A self-grown MOF-coated diaphragm and its preparation method
By using a self-grown MOF-coated separator preparation method, the problems of poor electrolyte wettability of polyolefin separators and coating peeling off of ceramic separators were solved, achieving high energy density and improved safety performance of batteries.
Patent Information
- Application Number
- CN202311255615.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-27
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-27
AI Technical Summary
Existing polyolefin separators have poor electrolyte wettability, which leads to prolonged battery electrolyte injection time and increased internal resistance. The thickness of ceramic separator coatings cannot be reduced, limiting the improvement of cell volumetric energy density. At the same time, the use of binders poses a risk of detachment.
A method for preparing a self-grown MOF coating membrane was adopted. The base membrane was modified with chitosan-sodium phytate and dopamine hydrochloride solution, and combined with zirconium metal source and organic ligand solution to self-grow the MOF coating, forming chemical bonds and reducing the use of binders.
It improves the electrolyte absorption capacity, enhances the volumetric energy density of the battery cell, improves the adhesion strength and flame retardant properties of the separator, and avoids the risk of coating peeling.
Smart Images

Figure BDA0004471280100000081 
Figure BDA0004471280100000091
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium battery technology, specifically to a MOF-coated self-grown separator and its preparation method. Background Technology
[0002] Currently, commercially available battery separators are mainly polyolefin separators and ceramic-coated separators. However, with the development of battery technology, the poor electrolyte wettability of polyolefin separators has seriously affected the electrolyte injection time of batteries, thereby increasing the production and manufacturing costs of batteries. At the same time, poor electrolyte wettability leads to increased internal resistance of the battery cells and reduced cycle life of the cells.
[0003] The coating thickness of ceramic separators can no longer be reduced, which limits further increases in cell volumetric energy density and contradicts current technological approaches to improving energy density. Furthermore, current ceramic separators rely heavily on adhesives for bonding, increasing the risk of coating detachment. If this detachment enters the cell system, it poses unpredictable risks. Therefore, the application of polyolefin separators has attracted widespread attention. To further improve the adhesion between the coating and the polyolefin separator, while simultaneously enhancing the safety performance of the polyolefin separator, coating modification research is necessary. Summary of the Invention
[0004] The purpose of this invention is to provide a self-grown MOF-coated separator and its preparation method to solve the problems mentioned in the background art.
[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a MOF-coated self-grown separator and its preparation method, comprising the following steps:
[0006] Step 1:
[0007] S1: Dissolve chitosan and sodium phytate in deionized water, adjust the pH of the solution to 2-3 with dilute hydrochloric acid, and stir to obtain chitosan-sodium phytate solution;
[0008] S2: Mix dopamine hydrochloride and deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution;
[0009] S3: Mix chitosan-sodium phytate solution and dopamine hydrochloride solution, and stir magnetically to obtain a mixed solution; immerse the base film in alkaline solution for 1-2 hours and then dry it; immerse the treated base film in hydrogen peroxide for 1-2 hours, wash with deionized water and dry it; place the base film in the mixed solution and keep it at 40-50℃ for 3-4 hours; add genipin to react; remove the base film and dry it to obtain polydopamine-chitosan modified base film;
[0010] Step 2:
[0011] The polydopamine-chitosan modified base film was immersed in a zirconium metal source solution, and then washed with methanol solution for 30-60 seconds. It was then immersed in an organic ligand solution and washed with methanol solution for 30-60 seconds. After repeated immersion and drying, a Zr-MOF self-grown septum was obtained.
[0012] Furthermore, in S1, the chitosan-sodium phytate solution contains, by weight, 2-3 parts chitosan, 2-3 parts sodium phytate, and 100 parts deionized water.
[0013] Furthermore, in S2, the content of each component in the dopamine hydrochloride solution, by weight, is 3-5 parts dopamine hydrochloride and 80-100 parts deionized water.
[0014] Furthermore, in S3, the mass ratio of chitosan to dopamine hydrochloride in the mixed solution is (2.4–2.7):(8.3–8.6).
[0015] Furthermore, in S3, the amount of genipin used is 3-5 wt.% of the amount of chitosan.
[0016] Furthermore, in step 2, the concentration of the zirconium metal source solution is 30–40 mM; the immersion time is 120–180 s.
[0017] Furthermore, in step 2, the zirconium metal source solution is either zirconium tetrachloride solution or zirconium dichloride octahydrate.
[0018] Furthermore, in step 2, the concentration of the organic ligand solution is 50–60 mM; the soaking time is 120–180 s.
[0019] Furthermore, in step 2, the organic ligand solution is any one of 4,4-biphenyl phthalic acid solution, 2,5-dihydroxyterephthalic acid solution, or 2-aminoterephthalic acid solution.
[0020] Furthermore, in step 2, the methanol cleaning time is 30–60 seconds.
[0021] Furthermore, in step 2, the number of immersion cycles is 10 to 100.
[0022] Furthermore, in step 2, the thickness of the MOF growth layer is 10–100 nm.
[0023] Compared with existing technologies, the beneficial effects achieved by this invention are as follows: First, due to the porosity of MOF, it has extremely strong liquid absorption capacity and can store a large amount of electrolyte, solving the problem of poor wettability of the base film; Second, because the MOF grows from itself onto the surface of the base film, the thickness does not increase significantly, which is beneficial to improving the volumetric energy density of the battery cell; Third, this invention immerses the base film in a mixed solution of polydopamine and chitosan, allowing chitosan and polydopamine to polymerize on the surface of the base film. Since the MOF material is distributed on the surface of the base film through chemical bonds, it prevents the membrane from shrinking and further improves the peel strength between the MOF layer and the base film. In addition, sodium phytate, which has flame-retardant properties, is added to the mixed solution. Therefore, the flame retardant performance of the membrane is also improved; fourth, polydopamine itself has a strong adhesion effect. After polymerization on the base membrane surface, the use of a large amount of adhesive is avoided. It should be noted that the amount of chitosan and dopamine hydrochloride in the mixed solution needs to be limited. Since there is an electrostatic adsorption effect between chitosan and sodium phytate, when the chitosan content is too low, less sodium phytate is adsorbed, resulting in a poor flame retardant effect. When the chitosan content is too high, the polydopamine-chitosan membrane will have a reduced adhesion effect to MOF due to the adsorption of more sodium phytate on the surface. Therefore, it is more preferable that the mass ratio of chitosan to dopamine hydrochloride in the mixed solution be controlled at (2.4~2.7):(8.3~8.6). Detailed Implementation
[0024] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] Materials used in this invention and their sources: The base membranes in Examples 1 to 8 were prepared by our company, and the preparation method refers to patent CN202010339196.2. The polyolefin membrane material is polyethylene with a thickness of 9 μm. The ceramic-coated membrane in Comparative Example 3 is from Beike New Materials Technology Co., Ltd., and the coating thickness is 1.5 μm.
[0026] Example 1: A method for preparing a self-grown MOF-coated separator, comprising the following steps:
[0027] Step 1:
[0028] S1: Dissolve 3g of chitosan and 3g of sodium phytate in 100g of deionized water, adjust the pH of the solution to 2 with dilute hydrochloric acid, and stir to obtain chitosan-sodium phytate solution;
[0029] S2: Mix 5g of dopamine hydrochloride and 95g of deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution;
[0030] S3: Chitosan-sodium phytate solution and dopamine hydrochloride solution were mixed and magnetically stirred at 25°C for 4 hours to obtain a mixed solution containing 2.4 g chitosan and 8.6 g dopamine hydrochloride. The base film was immersed in an alkaline solution for 1 hour and then dried to increase its surface activity. The treated base film was then immersed in hydrogen peroxide for 1 hour, washed with deionized water, and dried. The base film was then placed in the mixed solution and kept in an oven at 40°C for 3 hours. 0.12 g genipin was added, and the reaction was carried out for 1 hour. The base film was then removed and dried to obtain a polydopamine-chitosan modified base film.
[0031] Step 2:
[0032] The polydopamine-chitosan modified base membrane was immersed in a 30 mM zirconium tetrachloride metal source solution for 120 s, and then washed with methanol solution for 30 s. It was then immersed in a 50 mM 2,5-dihydroxyterephthalic acid organic ligand solution for 120 s and washed with methanol solution for 30 s. After 50 cycles of immersion, it was dried at 60 °C for 20 s to obtain a Zr-MOF self-grown septum.
[0033] Example 2: A method for preparing a self-grown MOF-coated separator, comprising the following steps:
[0034] Step 1:
[0035] S1: Dissolve 3g of chitosan and 3g of sodium phytate in 100g of deionized water, adjust the pH of the solution to 2.1 with dilute hydrochloric acid, and stir to obtain a chitosan-sodium phytate solution;
[0036] S2: Mix 5g of dopamine hydrochloride and 95g of deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution;
[0037] S3: Chitosan-sodium phytate solution and dopamine hydrochloride solution were mixed and magnetically stirred at 26℃ for 4.2h to obtain a mixed solution containing 2.4g chitosan and 8.6g dopamine hydrochloride. The base film was soaked in an alkaline solution for 1.1h and then dried to increase its surface activity. The treated base film was then soaked in hydrogen peroxide for 1.2h, washed with deionized water, and dried. The base film was then placed in the mixed solution and kept in an oven at 41℃ for 3.15h. 0.12g genipin was added, and the reaction was carried out for 1.1h. The base film was then removed and dried to obtain a polydopamine-chitosan modified base film.
[0038] Step 2:
[0039] The polydopamine-chitosan modified base membrane was immersed in a 30 mM zirconium tetrachloride metal source solution for 120 s, and then washed with methanol solution for 33 s. It was then immersed in a 50 mM 2,5-dihydroxyterephthalic acid organic ligand solution for 120 s and washed with methanol solution for 35 s. After 10 cycles of immersion, it was dried at 65 °C for 22 s to obtain a Zr-MOF self-grown septum.
[0040] Example 3: A method for preparing a self-grown MOF-coated separator, comprising the following steps:
[0041] Step 1:
[0042] S1: Dissolve 3g of chitosan and 3g of sodium phytate in 100g of deionized water, adjust the pH of the solution to 2.3 with dilute hydrochloric acid, and stir to obtain a chitosan-sodium phytate solution;
[0043] S2: Mix 5g of dopamine hydrochloride and 95g of deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution;
[0044] S3: Chitosan-sodium phytate solution and dopamine hydrochloride solution were mixed and magnetically stirred at 27℃ for 4.5h to obtain a mixed solution containing 2.4g chitosan and 8.6g dopamine hydrochloride. The base film was soaked in an alkaline solution for 1.4h and then dried to increase its surface activity. The treated base film was then soaked in hydrogen peroxide for 1.4h, washed with deionized water, and dried. The base film was then placed in the mixed solution and kept in an oven at 45℃ for 3.6h. 0.12g genipin was added, and the reaction was carried out for 1.5h. The base film was then removed and dried to obtain a polydopamine-chitosan modified base film.
[0045] Step 2:
[0046] The polydopamine-chitosan modified base membrane was immersed in a 30 mM zirconium tetrachloride metal source solution for 125 s, and then washed with methanol solution for 35 s. It was then immersed in a 50 mM 2,5-dihydroxyterephthalic acid organic ligand solution for 125 s and washed with methanol solution for 35 s. After 40 cycles of immersion, it was dried at 63 °C for 20 s to obtain a Zr-MOF self-grown septum.
[0047] Example 4: A method for preparing a self-grown MOF-coated separator, comprising the following steps:
[0048] Step 1:
[0049] S1: Dissolve 3g of chitosan and 3g of sodium phytate in 100g of deionized water, adjust the pH of the solution to 2.5 with dilute hydrochloric acid, and stir to obtain a chitosan-sodium phytate solution;
[0050] S2: Mix 5g of dopamine hydrochloride and 95g of deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution;
[0051] S3: Chitosan-sodium phytate solution and dopamine hydrochloride solution were mixed and magnetically stirred at 27℃ for 4.5h to obtain a mixed solution containing 2.4g chitosan and 8.6g dopamine hydrochloride. The base film was soaked in an alkaline solution for 1.5h and then dried to increase its surface activity. The treated base film was then soaked in hydrogen peroxide for 1.4h, washed with deionized water, and dried. The base film was then placed in the mixed solution and kept in an oven at 45℃ for 3.5h. 0.12g genipin was added, and the reaction was carried out for 1.8h. The base film was then removed and dried to obtain a polydopamine-chitosan modified base film.
[0052] Step 2:
[0053] The polydopamine-chitosan modified base membrane was immersed in a 30 mM zirconium tetrachloride metal source solution for 150 s, and then washed with methanol solution for 45 s. It was then immersed in a 50 mM 2,5-dihydroxyterephthalic acid organic ligand solution for 150 s and washed with methanol solution for 45 s. After 55 cycles of immersion, it was dried at 63 °C for 23 s to obtain a Zr-MOF self-grown septum.
[0054] Example 5: A method for preparing a self-grown MOF-coated separator, comprising the following steps:
[0055] Step 1:
[0056] S1: Dissolve 3g of chitosan and 3g of sodium phytate in 100g of deionized water, adjust the pH of the solution to 2.4 with dilute hydrochloric acid, and stir to obtain a chitosan-sodium phytate solution;
[0057] S2: Mix 5g of dopamine hydrochloride and 95g of deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution;
[0058] S3: Chitosan-sodium phytate solution and dopamine hydrochloride solution were mixed and magnetically stirred at 28℃ for 5.5h to obtain a mixed solution containing 2.4g chitosan and 8.6g dopamine hydrochloride. The base film was soaked in an alkaline solution for 1.8h and then dried to increase its surface activity. The treated base film was then soaked in hydrogen peroxide for 1.5h, washed with deionized water, and dried. The base film was then placed in the mixed solution and kept in an oven at 47℃ for 3.6h. 0.12g genipin was added, and the reaction was carried out for 1.45h. The base film was then removed and dried to obtain a polydopamine-chitosan modified base film.
[0059] Step 2:
[0060] The polydopamine-chitosan modified base membrane was immersed in a 30 mM zirconium tetrachloride metal source solution for 160 s, and then washed with methanol solution for 50 s. It was then immersed in a 50 mM 2,5-dihydroxyterephthalic acid organic ligand solution for 160 s and washed with methanol solution for 50 s. After 75 cycles of immersion, it was dried at 61 °C for 28 s to obtain a Zr-MOF self-grown septum.
[0061] Example 6: A method for preparing a self-grown MOF-coated separator, comprising the following steps:
[0062] Step 1:
[0063] S1: Dissolve 3g of chitosan and 3g of sodium phytate in 100g of deionized water, adjust the pH of the solution to 3 with dilute hydrochloric acid, and stir to obtain chitosan-sodium phytate solution;
[0064] S2: Mix 5g of dopamine hydrochloride and 95g of deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution;
[0065] S3: Chitosan-sodium phytate solution and dopamine hydrochloride solution were mixed and magnetically stirred at 34℃ for 5.8h to obtain a mixed solution containing 2.4g chitosan and 8.6g dopamine hydrochloride. The base film was soaked in an alkaline solution for 2h and then dried to increase its surface activity. The treated base film was then soaked in hydrogen peroxide for 1.5h, washed with deionized water, and dried. The base film was then placed in the mixed solution and kept in an oven at 50℃ for 3.9h. 0.12g genipin was added, and the reaction was carried out for 1.85h. The base film was then removed and dried to obtain a polydopamine-chitosan modified base film.
[0066] Step 2:
[0067] The polydopamine-chitosan modified base membrane was immersed in a 30 mM zirconium tetrachloride metal source solution for 150 s, and then washed with methanol solution for 58 s. It was then immersed in a 50 mM 2,5-dihydroxyterephthalic acid organic ligand solution for 170 s and washed with methanol solution for 60 s. After 85 cycles of immersion, it was dried at 68 °C for 30 s to obtain a Zr-MOF self-grown septum.
[0068] Example 7: A method for preparing a self-grown MOF-coated separator, comprising the following steps:
[0069] Step 1:
[0070] S1: Dissolve 3g of chitosan and 3g of sodium phytate in 100g of deionized water, adjust the pH of the solution to 2.8 with dilute hydrochloric acid, and stir to obtain a chitosan-sodium phytate solution;
[0071] S2: Mix 5g of dopamine hydrochloride and 95g of deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution;
[0072] S3: Chitosan-sodium phytate solution and dopamine hydrochloride solution were mixed and magnetically stirred at 33℃ for 5.5h to obtain a mixed solution containing 2.4g chitosan and 8.6g dopamine hydrochloride. The base film was soaked in an alkaline solution for 2h and then dried to increase its surface activity. The treated base film was then soaked in hydrogen peroxide for 1h, washed with deionized water, and dried. The base film was then placed in the mixed solution and kept in an oven at 47℃ for 3.8h. 0.12g genipin was added, and the reaction was carried out for 1.65h. The base film was then removed and dried to obtain a polydopamine-chitosan modified base film.
[0073] Step 2:
[0074] The polydopamine-chitosan modified base membrane was immersed in a 30 mM zirconium tetrachloride metal source solution for 175 s, and then washed with methanol solution for 58 s. It was then immersed in a 50 mM 2,5-dihydroxyterephthalic acid organic ligand solution for 170 s and washed with methanol solution for 58 s. After 57 cycles of immersion, it was dried at 70 °C for 28 s to obtain a Zr-MOF self-grown septum.
[0075] Example 8: A method for preparing a self-grown MOF-coated separator, comprising the following steps:
[0076] Step 1:
[0077] S1: Dissolve 3g of chitosan and 3g of sodium phytate in 100g of deionized water, adjust the pH of the solution to 3 with dilute hydrochloric acid, and stir to obtain chitosan-sodium phytate solution;
[0078] S2: Mix 5g of dopamine hydrochloride and 95g of deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution;
[0079] S3: Chitosan-sodium phytate solution and dopamine hydrochloride solution were mixed and magnetically stirred at 35℃ for 6 hours to obtain a mixed solution containing 2.4g chitosan and 8.6g dopamine hydrochloride. The base film was immersed in an alkaline solution for 2 hours and then dried to increase its surface activity. The treated base film was then immersed in hydrogen peroxide for 2 hours, washed with deionized water, and dried. The base film was then placed in the mixed solution and kept in an oven at 50℃ for 4 hours. 0.12g genipin was added, and the reaction was carried out for 2 hours. The base film was then removed and dried to obtain a polydopamine-chitosan modified base film.
[0080] Step 2:
[0081] The polydopamine-chitosan modified base membrane was immersed in a 30 mM zirconium oxychloride octahydrate metal source solution for 120 s, and then washed with methanol solution for 60 s. It was then immersed in a 50 mM 4,4-biphenyldicarboxylic acid organic ligand solution for 120 s and washed with methanol solution for 60 s. After 100 cycles of immersion, it was dried at 70 °C for 30 s to obtain a Zr-MOF self-grown septum.
[0082] Comparative Example 1: No polydopamine and chitosan were used to modify the surface of the base film; all other parameters were the same as in Example 1.
[0083] Step 1:
[0084] The base film was soaked in an alkaline solution for 1 hour and then dried to increase its surface activity. The treated base film was then soaked in hydrogen peroxide for 1 hour, washed with deionized water, and dried to obtain a surface-functionalized base film.
[0085] Step 2:
[0086] The surface-functionalized substrate was immersed in a 30 mM zirconium tetrachloride metal source solution for 120 s, and then washed with methanol solution for 30 s. It was then immersed in a 50 mM 2,5-dihydroxyterephthalic acid organic ligand solution for 120 s and washed with methanol solution for 30 s. After 50 cycles of immersion, it was dried at 60 °C for 20 s to obtain a Zr-MOF self-grown septum.
[0087] Comparative Example 2: The amount of chitosan in S3 was increased, while the other parameters were the same as in Example 2.
[0088] Step 1:
[0089] S1: Dissolve 3g of chitosan and 3g of sodium phytate in 100g of deionized water, adjust the pH of the solution to 2.1 with dilute hydrochloric acid, and stir to obtain a chitosan-sodium phytate solution;
[0090] S2: Mix 5g of dopamine hydrochloride and 95g of deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution;
[0091] S3: Chitosan-sodium phytate solution and dopamine hydrochloride solution were mixed and magnetically stirred at 26℃ for 4.2h to obtain a mixed solution containing 3g chitosan and 8.6g dopamine hydrochloride. The base film was soaked in an alkaline solution for 1.1h and then dried to increase its surface activity. The treated base film was then soaked in hydrogen peroxide for 1.2h, washed with deionized water, and dried. The base film was then placed in the mixed solution and kept in an oven at 41℃ for 3.15h. 0.12g genipin was added, and the reaction was carried out for 1.1h. The base film was then removed and dried to obtain a polydopamine-chitosan modified base film.
[0092] Step 2:
[0093] The polydopamine-chitosan modified base membrane was immersed in a 30 mM zirconium tetrachloride metal source solution for 120 s, and then washed with methanol solution for 33 s. It was then immersed in a 50 mM 2,5-dihydroxyterephthalic acid organic ligand solution for 120 s and washed with methanol solution for 35 s. After 50 cycles of immersion, it was dried at 65 °C for 22 s to obtain a Zr-MOF self-grown septum.
[0094] Comparative Example 3: Using a conventional ceramic-coated diaphragm.
[0095] Experiment: Performance tests were conducted on Examples 1-8 and Comparative Examples 1-3. The experimental results are shown in the table below. Wherein:
[0096] Contact angle: Using a contact angle measuring instrument, 2 microliters of electrolyte were dropped onto the diaphragm with a needle with an outer diameter of 1.6 mm, and the contact angle was measured in degrees at 5 seconds.
[0097] Coating thickness test: Using a Maer thickness gauge, manually lift the test head, place the membrane sample to be tested flat under the test head, click the "Start" button on the panel, and then read the value on the screen. First, measure the base film thickness, then measure the coating film thickness; therefore, coating thickness = coating film thickness - base film thickness.
[0098] Heat shrinkage: Prepare a 200×100mm (to distinguish between longitudinal and transverse) diaphragm sample using the cutting module. Sandwich the sample between several sheets of A3 paper and place it in a drying oven that has reached the preset temperature. After a specified time, remove the sample and measure the longitudinal and transverse dimensions using an image measuring instrument. Calculate the shrinkage rate using the following formula:
[0099] Shrinkage % = (Length (before drying) - Length (after drying)) / Length (before drying) × 100%;
[0100] Flame retardant performance test: The limiting oxygen index of the diaphragm is tested in accordance with GB / T 2406.
[0101]
[0102]
[0103] Conclusions: Data from Examples 1-8 show that modifying the polymer-based membrane using the method of this invention not only improves the limiting oxygen index and enhances flame retardant properties, but also facilitates MOF coating growth, resulting in a self-growing MOF separator. Comparing Example 1 with Comparative Example 1 reveals that the self-growing MOF separator has a smaller contact angle, indicating superior electrolyte wettability compared to commercially available polyethylene-based membranes and conventional ceramic-coated separators. Comparing Example 2 with Comparative Example 2 shows that increasing the amount of chitosan can increase the limiting oxygen index, but it also affects the self-growth effect of the MOF, resulting in poor heat shrinkage performance. Comparing Example 3 with Comparative Example 3 shows that the coating thickness of the self-growing MOF separator is much smaller than that of the ceramic-coated separator, and it exhibits superior heat shrinkage performance.
[0104] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method of making a MOF-coated autogrown separator, characterized by: Includes the following steps: Step 1: The base film was soaked in an alkaline solution for 1-2 hours and then dried. The treated base film was soaked in hydrogen peroxide for 1-2 hours and then washed with deionized water to obtain a surface-functionalized base film. The surface-functionalized base film was modified by a mixed solution of chitosan, sodium phytate and dopamine hydrochloride to obtain a polydopamine-chitosan modified base film. Step 2: The polydopamine-chitosan modified base film was immersed in a zirconium metal source solution for 120-180 s, and then washed with methanol solution for 30-60 s. It was then immersed in an organic ligand solution for 120-180 s and washed with methanol solution for 30-60 s. After repeated immersion and drying, a Zr-MOF self-grown septum was obtained.
2. The method for preparing a self-grown MOF-coated diaphragm according to claim 1, characterized in that: Step 1, the preparation method of the polydopamine-chitosan modified base film includes the following steps: S1: Dissolve chitosan and sodium phytate in deionized water, adjust the pH of the solution to 2-3 with dilute hydrochloric acid, and stir to obtain chitosan-sodium phytate solution. S2: Mix dopamine hydrochloride and deionized water, and stir until homogeneous to obtain a dopamine hydrochloride solution; S3: Mix chitosan-sodium phytate solution and dopamine hydrochloride solution, and stir magnetically to obtain a mixed solution; Place the surface-functionalized base film in the mixed solution, keep it at 40~50℃ for 3~4h, add genipin to react, and then take out the base film and dry it to obtain a polydopamine-chitosan modified base film.
3. The method for preparing a self-grown MOF-coated diaphragm according to claim 2, characterized in that: In S1, the chitosan-sodium phytate solution contains 2-3 parts chitosan, 2-3 parts sodium phytate, and 100 parts deionized water by weight. In S2, the dopamine hydrochloride solution contains 3-5 parts dopamine hydrochloride and 80-100 parts deionized water by weight.
4. The method for preparing a self-grown MOF-coated diaphragm according to claim 2, characterized in that: In S3, the mass ratio of chitosan to dopamine hydrochloride in the mixed solution is (2.4~2.7):(8.3~8.6); the amount of genipin used is 3~5 wt.% of the amount of chitosan.
5. The method for preparing a self-grown MOF-coated diaphragm according to claim 1, characterized in that: In step 2, the concentration of the zirconium metal source solution is 30~40mM.
6. The method for preparing a self-grown MOF-coated diaphragm according to claim 1, characterized in that: In step 2, the zirconium metal source solution is either zirconium tetrachloride solution or zirconium dichloride octahydrate.
7. The method for preparing a self-grown MOF-coated diaphragm according to claim 1, characterized in that: In step 2, the concentration of the organic ligand solution is 50-60 mM.
8. The method for preparing a self-grown MOF-coated diaphragm according to claim 1, characterized in that: In step 2, the organic ligand solution is any one of 4,4-biphenyl phthalic acid solution, 2,5-dihydroxyterephthalic acid solution, or 2-aminoterephthalic acid solution.
9. The method for preparing a self-grown MOF-coated diaphragm according to claim 1, characterized in that: In step 2, the number of immersion cycles is 10 to 100; the thickness of the Zr-MOF coating on the diaphragm is 10 to 100 nm.
10. A diaphragm prepared by any one of the methods for preparing a self-grown MOF-coated diaphragm according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of polyolefin diaphragm with high mechanical strength
CN111525076A
Poly-dopamine modified lithium-ion battery diaphragm and preparation method thereof
CN103545474A
MOFs-modified double-layer structure composite electrospun nanofiber membrane, preparation method and application of MOFs-modified double-layer structure composite electrospun nanofiber membrane in blood purification