A method for testing the gloss of a coating
By preparing a uniform oil-based paint slurry and performing multi-point testing and error correction, the accuracy problem of paint gloss testing was solved, achieving more precise gloss determination and eliminating the influence of instrument and quality fluctuation errors.
Patent Information
- Application Number
- CN202311278982.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-28
AI Technical Summary
Existing technologies are insufficient for accurately detecting coating gloss, as they are susceptible to errors from testing instruments and quality fluctuations, leading to inaccurate test results.
By preparing a uniform oil-based paint slurry, the gloss of the paint is tested at multiple locations using a gloss meter. The allowable error for gloss testing is determined by range calculation and correction using the standard error value of the gloss meter, thus eliminating the influence of instrument and quality fluctuations.
It enables more accurate characterization of coating gloss, eliminates the influence of errors caused by testing instruments and quality fluctuations, and provides a more accurate standard for gloss determination.
Smart Images

Figure CN117288726B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of titanium dioxide application performance, and particularly relates to a method for testing the gloss of coatings, which falls within the scope of titanium dioxide application performance testing. Background Technology
[0002] Titanium dioxide is a high-quality white powder pigment with excellent light scattering ability, resulting in good whiteness, high tinting strength, and strong hiding power. It also has high chemical stability and good weather resistance, is non-toxic and odorless, and has no irritating effect on the human body. It is widely used in coatings, plastics, inks, and papermaking industries.
[0003] Gloss is an important indicator of coatings, significantly impacting the appearance quality of the coating product. In practical applications, pigments are only one component of the coating; pigments themselves are matte, while the coating film has a gloss. If the titanium dioxide particles are very fine and can be evenly dispersed in the paint, the coating film will be smooth, mirror-like, and have good gloss. Conversely, if the titanium dioxide particles are too coarse, the coating film will be rough, the gloss will be reduced, and the color will appear darker after being colored with other base colors.
[0004] Therefore, the present invention provides a method for detecting the gloss of coatings, so as to eliminate the influence of uncertain factors or quality fluctuations on the accuracy of gloss detection.
[0005] In conclusion, there is an urgent need for a method to test the gloss of coatings in order to eliminate the impact of uncertain factors or quality fluctuations on the accuracy of gloss testing. Summary of the Invention
[0006] Therefore, in order to overcome the shortcomings of the existing technology, a method for detecting the gloss of coatings is provided, which eliminates the influence of errors caused by the testing instrument and quality fluctuations.
[0007] To achieve the above objectives, the following technical solution is adopted:
[0008] This invention provides a method for detecting the gloss of a coating, comprising the following steps:
[0009] a. Preparation of color paste: Ester solvent, dispersant, titanium dioxide and glass beads are added to the carrier resin in sequence, and the mixture is placed in a glass jar and sealed.
[0010] b. Vibrate the sealed glass jar to disperse the oil-based paint slurry, and obtain a uniformly dispersed slurry;
[0011] c. Prepare a sample of the dispersed oil-based paint slurry on a glass plate;
[0012] d. Place the sample prepared above in an oven to dry, then remove and cool to room temperature;
[0013] e. Use a gloss meter to measure the 60° gloss at three locations on the sample: the top, middle, and bottom.
[0014] f. Repeat step ae to obtain several sets of 60° gloss data for the same sample, and calculate the range for each set of 60° gloss data to obtain multiple ranges for the sample. Obtain the average range to get the allowable error of the sample.
[0015] g. Obtain the standard gloss meter allowable error value of the gloss meter, and add the allowable error value of the sample to the standard gloss meter allowable error value to obtain the gloss detection allowable error value;
[0016] h. Repeat step ae for the sample to be tested to obtain its 60° gloss data, and compare it with the 60° gloss data of the standard sample. If the difference is less than the allowable error value for gloss detection, it is a qualified coating; if the difference is greater than the allowable error value for gloss detection, it is an unqualified coating.
[0017] In some embodiments, in step b, the sealed glass jar is placed on a formulation optimization machine and vibrated for dispersion.
[0018] In some embodiments, in step c, the dispersed oily paint slurry is used to form a sample on a glass plate using an automatic coating machine.
[0019] In some embodiments, in step a, the amount of carrier resin added is 20g-50g; the amount of ester solvent added is 2g-10g; the amount of dispersant added is 2g±0.5g; the amount of titanium dioxide added is 55g±5g; and the amount of glass beads added is 100g.
[0020] In some embodiments, the dispersion time in step b is 30-150 min.
[0021] In some embodiments, the thickness of the film formed by the automatic coating instrument in step c is 100μm-200μm.
[0022] In some embodiments, the drying temperature in step d is 45°C-60°C, and the drying time is 15-30 min.
[0023] In some embodiments, the ester solvent is selected from one or more of butyl formate, isobutyl formate, methyl acetate, sec-butyl acetate, cyclohexyl acetate, ethyl propionate, n-butyl propionate, and methyl butyrate.
[0024] In some embodiments, the carrier resin is selected from one or more of polyamide resins and polycarbonate resins.
[0025] The present invention has the following beneficial technical effects:
[0026] The gloss characterization method of the present invention can analyze the range of gloss test results of titanium dioxide products in coatings, redefine and optimize the gloss judgment standard of titanium dioxide in coatings, and more accurately characterize the gloss of titanium dioxide in coatings.
[0027] The gloss characterization method of the present invention can eliminate the influence of errors caused by fluctuations in testing instruments and quality. Attached Figure Description
[0028] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0029] Figure 1 The range percentage statistics are obtained from 100 repeated experiments in one embodiment of the present invention. Detailed Implementation
[0030] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples and the accompanying drawings.
[0031] Embodiments of the present invention disclose a method for detecting the gloss of a coating, comprising the following steps:
[0032] a. Preparation of color paste: Ester solvent, dispersant, titanium dioxide and glass beads are added to the carrier resin in sequence, and the mixture is placed in a glass jar and sealed.
[0033] b. Vibrate the sealed glass jar to disperse the oil-based paint slurry, and obtain a uniformly dispersed slurry;
[0034] c. Prepare a sample of the dispersed oil-based paint slurry on a glass plate;
[0035] d. Place the sample prepared above in an oven to dry, then remove and cool to room temperature;
[0036] e. Use a gloss meter to measure the 60° gloss at three locations on the sample: the top, middle, and bottom.
[0037] f. Repeat step ae to obtain several sets of 60° gloss data for the same sample, and calculate the range for each set of 60° gloss data to obtain multiple ranges for the sample. Obtain the average range to get the allowable error of the sample.
[0038] g. Obtain the standard gloss meter allowable error value of the gloss meter, and add the allowable error value of the sample to the standard gloss meter allowable error value to obtain the gloss detection allowable error value;
[0039] h. Repeat step ae for the sample to be tested to obtain its 60° gloss data, and compare it with the 60° gloss data of the standard sample. If the difference is less than the allowable error value for gloss detection, it is a qualified coating; if the difference is greater than the allowable error value for gloss detection, it is an unqualified coating.
[0040] Preferably, in step b, the sealed glass jar is placed on a formulation optimization machine and shaken to disperse.
[0041] Preferably, in step c, the dispersed oily paint slurry is used to form a sample on a glass plate using an automatic coating machine.
[0042] Preferably, in step a, the amount of carrier resin added is 20g-50g; the amount of ester solvent added is 2g-10g; the amount of dispersant added is 2g±0.5g; the amount of titanium dioxide added is 55g±5g; and the amount of glass beads added is 100g.
[0043] Preferably, the dispersion time in step b is 30-150 min.
[0044] Preferably, the thickness of the film formed by the automatic coating instrument in step c is 100μm-200μm.
[0045] Preferably, the drying temperature in step d is 45℃-60℃, and the drying time is 15-30min.
[0046] Preferably, the ester solvent is selected from one or more of butyl formate, isobutyl formate, methyl acetate, sec-butyl acetate, cyclohexyl acetate, ethyl propionate, n-butyl propionate, and methyl butyrate.
[0047] Preferably, the carrier resin is selected from one or more of polyamide resin and polycarbonate resin.
[0048] Example
[0049] The method for characterizing the gloss of a coating described in this embodiment includes the following steps:
[0050] a. Weigh 36g of carrier resin, and add 2.5g of ester solvent, 1.5g of dispersant, 60g of titanium dioxide and 100g of glass beads into a glass jar in sequence.
[0051] b. Place the sealed glass jar on a formulation optimization machine and vibrate and disperse for 60 minutes to obtain a uniformly dispersed coating slurry;
[0052] c. Using an automatic coating machine, the prepared coating slurry is used to create a sample with a film thickness of 200μm on cardboard;
[0053] d. Place the sample prepared above in an oven to dry at a temperature of 45℃-60℃ for 30 minutes, then remove and cool to room temperature;
[0054] e. Perform 60° gloss tests on the top, middle and bottom three points of each sample to obtain a set of data, and calculate the range of each set of data to obtain the range of the sample.
[0055] f. By analyzing and comparing the data from 100 repeated experiments on the plate, the permissible error of the sample is determined. By consulting relevant literature, the permissible error of the testing instrument is found. Both sample error and instrument error are considered as factors affecting the test results. The test results are then corrected to eliminate the influence of permissible errors, thus obtaining more accurate test results.
[0056] Table 1. Range Statistics
[0057] Total number of experiments Range Number percentage% 100 0 2 2% 100 0.1 2 2% 100 0.2 10 10% 100 0.3 11 11% 100 0.4 12 12% 100 0.5 17 17% 100 0.6 20 20% 100 0.7 3 3% 100 0.8 5 5% 100 0.9 5 5% 100 ≥1.0 13 13%
[0058] From Table 1 and Figure 1 The analysis shows that the results of the same sample taken at different times will fluctuate to some extent, with the highest proportion (approximately 20%) having a range of 0.6. Through Xbar-R mean-range analysis, the average value of the samples in this experiment was 66.63°, and the average range was 0.591 (≈0.6). Therefore, the fluctuation range of gloss detection for the same sample can be obtained as ±0.6, which is the allowable error for the sample.
[0059] Table 2. Metrological performance of the gloss meter
[0060]
[0061] Table 2 shows the results obtained from consulting relevant materials. JJG696-2002 "Specular Gloss and Gloss Plate" stipulates that the allowable error value of the standard gloss meter for a 60° gloss meter is ±1.0.
[0062] Therefore, given that the sample fluctuation error is ±0.6 and the instrument's allowable error is ±1.0, the allowable error for gloss measurement should be ≥1.6. Since industry standards typically use integers for gloss values in external testing reports, using rounding, our optimal allowable error is ≥2. This means that when determining the result: Pass value = Standard value - 2.
[0063] Table 3. Detection results of three different samples
[0064]
[0065] Table 3 shows that the average 60° gloss of the standard samples in this experiment was 65, the average 60° gloss of sample #1 was 67, and the difference between the two was 2, which is equal to the allowable error. Therefore, the sample was qualified. The average 60° gloss of sample #2 was 53, and the difference between the two was 12, which is greater than the allowable error. Therefore, the sample was unqualified. The average 60° gloss of sample #3 was 67, and the difference between the two was 2, which is equal to the allowable error. Therefore, the sample was qualified.
[0066] Except for the source of titanium dioxide, the preparation of the standard sample and the sample are the same in terms of color paste preparation and subsequent steps.
[0067] The above are exemplary embodiments disclosed in this invention. However, it should be noted that various changes and modifications can be made without departing from the scope of the embodiments of this invention as defined by the claims. Although the elements disclosed in the embodiments of this invention may be described or claimed individually, they may be understood as multiple unless explicitly limited to a singular number.
[0068] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples. Within the framework of the invention, technical features of the above embodiments or different embodiments can be combined, and many other variations of different aspects of the invention exist, which are not provided in the details for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the protection scope of the invention.
Claims
1. A method of detecting the gloss of a paint, characterized in that, Includes the following steps: a. Preparation of color paste: Ester solvent, dispersant, titanium dioxide and glass beads are added to the carrier resin in sequence, and the mixture is placed in a glass jar and sealed. b. Vibrate the sealed glass jar to disperse the oil-based paint slurry, and obtain a uniformly dispersed slurry; c. Prepare a sample of the dispersed oil-based paint slurry on a glass plate; d. Place the sample prepared above in an oven to dry, then remove and cool to room temperature; e. Use a gloss meter to measure the 60° gloss at three locations on the sample: the top, middle, and bottom. f. Repeat step ae to obtain several sets of 60° gloss data for the same sample, and calculate the range for each set of 60° gloss data to obtain multiple ranges for the sample. Obtain the average range to get the allowable error of the sample. g. Obtain the standard gloss meter allowable error value of the gloss meter, and add the allowable error value of the sample to the standard gloss meter allowable error value to obtain the gloss detection allowable error value; h. Repeat step ae for the sample to be tested to obtain its 60° gloss data, and compare it with the 60° gloss data of the standard sample. If the difference is less than the allowable error value for gloss detection, it is a qualified coating; if the difference is greater than the allowable error value for gloss detection, it is an unqualified coating.
2. The method of detecting paint gloss according to claim 1, wherein, In step b, the sealed glass jar is placed on a formulation optimization machine and shaken to disperse.
3. The method of detecting paint gloss according to claim 1, wherein, In step c, the dispersed oil-based paint slurry is used to make a sample on a glass plate using an automatic coating machine.
4. The method of detecting paint gloss according to claim 1, wherein, In step a, the amount of carrier resin added is 20g-50g; the amount of ester solvent added is 2g-10g; the amount of dispersant added is 2g±0.5g; the amount of titanium dioxide added is 55g±5g; and the amount of glass beads added is 100g.
5. The method of detecting paint gloss according to claim 2, wherein, The dispersion time in step b is 30-150 min.
6. The method of detecting paint gloss according to claim 3, wherein The thickness of the film produced by the automatic coating machine in step c is 100μm-200μm.
7. The method of detecting paint gloss according to claim 1, wherein The drying temperature in step d is 45℃-60℃, and the drying time is 15-30min.
8. The method of detecting paint gloss according to claim 4, wherein, The ester solvent is selected from one or more of butyl formate, isobutyl formate, methyl acetate, sec-butyl acetate, cyclohexyl acetate, ethyl propionate, n-butyl propionate, and methyl butyrate.
9. The method of detecting paint gloss according to claim 4, wherein, The carrier resin is selected from one or more of polyamide resin and polycarbonate resin.