, and 5 parts of wood powder with a particle size of 100 nm, continuing to stir for 20 minutes, adding 30 parts of epoxy resin E51, and continuing to stir for 1 hour to obtain an anti-shedding pencil topcoat;

[0032] (4) using anhydrous ethanol and ultrapure water to prepare an ethanol aqueous solution with a concentration of 95%, and then adding N1-[(4-vinylphenylmethyl]-N2-3-(triethoxysilyl)propyl]-1,2-ethylenediamine to a mass fraction of 2%, and ultrasonically mixing at 20kHz for 1h to prepare a siloxane coupling agent solution; at room temperature, spraying the siloxane coupling agent solution on the surface of the pencil, repeatedly spraying 3 times, each spraying amount is 0.3mL / min, the spraying time is 8min, and the pencil is placed in an oven at 103°C and dried to constant weight to obtain a pre-modified pencil;

[0033] (5) Spray the anti-shedding pencil topcoat evenly on the pre-modified pencil with a thickness of 100 μm and use a 700W high-pressure mercury lamp with an illumination of 1.1 mW / cm 2 Curing for 60 seconds.

[0034] Example 2

[0035] (1) 2 parts of γ-methacryloxypropyltrimethoxysilane and 2 parts of tetramethylammonium cage-shaped polysilsesquioxane were mixed with 10 parts of deionized water, and hydrochloric acid was added to a pH value of 5. After reacting at 25° C. for 5 hours, ammonia water was added until the solution pH was 8.5, and then the temperature was raised to 30° C., and the reaction was continued for 3 hours. The solid was filtered, and the solid was taken, washed with deionized water and ethanol for 3 times respectively, and dried at 150° C. for 10 hours to obtain silicone polymer microspheres with a particle size of 8 μm;

[0036] (2) 35 parts of deionized water and 15 parts of layered silicate were stirred at 550 r / min for 2.5 min, then placed in a constant temperature water bath at 80° C., stirred at 550 r / min for 30 min, and 7.5 parts of an organosilicon microsphere solution was added, wherein the mass ratio of organosilicon polymer microspheres to deionized water in the organosilicon microsphere solution was 1.5:10. After reacting at 80° C. for 3 h, the mixture was allowed to stand for 12 h, filtered, and the solid was taken out. The solid was washed three times with hot deionized water at 80° C., and dried at a vacuum degree of -0.098 MPa and 70° C. for 5 h to obtain organosilicon microsphere-modified layered sodium silicate;

[0037] (3) adding lysine to deionized water until the pH of the solution is 8 to prepare a weak alkaline aqueous solution; adding 30 parts of acrylic acid to 55 parts of the weak alkaline aqueous solution, stirring at 2500 r / min for 35 minutes, adding 7.5 parts of organosilicon microsphere modified layered sodium silicate, 1.5 parts of dialkoxyacetophenone photoinitiator, 0.3 parts of emulsified silicone oil defoamer, and 7.5 parts of wood powder with a particle size of 200 nm, continuing to stir for 30 minutes, adding 30 parts of epoxy resin E51, and continuing to stir for 1.5 hours to obtain an anti-shedding pencil topcoat;

[0038] (4) using anhydrous ethanol and ultrapure water to prepare an ethanol aqueous solution with a concentration of 95%, and then adding N1-[(4-vinylphenylmethyl]-N2-3-(triethoxysilyl)propyl]-1,2-ethylenediamine to a mass fraction of 5%, and ultrasonically mixing at 20kHz for 1h to prepare a siloxane coupling agent solution; at room temperature, spraying the siloxane coupling agent solution on the surface of the pencil, repeatedly spraying 3 times, each spraying amount is 0.4mL / min, the spraying time is 10min, and the pencil is placed in an oven at 103°C and dried to constant weight to obtain a pre-modified pencil;

[0039] (5) Spray the anti-shedding pencil topcoat evenly on the pre-modified pencil with a thickness of 100 μm and use a 700W high-pressure mercury lamp with an illumination of 1.1 mW / cm 2 Curing for 80 seconds.

[0040] Example 3

[0041] (1) 3 parts of γ-methacryloxypropyltrimethoxysilane and 3 parts of tetramethylammonium cage-shaped polysilsesquioxane were mixed with 10 parts of deionized water, hydrochloric acid was added to a pH value of 6, and the mixture was reacted at 25° C. for 5 h, and then ammonia water was added to a solution pH of 11, and then the temperature was raised to 30° C. and the reaction was continued for 3 h. The solid was filtered and washed with deionized water and ethanol for 3 times respectively, and dried at 150° C. for 10 h to obtain organosilicon polymer microspheres with a particle size of 15 μm;

[0042] (2) 40 parts of deionized water and 20 parts of layered silicate were stirred at 600 r / min for 3 min, then placed in a constant temperature water bath at 80°C and stirred at 600 r / min for 30 min, 10 parts of an organosilicon microsphere solution were added, the mass ratio of organosilicon polymer microspheres to deionized water in the organosilicon microsphere solution was 2:10, reacted at 80°C for 3 h, allowed to stand for 12 h, filtered, the solid was taken, washed 4 times with 80°C hot deionized water, and dried at a vacuum degree of -0.098 MPa and 70°C for 5 h to obtain organosilicon microsphere modified layered sodium silicate;

[0043] (3) adding lysine to deionized water until the pH of the solution is 9 to prepare a weak alkaline aqueous solution; adding 30 parts of acrylic acid to 100 parts of the weak alkaline aqueous solution, stirring at 3000 r / min for 60 minutes, adding 10 parts of organosilicon microsphere modified layered sodium silicate, 2 parts of dialkoxyacetophenone photoinitiator, 0.5 parts of polyoxypropylene glycerol ether defoamer, and 10 parts of wood powder with a particle size of 300 nm, continuing to stir for 40 minutes, adding 30 parts of epoxy resin E51, and continuing to stir for 2 hours to obtain an anti-shedding pencil topcoat;

[0044] (4) using anhydrous ethanol and ultrapure water to prepare an ethanol aqueous solution with a concentration of 95%, and then adding N1-[(4-vinylphenylmethyl]-N2-3-(triethoxysilyl)propyl]-1,2-ethylenediamine to a mass fraction of 8%, and ultrasonically mixing at 20kHz for 1h to prepare a siloxane coupling agent solution; spraying the siloxane coupling agent solution on the surface of the pencil at room temperature, repeatedly spraying 3 times, each spraying amount is 0.5mL / min, the spraying time is 15min, and the pencil is placed in an oven at 103°C and dried to constant weight to obtain a pre-modified pencil;

[0045] (5) Spray the anti-shedding pencil topcoat evenly on the pre-modified pencil with a thickness of 100 μm and use a 700W high-pressure mercury lamp with an illumination of 1.1 mW / cm 2 Curing for 100 seconds.

[0046] Comparative Example 1

[0047] The difference between Comparative Example 1 and Example 2 is that there is no step (1), and step (2) is changed to: 35 parts of deionized water and 15 parts of layered silicate are stirred at 550 r / min for 2.5 min, then placed in a constant temperature water bath at 80°C, stirred at 550 r / min for 30 min, 7.5 parts of tetramethylammonium cage-shaped polysilsesquioxane solution are added, the mass ratio of tetramethylammonium cage-shaped polysilsesquioxane to deionized water in the tetramethylammonium cage-shaped polysilsesquioxane solution is 1.5:10, react at 80°C for 3 h, stand for 12 h, filter, take the solid, wash it with 80°C hot deionized water for 3 times, and dry it at a vacuum degree of -0.098 MPa and 70°C for 5 h to obtain coupling agent modified layered sodium silicate; the remaining steps are the same as those in Example 2.

[0048] Comparative Example 2

[0049] The difference between Comparative Example 2 and Example 2 is that there is no step (2), and step (3) is changed to: add lysine to deionized water until the solution pH is 8 to prepare a weak alkaline aqueous solution; add 30 parts of acrylic acid to 55 parts of the weak alkaline aqueous solution, stir at 2500r / min for 35min, add 7.5 parts of organosilicon polymer microspheres, 1.5 parts of dialkoxyacetophenone photoinitiator, 0.3 parts of emulsified silicone oil defoamer, 7.5 parts of wood powder with a particle size of 200nm, continue to stir for 30min, add 30 parts of epoxy resin E51, continue to stir for 1.5h, and obtain an anti-shedding pencil topcoat. The remaining steps are the same as Example 2.

[0050] Comparative Example 3

[0051] The difference between Comparative Example 3 and Example 2 is that there is no step (4), and step (5) is changed to: spray the anti-shedding pencil topcoat evenly on the pre-modified pencil with a thickness of 100 μm, and use a 700W high-pressure mercury lamp with an illumination of 1.1 mW / cm 2 The remaining steps are the same as those in Example 2.

[0052] Comparative Example 4

[0053] The difference between Comparative Example 4 and Example 2 is that step (5) is different, and step (5) is changed to: spray the coating uniformly on the sodium silicate modified wood to a thickness of 100 μm and cure at room temperature for 10 minutes. The remaining steps are the same as in Example 2.

[0054] Effect example

[0055] Table 1 below shows the performance analysis results of the anti-shedding pencil topcoats of Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.

[0056] Table 1

[0057] Peel resistance (peeling times) Hydrophobicity (contact angle / °) Example 1 161 151.20 Example 2 165 156.22 Example 3 158 153.54 Comparative Example 1 146 123.85 Comparative Example 2 116 137.59 Comparative Example 3 125 142.32 Comparative Example 4 136 132.47

[0058] From the comparison of the experimental data of the anti-shedding property of the embodiment and the comparative example, it can be found that after the pencil wood is aminated by N1-[(4-vinylphenylmethyl]-N2-3-(triethoxysilyl)propyl]-1,2-ethylenediamine, the pencil can be bonded with the topcoat, further improving the cohesion of the coating and not easy to crack and fall off; further, the layered sodium silicate is used as the structural frame and modified by organic silicon microspheres as the frame linker to further enhance the anti-shedding property of the coating; from the comparison of the experimental data of the hydrophobicity of the embodiment and the comparative example, it can be found that It is now found that the silicone microspheres formed by γ-methacryloxypropyltrimethoxysilane and tetramethylammonium cage-shaped polysilsesquioxane can reduce surface energy and improve the hydrophobicity of the topcoat, making it less likely for the pencil to be cracked and fall off due to the penetration of sweat or other moisture when it is used; at the same time, the surface of the loaded layered sodium silicate forms a micro-nano rough structure with nano-level wood powder, which further improves the hydrophobicity of the coating surface; and after the topcoat is cured, a long-chain polypropylene structure is formed, which further improves the waterproof performance of the topcoat, thereby achieving an anti-falling effect.

[0059] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. An anti-shedding pencil topcoat, characterized in that: The anti-shedding pencil topcoat comprises epoxy resin E51, organic silicon microsphere modified layered sodium silicate, acrylic acid, and other additives; the organic silicon microsphere modified layered sodium silicate is obtained by hydrolyzing and polymerizing γ-methacryloxypropyltrimethoxysilane and tetramethylammonium cage-shaped polysilsesquioxane to obtain organic silicon polymer microspheres, which are then reacted with layered sodium silicate; The method comprises the following preparation steps: (1) 1-3 parts of γ-methacryloxypropyltrimethoxysilane and 1-3 parts of tetramethylammonium cage-shaped polysilsesquioxane are mixed with 10 parts of deionized water, hydrochloric acid is added to a pH value of 4-6, and the mixture is reacted at 25° C. for 5 hours, and then ammonia water is added to a solution pH of 6-11, and then the temperature is raised to 30° C., and the reaction is continued for 3 hours, filtered, washed, and dried at 150° C. for 10 hours to obtain silicone polymer microspheres with a particle size of 1-15 μm; (2) 30-40 parts of deionized water and 10-20 parts of layered silicate were stirred at 500-600 r / min for 2-3 minutes, then placed in a constant temperature water bath at 80° C., stirred at 500-600 r / min for 30 minutes, 5-10 parts of an organosilicon microsphere solution were added, the mass ratio of organosilicon polymer microspheres to deionized water in the organosilicon microsphere solution was 1:10-2:10, reacted at 80° C. for 3 hours, allowed to stand for 12 hours, filtered, the solid was taken, washed with 80° C. hot deionized water for 2-4 times, and dried at a vacuum degree of -0.098 MPa and 70° C. for 5 hours to obtain organosilicon microsphere modified layered sodium silicate; (3) adding lysine to deionized water until the pH value of the solution is 7-9 to prepare a weak alkaline solution; then adding 30 parts of acrylic acid to 10-100 parts of the weak alkaline aqueous solution, stirring at 2000-3000 r / min for 10-60 min, adding 5-10 parts of organosilicon microsphere modified layered sodium silicate, 1-2 parts of photoinitiator, 0.1-0.5 parts of defoamer, 5-10 parts of wood powder with a particle size of 100-300 nm, continuing to stir for 20-40 min, adding 30 parts of epoxy resin E51, continuing to stir for 1-2 h, and obtaining an anti-shedding pencil topcoat; The spraying method of the anti-shedding pencil topcoat comprises the following steps: a. Prepare an ethanol aqueous solution with a concentration of 95% using anhydrous ethanol and ultrapure water, then add N1-[(4-vinylphenylmethyl]-N2-3-(triethoxysilyl)propyl]-1,2-ethylenediamine to a mass fraction of 2%-8%, and mix ultrasonically at 20kHz for 1h to prepare a siloxane coupling agent solution; at room temperature, spray the siloxane coupling agent solution on the surface of the pencil, place it in an oven at 103°C, and dry it to constant weight to obtain a pre-modified pencil; b. Spray the anti-shedding pencil topcoat evenly on the pre-modified pencil with a thickness of 100 μm, and cure it for 60-100 seconds using a 700W high-pressure mercury lamp with an illumination of 1.1 mW / cm.

2. The anti-shedding pencil topcoat according to claim 1, characterized in that: The washing in step (1) is to wash the filtered solid with deionized water and ethanol three times respectively.

3. The anti-shedding pencil topcoat according to claim 1, characterized in that: The photoinitiator described in step (3) is dialkoxyacetophenone.

4. The anti-shedding pencil topcoat according to claim 1, characterized in that: The defoaming agent in step (3) is a mixture of one or more of tributyl phosphate, emulsified silicone oil, polyoxypropylene glycerol ether or ether defoaming agents.

5. The anti-shedding pencil topcoat according to claim 1, characterized in that: The spraying in step a is repeated 3 times, each spraying amount is 0.3-0.5 mL / min, and the spraying time is 8-15 min.