Additive for blast furnace coal injection, preparation method and use thereof
Additives prepared from limestone and waste lithium iron phosphate battery cathode materials solve the problems of high ignition point and insufficient combustion of pulverized coal in blast furnace coal injection, improve combustion efficiency and reuse resources, reduce nitrogen oxide emissions, and avoid Coke dissolution and furnace lining corrosion have reached low emission standards.
Patent Information
- Application Number
- CN202311265197.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-27
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-09-27
AI Technical Summary
In blast furnace coal injection technology, pulverized coal has a high ignition point and insufficient combustion. The existing combustion-supporting additives have problems such as coke loss caused by alkali metal oxides, furnace lining corrosion, high cost of rare earth oxides, chlorine salt and nitrate corrosion, and decommissioned iron phosphate Insufficient utilization of lithium battery resources leads to environmental pollution and resource waste.
Limestone and waste lithium iron phosphate battery cathode materials are used to prepare additives for coal injection in blast furnaces. After grinding and mixing evenly, they are combined with pulverized coal to reduce the ignition point and burnout temperature of pulverized coal, improve combustion efficiency, and realize resource reuse.
It can effectively reduce the ignition point and burnout temperature of pulverized coal, increase the combustion rate, reduce nitrogen oxide emissions, avoid coke dissolution and furnace lining corrosion, and achieve efficient resource utilization and low emission standards.
Smart Images

Figure CN117265194B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an additive, in particular to an additive for blast furnace coal injection, belonging to the technical field of blast furnace coal powder injection. Background Art
[0002] Pulverized coal injection in blast furnaces is to directly inject finely ground anthracite or bituminous coal or a mixture of the two into the furnace from the tuyere of the blast furnace to replace coke to provide heat and reduce the coke ratio and reduce the cost of pig iron. Pulverized coal injection technology in blast furnaces is an effective technical means to reduce the amount of coke used in blast furnace ironmaking, reduce ironmaking production costs, and reduce environmental pollution. Since the residence time of pulverized coal in the tuyere combustion zone is extremely short, the unburned pulverized coal gradually increases with the increase in the amount of coal injection, resulting in enrichment, causing airflow blockage and poor slag fluidity, which is not conducive to stable production of the blast furnace. Therefore, improving the combustion efficiency and promoting the rapid combustion of pulverized coal in the tuyere area of the blast furnace is the key to achieving efficient injection, and adding combustion aids to pulverized coal is one of the effective methods to improve the combustion effect of pulverized coal and increase the efficiency of coal injection.
[0003] At present, there are still some shortcomings in the combustion-supporting additives for blast furnace coal injection. For example, the addition of alkali metal oxides or alkali metal salts will cause the alkali metal to circulate and accumulate in the blast furnace, causing problems such as coke dissolution, furnace lining corrosion, and furnace nodules. Although potassium permanganate (KMnO4) has a good combustion-supporting effect, its decomposition temperature (248°C) is relatively low, posing a safety hazard to powder making. Rare earth oxides are scarce resources with high usage costs and are difficult to promote and apply. Chloride salts, nitrates, etc. are corrosive to blast furnace equipment and gas pipelines, which will lead to poor furnace conditions.
[0004] With the rapid development of new energy vehicles, microelectronic devices and energy storage, lithium iron phosphate batteries have been widely used. However, with the promotion of electric vehicles for many years, the retirement peak will come, and it is estimated that 1.6 million tons of lithium iron phosphate will be retired in 2030. If retired lithium iron phosphate batteries are not properly disposed of, it will cause environmental pollution and waste of resources. Lithium iron phosphate batteries are rich in Al, Fe and P, and have a low content of precious metals, so the economic value of their recycling is not high. However, due to the continuous accumulation of scrapped batteries and the severity of environmental and resource problems, it is also urgent to find another way to develop harmless treatment and resource recycling solutions for waste lithium iron phosphate batteries. Summary of the invention
[0005] In view of the technical problems such as high ignition point and incomplete combustion of coal powder in the blast furnace coal injection technology in the prior art, the present invention proposes to combine the blast furnace coal powder injection technology with the recycling and reuse of waste lithium iron phosphate batteries, and use waste lithium iron phosphate battery positive electrode materials to replace previously reported alkali metal oxides, alkali metal salts, potassium permanganate, rare earth oxides, chloride salts, nitrates and other additives, and use limestone and lithium iron phosphate battery positive electrode materials as raw materials to prepare additives, which are used in blast furnace coal injection, thereby achieving the purpose of lowering the ignition point of coal powder, improving the combustion efficiency of blast furnace coal powder injection and resource reuse of retired lithium iron phosphate batteries.
[0006] The first purpose of the present invention is to provide a combustion-supporting additive for blast furnace coal injection, which has easy-to-obtain raw materials, does not contain alkali metals, has a stable combustion-supporting effect, and can effectively improve economic benefits.
[0007] The second object of the present invention is to provide a method for preparing the additive for achieving the first object.
[0008] The third object of the present invention is to provide a method for using the additive for blast furnace coal injection to achieve the first object.
[0009] According to a first embodiment provided by the present invention, an additive for blast furnace coal injection is provided.
[0010] An additive for blast furnace coal injection, the additive comprising: in weight percentage,
[0011] Limestone 60% to 80%, preferably 65% to 75%, more preferably 68% to 72%, further preferably 69% to 71%, for example 70%.
[0012] The positive electrode material of lithium iron phosphate battery is 20% to 40%, preferably 25% to 35%, more preferably 28% to 32%; further preferably 29% to 31%; for example 30%.
[0013] Preferably, the positive electrode material of the lithium iron phosphate battery is a waste positive electrode material of the lithium iron phosphate battery.
[0014] In the present invention, the content of CaCO3 in the limestone is greater than 95wt%, the content of SiO2 is not greater than 1.5wt%, the content of MgO is not greater than 3wt%, and the content of S is not greater than 0.025wt%.
[0015] In the present invention, the composition of the positive electrode material of the lithium iron phosphate battery is: 68-76wt% Al, 22-28wt% LiFePO4, and the balance is a conductive agent and a binder. Generally, the conductive agent is acetylene black, carbon nanotubes, etc. The binder is PVDF, PAA, PMMA, PTFE, etc.
[0016] According to a second embodiment provided by the present invention, a method for preparing an additive for blast furnace coal injection is provided.
[0017] A method for preparing an additive for blast furnace coal injection, the method comprising the following steps: grinding limestone and lithium iron phosphate battery positive electrode material, and mixing them evenly after grinding to obtain the additive for blast furnace coal injection.
[0018] In the present invention, limestone and lithium iron phosphate battery positive electrode material can be ground separately, and then the ground limestone powder and lithium iron phosphate battery positive electrode material powder are mixed evenly; limestone and lithium iron phosphate battery positive electrode material can also be mixed and then ground together.
[0019] In the present invention, the limestone is ground to a particle size of less than 5 mm; and the positive electrode material of the lithium iron phosphate battery is ground to a particle size of less than 10 mm.
[0020] In the present invention, among the additives for blast furnace coal injection obtained by uniform mixing, the proportion of particles with a particle size of less than 0.074 mm is greater than 70%.
[0021] Preferably, the positive electrode material of the lithium iron phosphate battery is a waste lithium iron phosphate battery positive electrode material. The waste lithium iron phosphate battery positive electrode material comes from recycled waste lithium iron phosphate batteries. The waste lithium iron phosphate battery is pretreated to obtain the waste lithium iron phosphate battery positive electrode material. The pretreatment is specifically: disassembling, physically crushing and separating the waste lithium iron phosphate battery to obtain the waste lithium iron phosphate positive electrode material.
[0022] In the present invention, the additive comprises: by weight percentage,
[0023] Limestone 60% to 80%, preferably 65% to 75%, more preferably 68% to 72%, further preferably 69% to 71%, for example 70%.
[0024] The positive electrode material of lithium iron phosphate battery is 20% to 40%, preferably 25% to 35%, more preferably 28% to 32%; further preferably 29% to 31%; for example 30%.
[0025] In the present invention, the content of CaCO3 in the limestone is greater than 95wt%, the content of SiO2 is not greater than 1.5wt%, the content of MgO is not greater than 3wt%, and the content of S is not greater than 0.025wt%.
[0026] In the present invention, the composition of the positive electrode material of the lithium iron phosphate battery is: 68-76wt% Al, 22-28wt% LiFePO4, and the balance is a conductive agent and a binder. Generally, the conductive agent is acetylene black, carbon nanotubes, etc. The binder is PVDF, PAA, PMMA, PTFE, etc.
[0027] According to a third embodiment provided by the present invention, there is provided a use of an additive for blast furnace coal injection.
[0028] A use of an additive for blast furnace coal injection, wherein the additive for blast furnace coal injection according to the first embodiment or the additive for blast furnace coal injection prepared by the preparation method described in the second embodiment is mixed with raw coal and used for blast furnace injection.
[0029] In the present invention, the additive is mixed with coal powder, dried, crushed, and then injected into the blast furnace.
[0030] Preferably, the amount of the additive is 1 to 6 wt % of the coal powder, preferably 2 to 5 wt %.
[0031] A mixed coal powder for blast furnace injection comprises coal powder and additives, wherein the amount of the additive is 1-6wt% of the mass of the coal powder, preferably 2-5wt%.
[0032] The additives include: by weight percentage,
[0033] Limestone 60% to 80%, preferably 65% to 75%, more preferably 68% to 72%, further preferably 69% to 71%, for example 70%.
[0034] The positive electrode material of lithium iron phosphate battery is 20% to 40%, preferably 25% to 35%, more preferably 28% to 32%; further preferably 29% to 31%; for example 30%.
[0035] In response to the technical problems of high ignition point and incomplete combustion of pulverized coal in the existing blast furnace coal injection technology, the inventors conducted experiments on adding alkali metals and potassium permanganate to pulverized coal. By selecting different materials, they unexpectedly found that the additive obtained by mixing limestone and lithium iron phosphate battery positive electrode material has a significant improvement effect on blast furnace pulverized coal injection, which can significantly reduce the ignition point temperature and burnout temperature of pulverized coal, shorten the relative combustion time of pulverized coal, and improve the combustion rate.
[0036] The present invention creatively uses limestone and waste lithium iron phosphate battery positive electrode materials as blast furnace coal injection combustion aids, which are mixed with raw coal and pulverized before being sprayed into the blast furnace for combustion, thereby improving the combustion efficiency and promoting rapid combustion of coal powder in the tuyere area of the blast furnace, thereby achieving the effect of improving the combustion effect of coal powder and increasing the replacement of coal injection (solid fuel in the material). In addition, the inventors further discovered that the use of the additive provided by the present invention can promote the combustion of coal powder while effectively reducing the generation of thermal nitrogen oxides caused by coal powder combustion, thereby reducing the content of nitrogen oxides in the flue gas discharged from the blast furnace.
[0037] In the present invention, the cathode material of waste lithium iron phosphate battery mainly includes 1-2wt% binder (such as PVDF / PAA / PMMA / PTFE), 1-2wt% conductive agent (such as acetylene black, carbon nanotubes, etc.), 22-28wt% LiFePO4 and 68-76wt% Al (aluminum foil). The binders are all high molecular hydrocarbons, which will produce high thermal energy and chemical energy after combustion, and will also produce a large amount of small molecular gas, which will further increase the volume of coal gas and increase the kinetic energy of blast. The conductive agents are all carbon materials, and the introduction of carbon can replace part of anthracite and improve the combustion characteristics of coal powder. LiFePO4 has good thermal stability, and its crystal structure is stable below 300°C. From above 400°C, it begins to decompose as the temperature rises, generating FePO4, Li2O and O2. FePO4 produces H3PO4 and Fe2O3 through combustion in a blast furnace. These metal oxides (Fe2O3 and Li2O) play a vital role in the oxygen transfer process and can improve the combustion characteristics of coal by reducing the ignition temperature and reaction activation energy of coal combustion. Al in the cathode material of waste lithium iron phosphate batteries can react with water vapor in coal powder under high temperature of hot air to produce a large amount of H2, which can increase the volume of coal gas and kinetic energy of blasting; at the same time, the increase of H2 can increase the temperature in the center area of the furnace and improve the liquid permeability of the center column; in addition, the increase of H2 concentration can reduce the viscosity of coal gas, accelerate the diffusion rate and reaction rate, promote indirect reduction reaction, and reduce direct reduction.
[0038] In the present invention, limestone enters the blast furnace and rapidly decomposes at high temperature to produce CO2 gas, which can quickly disperse coal powder, improve the contact between coal powder and O2 in the blast, and thus improve the combustion rate of coal powder; at the same time, the CaO produced by the decomposition of limestone reacts with water in the material in the blast furnace to release a large amount of heat, which helps to heat the reactants in the furnace, and thus promotes the high-temperature decomposition process of the positive electrode material of the waste lithium iron phosphate battery. Because the combustion of the positive electrode material of the waste lithium iron phosphate battery will produce a trace amount of H3PO4, the alkaline CaO can neutralize the excess acidic substances and maintain a suitable pH. In addition, CaO can also participate in slag making, which can increase the alkalinity of the slag, effectively reduce the S content of the molten iron, and thus improve the quality of the molten iron.
[0039] The inventor further discovered through experiments that if the addition ratio of lithium iron phosphate battery positive electrode material is increased, it will have a positive effect on reducing the ignition point temperature and burnout temperature, but the increase of lithium iron phosphate battery positive electrode material will also affect the precipitation rate of volatile matter. When the addition ratio of lithium iron phosphate battery positive electrode material is higher than 40%, the volatile analysis rate of coal powder combustion is significantly increased, which is not conducive to blast furnace coal injection. When the addition amount of lithium iron phosphate battery positive electrode material is too low, the effect on reducing the ignition point temperature and burnout temperature is very limited. Through experimental verification, when the addition ratio of lithium iron phosphate battery positive electrode material is controlled to 20% to 40%, the effect is better, which can not only reduce the ignition point temperature and burnout temperature, but also effectively control the precipitation of volatile matter in coal powder combustion, and at the same time effectively reduce the generation of thermal nitrogen oxides. Through experiments, when the proportion of lithium iron phosphate battery positive electrode material is added to 30%, the effect is best.
[0040] In the present invention, the limestone used is common limestone available on the market, and the components of the limestone are roughly the same, and can be used in the technical solution of the present invention. The lithium iron phosphate battery positive electrode materials used are lithium iron phosphate batteries used in the new energy field in the prior art, which are scrapped after use and then recycled and separated to obtain the lithium iron phosphate battery positive electrode materials. The components of the various substances in the materials are also roughly the same, and can be used in the technical solution of the present invention.
[0041] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0042] 1. The present invention uses limestone and lithium iron phosphate battery positive electrode materials as additives, which can reduce the ignition point of coal powder by 17-53°C, reduce the burnout temperature by 13-63°C, and increase the combustion rate by 10-20%;
[0043] 2. The additive provided by the present invention eliminates the problems of coke loss, furnace lining corrosion, furnace nodules, and safety hazards in milling;
[0044] 3. The additive provided by the present invention promotes efficient combustion of pulverized coal in a blast furnace, reduces the generation of nitrogen oxides in the blast furnace, reduces the content of nitrogen oxides in the flue gas emitted by the blast furnace, and can achieve ultra-low emission standards. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is the infrared spectrum of the additive I prepared in the embodiment of the present invention;
[0046] Figure 2 This is the infrared spectrum of the raw material limestone used in the present invention;
[0047] Figure 3 This is the infrared spectrum of the raw material of the lithium iron ion battery positive electrode material used in the present invention. DETAILED DESCRIPTION
[0048] The technical solution of the present invention is illustrated below by way of example, and the scope of protection requested by the present invention includes but is not limited to the following embodiments.
[0049] Raw materials preparation:
[0050] Limestone: Limestone mined from a limestone mine in Zhengzhou, Henan Province was selected, and its main components were tested as follows:
[0051] <![CDATA[CaCO3,wt%]]> <![CDATA[SiO2,wt%]]> MgO, wt% S, wt% 95.85 1.31 2.74 0.021
[0052] Lithium iron phosphate battery positive electrode material: The lithium iron phosphate battery positive electrode material is obtained by recycling the lithium iron phosphate batteries produced by CATL. The recycled waste lithium iron phosphate batteries are disassembled, physically crushed and separated to obtain the waste lithium iron phosphate positive electrode material. The main components of the waste lithium iron phosphate positive electrode material obtained by testing are as follows:
[0053]
[0054]
[0055] Coal powder: coal mined from a coal mine in Changzhi City, Shanxi Province.
[0056] Example 1
[0057] An additive for blast furnace coal injection, the additive comprising: in weight percentage,
[0058] 60g limestone, 40g waste lithium iron phosphate battery positive electrode material.
[0059] Preparation method: limestone and waste lithium iron phosphate battery positive electrode material are ground separately, the limestone is ground to a particle size of less than 5 mm; the lithium iron phosphate battery positive electrode material is ground to a particle size of less than 10 mm. Then the ground limestone powder and lithium iron phosphate battery positive electrode material powder are mixed evenly and ground. In the additive for blast furnace pulverized coal obtained by mixing evenly, the proportion of particles with a particle size of less than 0.074 mm is greater than 70%, and additive I is obtained.
[0060] The method described in Example 1 was adopted to adjust the usage ratio of limestone and waste lithium iron phosphate battery positive electrode material to prepare additives II to VIII respectively.
[0061] Comparative Example 1
[0062] The limestone was ground to a particle size less than 0.074 mm, which was greater than 70%, and was labeled as additive DI.
[0063] Comparative Example 2
[0064] An additive for blast furnace coal injection, the additive comprising: in weight percentage,
[0065] 60g limestone, 28g aluminum powder.
[0066] Preparation method: grind limestone and aluminum powder separately, grind limestone to a particle size of less than 5 mm; grind aluminum powder to a particle size of less than 10 mm. Then mix the ground limestone powder and aluminum powder evenly and grind them. Among the additives for blast furnace pulverized coal obtained by mixing evenly, the proportion of particles with a particle size of less than 0.074 mm is greater than 70%, and is marked as additive DII.
[0067] Comparative Example 3
[0068] An additive for blast furnace coal injection, the additive comprising: in weight percentage,
[0069] 60g limestone, 10g iron oxide powder.
[0070] Preparation method: limestone and iron oxide powder are ground separately, limestone is ground to a particle size of less than 5 mm; iron oxide powder is ground to a particle size of less than 10 mm. Then the ground limestone powder and iron oxide powder are mixed evenly and ground. Among the additives for blast furnace pulverized coal obtained by mixing evenly, the proportion of particles with a particle size of less than 0.074 mm is greater than 70%, and is marked as additive DIII.
[0071] Comparative Example 4
[0072] An additive for blast furnace coal injection, the additive comprising: in weight percentage,
[0073] 60g limestone, 30g aluminum powder, 10g iron oxide powder.
[0074] Preparation method: limestone, aluminum powder and iron oxide powder are ground separately, limestone is ground to a particle size of less than 5 mm; aluminum powder and iron oxide powder are ground to a particle size of less than 10 mm. Then the ground limestone powder, aluminum powder and iron oxide powder are mixed evenly and ground. Among the additives for blast furnace pulverized coal obtained by mixing evenly, the proportion of particles with a particle size of less than 0.074 mm is greater than 70%, and is marked as additive DIV.
[0075] Application test 1
[0076] The obtained additives I to VIII and additives DI to DIV are mixed, dried, and crushed to a particle size of less than 0.074 mm and a ratio greater than 70% according to a weight ratio of 4:100, respectively, to obtain mixed coal powders I to VIII and DI to DIV. Mixed coal powders I to VIII and DI to DIV are tested for ignition point, burnout temperature, and relative burnout time in accordance with GB / T18511-2001, and the volatile matter of each group of coal powders is tested in accordance with GB / T5751-2006. Sulfur content test: The spring content of the mixed coal powder is tested according to the Aska method in GB / T214-1996; the sulfur content in the ash after burnout is tested according to the barium sulfate weight method in GB / T1574-1995. The experimental results are as follows:
[0077] Table 1 Coal powder performance test
[0078]
[0079]
[0080] Through experiments, it was found that by adding additives, the ignition point temperature of coal powder can be reduced, the burnout temperature can be reduced, the relative burnout time can be shortened, and the precipitation of volatiles can be reduced. Among them, by adding a lithium iron phosphate battery positive electrode material in a proportion greater than 10% and less than 80% to the additive, the ignition point temperature of coal powder can be reduced to below 500°C, the burnout temperature can be controlled within 672°C, the relative burnout time can be shortened by more than 10%, and the volatile analysis rate can be controlled within 7%. As the amount of lithium iron phosphate battery positive electrode material added increases, the precipitation of volatiles increases. As the amount of lithium iron phosphate battery positive electrode material added decreases, the ignition point temperature and burnout temperature increase significantly, and the relative burnout time increases.
[0081] Application Test 2
[0082] The mixed coal powders I to VIII and DI to DIV were used in the same blast furnace of a steel plant in Shanxi Province. The same batch of sintered mineral materials and the same blast furnace process conditions were used to conduct pilot experiments to detect the NO in the flue gas discharged from the blast furnace after different coal powders were injected. x The experimental results are as follows:
[0083] Table 2 Coal powder used for blast furnace performance testing
[0084]
[0085]
[0086] Through experiments, it was found that the mixed coal powders I to VI prepared by adding the additives of the present invention and adding limestone and lithium iron phosphate battery positive electrode materials in proportion can promote the combustion of coal powder in the blast furnace, reduce the amount of thermal nitrogen oxides generated in the blast furnace, and thus reduce the concentration of nitrogen oxides in the flue gas discharged from the blast furnace. The mixed coal powders I to VI are used for blast furnace coal injection combustion, and the concentration of nitrogen oxides in the flue gas discharged from the blast furnace is less than 20 mg / Nm 3 , in line with the standards of Class I areas; by controlling the additive of limestone in the positive electrode material of lithium iron phosphate batteries, the concentration of nitrogen oxides in blast furnace exhaust gas can even be reduced to 1020mg / Nm 3 Below (8.9mg / Nm of mixed coal powder IV 3 ).
[0087] Note: Since the content of components in coal powder mined from different mines is different, the properties of the coal powder itself are also different. The present invention uses the same batch of coal powder mined from the same mine for the experiment, and the properties of the coal powder itself are based on the control group. The grinding of all materials in this application is processed by the same ball mill.
Claims
1. An additive for blast furnace coal injection, the additive comprising: In percentage by weight, Limestone 60%~80%; Lithium iron phosphate battery positive electrode material 20%~40%; Wherein: the composition of the positive electrode material of the lithium iron phosphate battery is: 68-76wt% Al, 22-28wt% LiFePO4, and the remainder is a conductive agent and a binder.
2. The additive for blast furnace coal injection according to claim 1, characterized in that: The additive includes: by weight percentage, 65% to 75% limestone; 25% to 35% lithium iron phosphate battery positive electrode material.
3. The additive for blast furnace coal injection according to claim 2, characterized in that: The additive includes: by weight percentage, 68% to 72% limestone; 28% to 32% lithium iron phosphate battery positive electrode material.
4. The additive for blast furnace coal injection according to any one of claims 1 to 3, characterized in that: The positive electrode material of the lithium iron phosphate battery is a waste positive electrode material of the lithium iron phosphate battery.
5. The additive for blast furnace coal injection according to any one of claims 1 to 3, characterized in that: The content of CaCO3 in the limestone is greater than 95 wt%, the content of SiO2 is not greater than 1.5 wt%, the content of MgO is not greater than 3 wt%, and the content of S is not greater than 0.025 wt%.
6. A method for preparing the additive for blast furnace coal injection according to any one of claims 1 to 5, the method comprising the following steps: Limestone and lithium iron phosphate battery positive electrode material are ground and mixed evenly to obtain an additive for blast furnace coal injection.
7. The preparation method according to claim 6, characterized in that: The limestone and the lithium iron phosphate battery positive electrode material are ground separately, and then the ground limestone powder and the lithium iron phosphate battery positive electrode material powder are mixed evenly; or the limestone and the lithium iron phosphate battery positive electrode material are mixed and then ground together.
8. The preparation method according to claim 6, characterized in that: The limestone is ground to a particle size of less than 5 mm; the positive electrode material of the lithium iron phosphate battery is ground to a particle size of less than 10 mm; and / or the additive for blast furnace pulverized coal obtained by mixing evenly has a proportion of particles less than 0.074 mm greater than 70%.
9. The preparation method according to claim 6, characterized in that: The lithium iron phosphate battery positive electrode material is a waste lithium iron phosphate battery positive electrode material, which comes from recycled waste lithium iron phosphate batteries. The waste lithium iron phosphate batteries are pretreated to obtain the waste lithium iron phosphate battery positive electrode material; the pretreatment is specifically: disassembling, physically crushing and separating the waste lithium iron phosphate batteries to obtain the waste lithium iron phosphate positive electrode material.
10. Use of an additive for blast furnace coal injection, comprising the additive for blast furnace coal injection according to any one of claims 1 to 5 or the additive for blast furnace coal injection prepared by the preparation method according to any one of claims 6 to 9, wherein the additive is mixed with raw coal and then used for blast furnace injection.
11. The use according to claim 10, characterized in that: The additive is mixed with coal powder, dried, crushed, and then injected into a blast furnace; Among them: the amount of additives used is 1~6wt% of the coal powder mass.
12. The use according to claim 11, characterized in that: The dosage of the additive is 2~5wt% of the coal powder mass.