Polarizers, polarizing lenses and optical components
By using a combination of a uniaxially stretched polarizing film and a birefringent protective sheet in a polarizing lens, and employing polyurethane adhesives and injection molding, the problem of reduced transparency of polarizing lenses at high temperatures was solved, achieving both transparency maintenance and improved reliability in high-temperature environments.
Patent Information
- Application Number
- CN202280025504.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-31
- Filing Date
- 2022-03-31
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-03-31
AI Technical Summary
Existing polarizing lenses tend to have reduced transparency at high temperatures, which affects their reliability.
A uniaxially stretched polarizing film is combined with a protective sheet of different birefringence, and a polyurethane adhesive is used as the bonding layer. The optical lens is formed by injection molding to ensure that the transparency does not decrease at high temperatures.
It effectively suppresses or prevents the reduction of transparency at high temperatures, thus improving the reliability of polarizing lenses and optical components.
Smart Images

Figure CN117295986B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a polarizer, a polarizing lens, and an optical component. Background Technology
[0002] A polarizing lens having a polarizing laminate (polarizer) has been proposed, wherein the polarizing laminate is configured to cover both sides of the polarizing film with a coating layer made of a polycarbonate resin or polyamide resin as the main material (for example, see Patent Document 1).
[0003] The polarizing lens is manufactured by, for example, by having protective films adhered to both sides of a polarizing laminate (polarizer) that appears as a flat plate when viewed from above, punching the polarizing laminate into a predetermined shape, such as a circle when viewed from above. Then, by hot bending the polarizing laminate under heat, a polarizer formed into a curved plate shape is produced. After peeling off the protective film from the polarizer, the polarizer is attached to a mold having a curved plate-shaped recess, with the recess of the mold and the protrusion of the polarizer abutting each other. Then, injection molding is used to form a resin layer (optical lens) on the concave surface of the polarizer, primarily composed of a polycarbonate-based resin or a polyamide-based resin.
[0004] Furthermore, depending on its intended use, a hard coating is formed on at least one side of the polarizing lens as the outermost layer.
[0005] In the polarization laminate of such a polarizing lens, the bonding between the polarizing film and the coating layer is carried out through a bonding layer. Considering its transparency and bonding strength, a urethane adhesive can sometimes be used for this bonding layer.
[0006] However, if the polarizing lens is manufactured using the above-described method, the following problem arises: the transparency of the polarizing laminate decreases after the hot bending process of the polarizing laminate (polarizer), the injection molding of the resin layer (optical lens), and the formation of the hard coating.
[0007] Furthermore, this problem, namely the reduction in the transparency of the polarization laminate, also occurs when sunglasses (eyeglasses) equipped with the polarization lens are placed in high-temperature spaces such as the dashboard of a car for extended periods.
[0008] Existing technical documents
[0009] Patent documents
[0010] Patent document 1: Japanese Patent Application Publication No. 2009-294445. Summary of the Invention
[0011] The problem that the invention aims to solve
[0012] The purpose of this invention is to provide a polarizer that can reliably suppress or prevent the reduction of transparency even when exposed to high temperatures, and to provide a polarizing lens and optical component with excellent reliability incorporating the polarizer.
[0013] Methods for solving problems
[0014] This objective is achieved by the present invention described below (1) to (11).
[0015] (1) A polarizer comprising: a polarizing film, the polarizing film being uniaxially stretched and having an absorption axis in the direction of the uniaxial stretching; a first protective sheet, the first protective sheet being stacked on one side of the polarizing film and having birefringence; a second protective sheet, the second protective sheet being stacked on the other side of the polarizing film and having lower birefringence than the first protective sheet; a first bonding layer, the first bonding layer bonding the polarizing film and the first protective sheet; and a second bonding layer, the second bonding layer bonding the polarizing film and the second protective sheet, characterized in that the first bonding layer is a bonding layer mainly composed of a polyurethane adhesive, and when the polarizer is immersed in distilled water at 80°C for 15 minutes according to JIS K 7136:2000, the haze value of the polarizer is measured to be 0.05% or more and 1.00% or less.
[0016] (2) According to the polarizer described in (1) above, when the polarizer is immersed in distilled water at 80°C for 15 minutes in accordance with JIS K 7136:2000, the adhesion force of the polarizer is measured and the adhesion force satisfies the following requirement A.
[0017] Requirement A: According to JIS K 6854-2, the polarizer is cut into pieces with a length of 200mm and a width of 25mm. Then, at 140°C, one end of the first protective sheet of the polarizer is held and peeled at a speed of 10mm / min in a 180° direction to a length of 10mm. The adhesion force of the first protective sheet to the polarizing film is measured to be more than 40N / 25mm and less than 500N / 25mm.
[0018] (3) The polarizer according to (1) or (2) above, wherein the polyurethane adhesive is a single-liquid moisture crosslinking type or a two-liquid crosslinking type.
[0019] (4) The polarizer according to any one of (1) to (3) above, wherein the first protective sheet is a protective sheet made of polycarbonate resin or polyamide resin as the main material, and the second protective sheet is a protective sheet made of cellulose resin as the main material.
[0020] (5) The polarizer according to any one of (1) to (4) above, wherein the polarizing film is made of polyvinyl alcohol resin or its derivative as the main material, and contains dichroic dye and is uniaxially stretched.
[0021] (6) The polarizer according to any one of (1) to (5) above, wherein the polarizer is formed into a curved plate shape with the first protective sheet forming a concave surface and the second protective sheet forming a convex surface, and the polarizer is disposed in the cavity of the mold of the injection molding machine with the convex side of the polarizer becoming the mold side of the injection molding machine and the concave side exposed, so as to form an optical lens made of injection molding optical resin as the main material and bonded to the first protective sheet by injection molding.
[0022] (7) A polarizing lens, characterized in that the polarizing lens comprises: a polarizing sheet as described in any one of (1) to (6) above, the polarizing sheet being formed into a curved plate shape such that the first protective sheet forms a concave surface and the second protective sheet forms a convex surface; and an optical lens, the optical lens being joined to the first protective sheet on the concave surface and formed by injection molding.
[0023] (8) The polarizing lens according to (7) above, wherein when the polarizing lens is immersed in distilled water at 80°C for 15 minutes in accordance with JIS K 7136:2000 and the haze value of the polarizing lens is measured, the haze value is 0.05% or more and 1.00% or less.
[0024] (9) The polarizing lens according to (7) or (8) above, wherein, when using the polarizing lens, the concave surface of the first protective sheet side of the polarizing sheet faces the user's eye side.
[0025] (10) The polarizing lens according to any one of (7) to (9) above, wherein, in the polarizing sheet provided by the polarizing lens, the difference between the curvature on MD and the curvature on TD is 0.05 or more and 0.5 or less.
[0026] (11) An optical component, characterized in that the optical component comprises a polarizing lens as described in any one of (7) to (10) above.
[0027] The effects of the invention
[0028] According to the present invention, when the haze value of a polarizer is measured after immersing it in distilled water at 80°C for 15 minutes in accordance with JIS 7136:2000, the haze value satisfies the condition of being 0.05% or more and 1.00% or less. Therefore, for example, in cases such as hot bending of the polarizer under heating for manufacturing a polarizing lens or injection molding of an optical lens, even when the polarizer is exposed to high temperatures, it can be said that the reduction in the transparency of the polarizer is reliably suppressed or prevented. Therefore, it is possible to manufacture polarizing lenses and optical components with excellent reliability. Attached Figure Description
[0029] Figure 1 This is a perspective view showing an embodiment when the polarizing lens having the polarizer of the present invention is applied to sunglasses.
[0030] Figure 2 This is a schematic diagram illustrating a method for manufacturing a polarizing lens having the polarizer of the present invention.
[0031] Figure 3 This is a longitudinal sectional view showing an embodiment of the polarizer of the present invention. Detailed Implementation
[0032] Hereinafter, the polarizer, polarizing lens, and optical components of the present invention will be described in detail with reference to the preferred embodiments shown in the accompanying drawings. Furthermore, the term "main material" in this specification refers to a constituent material containing 50% by weight or more. For example, "the first protective film contains polycarbonate resin as its main material" means that when the total weight of the first protective film is set to 100% by weight, the polycarbonate resin contained in the first protective film accounts for 50% by weight or more in the first protective film.
[0033] The polarizer 10 of the present invention comprises: a polarizing film 13; a first protective sheet 11 laminated on one side of the polarizing film 13; a second protective sheet 12 laminated on the other side of the polarizing film; a first bonding layer 16 bonding the polarizing film 13 and the first protective sheet 11; and a second bonding layer 17 bonding the polarizing film 13 and the second protective sheet 12. Furthermore, the polarizer 10 is formed in a curved plate shape with the first protective sheet 11 having a concave surface and the second protective sheet 12 having a convex surface. The polarizer 10 is disposed in the cavity of the mold 40 of the injection molding machine with the convex side of the polarizer 10 serving as the mold side of the injection molding machine and the concave side exposed, thereby enabling the formation of a resin layer 35 (optical lens) made primarily of injection molding optical resin and bonded to the first protective sheet 11 by injection molding. Furthermore, the first bonding layer 16 is constructed primarily of a polyurethane adhesive, and according to JIS 7136:2000, when the polarizer 10 is immersed in distilled water at 80°C for 15 minutes, the haze value of the polarizer 10 is measured and meets the condition that the haze value is 0.05% or more and 1.00% or less.
[0034] Therefore, for example, when manufacturing a polarizing lens 30 equipped with a polarizer 10, such as by performing a hot bending process on the polarizer 10 under heating or by injection molding the resin layer 35 (optical lens), even if the polarizer 10 is exposed to high temperatures, it can be said that the reduction in the transparency of the polarizer 10 is reliably suppressed or prevented. Therefore, it is possible to manufacture a polarizing lens 30 with excellent reliability and a sunglasses 100 as an optical component.
[0035] The polarizer 10 of the present invention is used, for example, as a resin substrate with polarizing properties in the polarizing lens 30 of a sunglasses 100, which is an optical component of eyeglasses. Therefore, before describing the polarizer 10 of the present invention, the sunglasses 100 (the optical component of the present invention) will be described below.
[0036] Sunglasses
[0037] Figure 1 This is a perspective view showing an embodiment in which a polarizing lens incorporating the polarizer of the present invention is applied to sunglasses. Furthermore, in Figure 1 In Chinese, when sunglasses are worn on a user's head, the side of the lens facing the user's eyes is called the back side, and the side opposite to it is called the front side.
[0038] like Figure 1 As shown, the sunglasses 100 includes a frame 20 and a polarizing lens 30 (the polarizing lens of the present invention).
[0039] In addition, in this specification, "polarizing lens" includes both polarizing lenses with light-gathering function and polarizing lenses without light-gathering function.
[0040] The frame 20 is worn on the user's head and is a component used to position the polarizing lens 30 near the front of the user's eyes.
[0041] The frame 20 has a rim 21, a bridge 22, a temple 23, and a nose pad 24.
[0042] The frame portion 21 is ring-shaped and is provided for the right and left eyes respectively, with a polarizing lens 30 installed on the inner side. Thus, the user can see external information through the polarizing lens 30.
[0043] Furthermore, the bridging part 22 is rod-shaped and is located in front of the upper part of the user's nose when worn on the user's head, connecting a pair of frame parts 21.
[0044] The temple 23 is vine-like and connects to the edge on the opposite side of the position where it connects to the bridging portion 22 of each frame portion 21. When worn on the user's head, the temple 23 hangs on the user's ears.
[0045] When the sunglasses 100 are worn on the user's head, the nose pads 24 are provided on the edges of each frame 21 corresponding to the user's nose and abut against the user's nose, at which time they are shaped to correspond to the abutment portion of the user's nose. As a result, the wearing state can be stably maintained.
[0046] The materials used to construct the various parts of the frame 20 are not particularly limited; for example, various metal materials or various resin materials can be used. Furthermore, the shape of the frame 20 is not limited to the shape shown in the illustration, as long as it can be worn on the user's head.
[0047] Polarizing lenses 30 are respectively mounted on each frame portion 21. The polarizing lens 30 is light-transmitting and is a plate-shaped component that is curved outward, that is, a component with the curved convex surface facing outward and the concave surface facing the user's eye side, and has a polarizing film 10 and a resin layer 35 bonded to the polarizing film 10.
[0048] The resin layer 35 is transparent and is located on the back side of the polarizing lens 30. It functions as an optical lens and has a light-concentrating function when the polarizing lens 30 is given a light-concentrating function.
[0049] As the main material constituting the resin layer 35 (optical lens), there are no particular limitations as long as it is a resin material (optical resin for injection molding) that is transparent and can be formed by injection molding as described in the manufacturing method of the polarizing lens 30 described later. For example, various thermoplastic resins, thermosetting resins, photocurable resins and other curable resins can be used, and one or more of them can be combined.
[0050] Examples of resin materials (optical resins for injection molding) include polyolefins such as polyethylene, polypropylene, and ethylene-propylene copolymer; polyvinyl chloride, polystyrene, polyamide, polyimide, polycarbonate, poly-(4-methylpentene-1), ionomers, acrylic resins, polymethyl methacrylate, acrylonitrile-butadiene-styrene copolymer (ABS resin), acrylonitrile-styrene copolymer (AS resin), butadiene-styrene copolymer, polyethylene terephthalate (PET), and polybutylene terephthalate (PBT). Esters; polyethers, polyetherketones (PEK), polyetheretherketones (PEEK), polyetherimides, polyacetals (POM), polyphenylene ethers, polysulfones, polyethersulfones, polyphenylene sulfides, polyarylates, aromatic polyesters (liquid crystal polymers), polytetrafluoroethylene, polyvinylidene fluoride, other fluorinated resins; epoxy resins, phenolic resins, urea resins, melamine resins, silicone resins, polyurethanes, etc., or copolymers, blends, polymer alloys, etc., mainly composed of these, wherein, preferably, the resin material is the same as or identical to the resin material of the first protective sheet 11 constituting the polarizer 10 described later. Therefore, excellent adhesion can be achieved between the resin layer 35 and the polarizer 10, thus reliably suppressing or preventing the resin layer 35 from detaching from the polarizer 10.
[0051] The thickness of the resin layer 35 is not particularly limited, but is preferably 0.5 mm or more and 5.0 mm or less, and more preferably 1.0 mm or more and 3.0 mm or less. This allows for a balance between high strength and lightweight polarizing lens 30.
[0052] The polarizer 10 is a polarizing resin substrate formed by hot bending into a curved plate shape on the outer surface of the resin layer 35, i.e., the curved convex surface, corresponding to the shape of the substrate. This polarization imparts polarization to the sunglasses 100. As a result, the sunglasses 100 functions as polarized sunglasses. The polarizer 10 is constructed using the polarizer of the present invention, which will be described in detail later.
[0053] In addition, as mentioned above, the polarizing lens 30 of the sunglasses 100 can be either a polarizing lens with a light-gathering function or a polarizing lens without a light-gathering function.
[0054] Furthermore, as mentioned above, the sunglasses 100 can not only have a frame 20, but also, from the perspective of fashion and lightweight, a frameless structure.
[0055] Furthermore, in this embodiment, the optical component of the present invention is applied to sunglasses 100, but it is not limited thereto. The optical component of the present invention may be, for example, eyeglasses with prescription lenses, eyeglasses such as Iida glasses (decorative eyeglasses), goggles to protect the eyes from wind, rain, dust, medicines, etc., face shields, sun visors, and goggles for smart glasses.
[0056] In the sunglasses 100 having the above structure, the polarizing lens 30 (the polarizing lens of the present invention) provided by the sunglasses 100 is manufactured in the present invention by the manufacturing method of the polarizing lens 30 shown below.
[0057] <Manufacturing Method of Polarizing Lens>
[0058] Figure 2 This is a schematic diagram illustrating a method for manufacturing a polarizing lens having the polarizer of the present invention. Furthermore, for ease of explanation, the following will... Figure 1 The upper side is called "upper", and the lower side is called "lower".
[0059] Hereinafter, each step of the manufacturing method of the polarizing lens 30 equipped with the polarizer 10 of the present invention will be described in detail.
[0060] [1] First, a polarizing sheet 10 is prepared, consisting of a first protective sheet 11, a polarizing film 13, and a second protective sheet 12, and stacked in this order to form a flat plate. Then, protective films 50 (masking tape) are attached to both sides of the polarizing sheet 10, thereby obtaining a multilayer laminate 200 with protective films 50 attached to both sides of the polarizing sheet 10 (see reference). Figure 1 (a)).
[0061] [2] Next, as Figure 1 As shown in (b), with the prepared multilayer laminate 200, i.e., with the protective film 50 pasted on both sides of the polarizer 10, the polarizer 10 is punched along its thickness direction, so that the multilayer laminate 200 appears circular when viewed from above.
[0062] [3] Next, as Figure 1 As shown in (c), the circular multilayer laminate 200 is subjected to hot bending under heating.
[0063] Thus, the multilayer laminate 200 is formed into a curved plate shape with the first protective sheet 11 side having a curved concave surface and the second protective sheet 12 side having a curved convex surface. As a result, the polarizer 10, with the protective film 50 attached to both sides, is in the shape of a curved plate with the first protective sheet 11 side having a curved concave surface and the second protective sheet 12 side having a curved convex surface.
[0064] Furthermore, by performing a hot bending process on the multilayer laminate 200, the difference between the curvature on the MD and the curvature on the TD of the polarizer 10 is preferably set to 0.05 or more and 0.5 or less, and more preferably set to 0.05 or more and 0.2 or less.
[0065] This hot bending process is typically carried out by stamping or vacuum forming.
[0066] As described above, in this embodiment, the polarizer 10 includes a protective sheet 11 and a protective sheet 12. Considering the melting or softening temperatures of the protective sheets 11 and 12, the heating temperature (forming temperature) of the multilayer laminate 200 (polarizer 10) is preferably set to approximately 110°C or higher and 170°C or lower, more preferably to approximately 140°C or higher and 160°C or lower. By setting the heating temperature within this range, deterioration and degradation of the polarizer 10 are prevented, and the polarizer 10 is made into a softened or molten state, allowing the polarizer 10 to be reliably thermally bent. For example, it is possible to produce a bent plate-shaped polarizer 10 in which the difference between the curvature on the MD and the curvature on the TD is set within the stated range.
[0067] Furthermore, it is preferable to perform a drying process to dry the multilayer laminate 200 before the hot bending process in this step [3]. As a result, deformation of the polarizer 10 caused by moisture absorption can be reliably suppressed or prevented, and thus the hot bending process of the multilayer laminate 200, that is, the hot bending process of the polarizer 10 with the protective film 50 attached to both sides, can be performed with excellent precision. The drying of the multilayer laminate 200 can be performed, for example, by blowing hot air at a temperature of 70°C or higher and 80°C onto the surface of the multilayer laminate 200 for a period of about 5 hours to 15 hours.
[0068] [4] Next, the protective film 50 is peeled off from the thermally bent polarizer 10, i.e., the multilayer laminate 200. Then, as... Figure 2As shown in (d), the polarizer 10 is attached to the mold 40 of an injection molding machine having a curved concave surface in the shape of a curved plate, such that the curved concave surface of the mold 40 abuts against the curved convex surface of the polarizer 10, i.e., the side of the second protective sheet 12. Thus, with the curved concave surface of the polarizer 10, i.e., the side of the first protective sheet 11, exposed, the polarizer 10 is placed in the cavity 401 of the mold 40. Then, in this state, an injection molding method (injection molding) is used to injection mold a resin layer 35 made of resin material onto the curved concave surface (first protective sheet 11) of the polarizer 10. Thus, a polarizing lens 30 having a thermally bent polarizer 10 and a resin layer 35 (optical lens) is manufactured.
[0069] Furthermore, in the embedding injection molding method, injection compression molding is preferred. Injection compression molding involves injecting resin material (optical resin for injection molding) for forming the resin layer 35 into the mold 40 under low pressure, and then closing the mold 40 under high pressure and applying compressive force to the resin material. Therefore, optical anisotropy caused by molding deformation or local orientation of resin molecules during molding is less likely to occur in the resin layer 35 and even the polarizing lens 30, which are the molded body. Furthermore, by controlling the uniform application of mold compression force to the resin material, the resin material can be cooled with a certain specific volume, thus obtaining a resin layer 35 with high dimensional accuracy.
[0070] Furthermore, it is preferable to perform a drying process to dry the heat-bent polarizer 10 before forming the resin layer 35 in this process [4]. This reliably suppresses or prevents deformation caused by moisture absorption by the heat-bent polarizer 10, thus enabling the molding of the resin layer 35 on the heat-bent polarizer 10 with excellent precision. Therefore, a polarizing lens 30 having the polarizer 10 and the resin layer 35 can be obtained with higher dimensional accuracy. The drying of the polarizer 10 can be performed, for example, by blowing hot air at a temperature of 75°C or higher and 85°C or lower onto the surface of the polarizer 10 for a period of approximately 15 minutes to 2 hours.
[0071] Furthermore, depending on its application, a hard coating may be provided as the outermost layer on at least one side of the polarizing lens 30. This hard coating can be formed, for example, by applying a thermosetting resin composition to the surface of the polarizing lens 30, followed by heating and drying. In this case, the heating and drying of the resin composition can be performed, for example, by blowing hot air at a temperature of 100°C or higher and 130°C onto the surface of the polarizer 10 for a period of approximately 1 hour to 3 hours.
[0072] As the polarizer 10 used in the manufacturing method of the polarizing lens 30 described above, the polarizer 10 of the present invention is used, and thus, when the haze value of the polarizer 10 is measured after immersing it in distilled water at 80°C for 15 minutes according to JIS K 7136:2000, the haze value meets the condition of 0.05% or more and 1.00% or less. Therefore, when manufacturing the polarizing lens 30 equipped with the polarizer 10, even if the polarizer 10 is subjected to hot bending processing under heating or injection molding of the resin layer 35 (optical lens), it can be said that the reduction of the transparency of the polarizer 10 is reliably suppressed or prevented. Hereinafter, the polarizer of the present invention will be described in detail.
[0073] <Polarizer 10>
[0074] The polarizer 10 (the polarizer of the present invention) is a polarizing laminate comprising: a polarizing film 13; a first protective sheet 11 laminated on one side of the polarizing film 13; a second protective sheet 12 laminated on the other side of the polarizing film; a first bonding layer 16 bonding the polarizing film 13 and the first protective sheet 11; and a second bonding layer 17 bonding the polarizing film 13 and the second protective sheet 12. Hereinafter, each part (layer) constituting the polarizer 10 will be described.
[0075] Figure 3 This is a longitudinal sectional view showing an embodiment of the polarizer of the present invention. Furthermore, for ease of explanation, the following will... Figure 1 The upper side is called "upper", and the lower side is called "lower".
[0076] (Polarizing film 13)
[0077] The polarizing film 13 is uniaxially stretched and has an absorption axis in the direction of the uniaxial stretching, thereby having the function of extracting linearly polarized light with a polarization plane in the direction of the uniaxial stretching from the incident light (unpolarized natural light). As a result, the light passing through the polarizer 10 becomes polarized light.
[0078] The degree of polarization of the polarizing film 13 is not particularly limited, but is preferably 50% or more and 100% or less, more preferably 80% or more and 100% or less. Furthermore, the visible light transmittance of the polarizing film 13 is not particularly limited, but is preferably 10% or more and 80% or less, more preferably 20% or more and 50% or less.
[0079] As for the constituent material of this polarizing film 13, there are no particular limitations as long as it has the above-mentioned functions. Examples include polyvinyl alcohol (PVA), partially formalized polyvinyl alcohol, polyvinyl alcohol, polyvinyl butyral, polycarbonate, and partially saponified ethylene-vinyl acetate copolymer. As for the polarizing film 13, examples include thin films (membranes) that adsorb dichroic substances such as iodine or dichroic dyes onto a polymer film made of the constituent material, dye it, and then uniaxially stretch it.
[0080] The polarizing film 13 is preferably a thin film made by adsorbing iodine or dichroic dyes onto a polymer film mainly composed of polyvinyl alcohol (PVA) to dye it and then subjecting it to uniaxial stretching. Polyvinyl alcohol (PVA) is a material with excellent transparency, heat resistance, affinity for iodine or dichroic dyes used as dyeing agents, and orientation during stretching. Therefore, the polarizing film 13 made of PVA as the main material has excellent heat resistance and excellent polarization capability.
[0081] In addition, examples of the aforementioned dichroic dyes include Chlorantine FastRed, Congo Red, Brilliant Blue 6B, Benzopurpurine, Chlorazole Black BH, Direct Blue 2B, Diamine Green, Direct Yellow, Sirius Yellow, Direct Red, and Acid Black.
[0082] The thickness of the polarizing film 13 is not particularly limited, but is preferably 5 μm or more and 60 μm or less, and more preferably 10 μm or more and 40 μm or less.
[0083] (First protective piece 11)
[0084] The first protective sheet 11 is a birefringent resin layer, such as... Figure 2 (d) and Figure 3 As shown, the side of the lower surface (one side) of the polarizing film 13 is stacked to form a curved concave surface (concave surface), thereby serving as a protective layer for the lower surface of the polarizing film 13.
[0085] The first protective sheet 11 is not particularly limited as long as it has birefringence. For example, it can be mainly composed of resin materials such as polyamide resin and polycarbonate resin, and one or more of these resin materials can be combined for use. By manufacturing a first protective sheet 11 composed of at least one of polyamide resin and polycarbonate resin as the main material, the first protective sheet 11 has relatively high birefringence.
[0086] Polycarbonate resins, due to their high transparency (light transmittance) and rigidity, can improve the transparency and impact resistance of the polarizer 10. Furthermore, polycarbonate resins have a specific gravity of approximately 1.2, classifying them as lightweight among resin materials, thus enabling the polarizer 10 to be made lighter. In addition to transparency and impact resistance, polyamide resins also offer chemical resistance and stress resistance.
[0087] There are no particular limitations on the polyamide resin used; various polyamide resins can be used, such as alicyclic polyamides and semi-aromatic polyamides. Alicyclic polyamides are materials with excellent impact resistance. Therefore, the polarizer 10 can exhibit excellent impact resistance. Furthermore, semi-aromatic polyamides are materials with high elastic modulus. Therefore, a polarizer 10 with excellent resistance to bending and other stresses can be manufactured.
[0088] In addition, in this specification, semi-aromatic polyamide refers to a polyamide in which one of the dicarboxylic acid and diamine monomers constituting the polyamide is an aromatic compound and the other is an aliphatic compound, specifically, it can be represented by the following formula (1B).
[0089]
[0090] (where R in equation (1B) 1 and R 2 In this context, one side has a divalent aromatic substituent, and the other side has a divalent aliphatic substituent, where n is an integer greater than or equal to 2.
[0091] In addition, for at least one of dicarboxylic acid and diamine, polyamide can also be a copolymer containing two or more monomers (random copolymer, block copolymer, etc.).
[0092] Furthermore, R in the above equation (1B) 1 R 2 The aromatic substituents in the form are preferably substituents represented by the following formula (2B).
[0093]
[0094] (In equation (2B), l and m are independent integers greater than 0 and less than 2.)
[0095] This allows for better protection of the polarizing film 13 and improves the processability of the polarizer 10. Furthermore, by imposing a delay on the first protective film 11, delay control based on the stretching of the first protective film 11 can be performed more easily.
[0096] R in the above formula (1B) 1 R 2The aliphatic substituents in the form of the substituents are preferably hydrocarbon groups with 4 or more and 18 or less carbon atoms, more preferably hydrocarbon groups with 4 or more and 18 or less carbon atoms, and even more preferably saturated hydrocarbon groups with 4 or more and 18 or less carbon atoms.
[0097] As a result, the polarizer 10 has better processability.
[0098] Furthermore, the semi-aromatic polyamide preferably contains aromatic dicarboxylic acids and aliphatic diamines as constituent monomers. This provides better protection for the polarizing film 13 and improves the processability of the polarizer 10. Additionally, it facilitates easier stretch-based delay control.
[0099] Alicyclic polyamides have an alicyclic chemical structure within their molecules, which can be present in the main chain or in the side chain.
[0100] Examples of alicyclic polyamides include compounds in which at least one of the dicarboxylic acid or diamine, which are monomers of the polyamide, has an alicyclic chemical structure. Specifically, it can be represented by the following formula (3B).
[0101]
[0102] (wherein, in equation (3B), R) 3 R 4 Each group is independently a hydrocarbon group consisting of 4 or fewer hydrogen or carbon atoms; o is an integer between 2 and 14; p is an integer between 0 and 6; and n is an integer between 2 and 6.
[0103] There are no particular limitations on the polycarbonate resin used; various polycarbonate resins can be used, with aromatic polycarbonate resins being preferred. Aromatic polycarbonate resins have aromatic rings in their main chain, thereby resulting in superior strength of the polarizer 10.
[0104] This aromatic polycarbonate resin is synthesized, for example, through interfacial condensation reaction of bisphenol and phosgene, or transesterification reaction of bisphenol and diphenyl carbonate.
[0105] Examples of bisphenols include bisphenol A, bisphenols that are the origin of repeating units of polycarbonate as shown in formula (1A) (modified bisphenols), etc.
[0106]
[0107] (In formula (1A), X is an alkyl, aromatic or cyclic aliphatic group with 1 to 18 carbon atoms, Ra and Rb are alkyl groups with 1 to 12 carbon atoms, m and n are integers from 0 to 4, and p is the number of repeating units.)
[0108] In addition, bisphenols that form the origin of the repeating unit of the polycarbonate shown in formula (1A) can specifically include, for example, 4,4'-(pentane-2,2-diyl)diphenol, 4,4'-(pentane-3,3-diyl)diphenol, 4,4'-(butane-2,2-diyl)diphenol, 1,1'-(cyclohexanediyl)diphenol, 2-cyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 2,3-biscyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 1,1'-bis(4-hydroxy-3-methylphenyl)cyclohexane, 2,2'-bis(4-hydroxy-3-methylphenyl)propane, etc., and one or more of them can be used in combination.
[0109] Specifically, the polycarbonate resin may contain a bisphenol-type polycarbonate resin having a bisphenol-derived backbone, and preferably a bisphenol-type polycarbonate resin having a bisphenol-derived backbone as the main component. By using this bisphenol-type polycarbonate resin, the polarizer 10 exhibits superior strength.
[0110] The glass transition temperature (Tg) of the resin material contained in the first protective sheet 11 as the main material is preferably 100°C or higher and 190°C or lower, more preferably 105°C or higher and 155°C or lower. This allows for easier implementation of the hot bending process of the polarizer 10 in the aforementioned step [3]. Furthermore, when the first protective sheet 11 is made to show a delay, appropriate stretching for showing this delay can be performed. Moreover, the durability and reliability of the polarizer 10 can be further improved.
[0111] Furthermore, the first protective sheet 11 may contain other components besides the resin material contained as the main material. There are no particular limitations on such components, and examples include resin materials other than the main material, colorants such as dyes, fillers, orientation aids, stabilizers (heat stabilizers, ultraviolet absorbers, and antioxidants, etc.), plasticizers, colorants, flame retardants, antistatic agents, and viscosity modifiers, etc.
[0112] At this point, the content of resin material in the first protective sheet 11 is not particularly limited, but it is preferably 75 parts by mass or more, more preferably 85 parts by mass or more, out of 100 parts by mass of the first protective sheet 11. By setting the content of resin material within the above range, the polarizer 10 can exhibit excellent strength.
[0113] Furthermore, when delaying the display of the first protective sheet 11, it is preferable to set the delay of the first protective sheet 11 to a relatively low value.
[0114] This makes it difficult for the first protective sheet 11 to deform due to thermal shrinkage. Therefore, as... Figure 2 and Figure 3As shown, by applying the polarizer 10 to the polarizing lens 30, the polarizer 10 is used in a bent state as described above. At this time, the first protective sheet 11 is located on the concave side of the bend, and the polarizer 10 as a whole can prevent excessive deformation caused by heat. As a result, the shape deformation of the polarizing lens 30 itself caused by thermal deformation of the polarizer 10 can be reliably suppressed or prevented.
[0115] The delay of the first protective sheet 11 is preferably 0 nm or more and 500 nm or less, more preferably 50 nm or more and 350 nm or less. This allows the polarization performance of the polarizer 10 to be fully utilized. Furthermore, as described above, when the polarizer 10 is configured such that the curvature on the MD and the curvature on the TD differ, deviations in this curvature difference due to thermal shrinkage of the first protective sheet 11 can be reliably suppressed or prevented.
[0116] Furthermore, the difference in delay of the first protective sheet 11 can be reflected by making the constituent materials contained in the layer or the thickness or even the stretching ratio different.
[0117] The average thickness of the first protective sheet 11 is not particularly limited, but is preferably 0.05 mm or more and 0.5 mm or less, or preferably 0.1 mm or more and 0.4 mm or less.
[0118] The stretch ratio of the first protective sheet 11 is not particularly limited, but it is preferably set to the size of the delay, for example, 0.95 or more and 1.1 or less.
[0119] Furthermore, it is preferable that the stretching directions of the first protective sheet 11 and the polarizing film 13 are aligned. This further improves the polarization performance of the polarizer 10.
[0120] (Second protective piece 12)
[0121] The second protective film 12 is a resin layer with a lower birefringence than the first protective film 11, such as Figure 2 (d) and Figure 3 As shown, the side of the upper surface (the other side) of the polarizing film 13 becomes a curved convex surface, thereby serving as a protective layer for the upper surface of the polarizing film 13.
[0122] The second protective sheet 12 is not particularly limited as long as it has a lower birefringence than the first protective sheet 11. For example, as described above, when the first protective sheet 11 is mainly composed of resin materials such as polyamide resin and polycarbonate resin, the second protective sheet 12 is mainly composed of resin materials such as cellulose resin. By manufacturing a second protective sheet 12 mainly composed of cellulose resin, the second protective sheet 12 reliably has a lower birefringence than the first protective sheet 11.
[0123] There are no particular limitations on the cellulose-based resin used; various cellulose-based resins can be used, such as cellulose esters like triacetyl cellulose, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate; alkyl celluloses like methyl cellulose and ethyl cellulose; hydroxyalkyl celluloses like hydroxypropyl cellulose; aralkyl celluloses like benzyl cellulose; cyanalkyl celluloses like cyanoethyl cellulose; carboxylalkyl celluloses like carboxyethyl cellulose; and aminoalkyl celluloses like aminoethyl cellulose. One or more of these resins can be used in combination. Among these, cellulose esters are preferred as the cellulose resin, and triacetyl cellulose is particularly preferred. Cellulose esters (especially triacetyl cellulose) are preferred as the main material for the second protective sheet 12, which constitutes the curved convex surface of the polarizer 10, i.e., the surface opposite to the resin layer 35, due to their low birefringence, high transparency, and excellent surface appearance.
[0124] Similar to the first protective sheet 11, the glass transition temperature (Tg) of the resin material contained in the second protective sheet 12 as the main material is preferably 100°C or higher and 190°C or lower, more preferably 105°C or higher and 155°C or lower. This allows for easier implementation of the hot bending process of the polarizer 10 in the aforementioned step [3]. Furthermore, it further improves the durability and reliability of the polarizer 10.
[0125] Furthermore, the second protective sheet 12 may contain other components besides the resin material that serves as the main material. There are no particular limitations on such components; examples include resin materials other than the main material, colorants such as dyes, fillers, orientation aids, stabilizers (heat stabilizers, UV absorbers, and antioxidants, etc.), plasticizers, colorants, flame retardants, antistatic agents, and viscosity modifiers, etc.
[0126] At this point, the content of resin material in the second protective sheet 12 is not particularly limited, but it is preferably 75 parts by mass or more, more preferably 85 parts by mass or more, out of 100 parts by mass of the second protective sheet 12. By setting the content of resin material within the above range, the polarizer 10 can exhibit excellent strength.
[0127] The average thickness of the second protective sheet 12 is not particularly limited, but is preferably 0.05 mm or more and 0.5 mm or less, or preferably 0.1 mm or more and 0.4 mm or less.
[0128] (First bonding layer 16)
[0129] The first bonding layer 16 (first adhesive layer) has the function of bonding the polarizing film 13 and the first protective sheet 11, thereby improving the durability of the polarizing film 10.
[0130] In this invention, a urethane-based adhesive is used as the adhesive (or binder) constituting the first bonding layer 16. This further improves the transparency, bond strength, and durability of the first bonding layer 16, and particularly enhances its adaptability to changes in shape. Therefore, in this invention, a urethane-based adhesive is used as the adhesive constituting the first bonding layer 16.
[0131] In order to function as an adhesive, the urethane-based adhesive contains polyisocyanate compounds with isocyanate groups as its constituent materials. When these isocyanate groups react with water, such as in the air, carbon dioxide is generated via urethane, forming an amino group.
[0132] Furthermore, as described above, the first protective sheet 11 has birefringence, and in particular, when it is made of resin materials such as polyamide resin and polycarbonate resin as the main material, the first protective sheet 11 exhibits excellent gas barrier properties.
[0133] Thus, while the first protective sheet 11 exhibits excellent gas barrier properties, carbon dioxide generated in the first bonding layer 16 remains in the first bonding layer 16, resulting in the formation of bubbles in the first bonding layer 16. Furthermore, the formation of these bubbles leads to a decrease in the transparency of the first protective sheet 11. In particular, as in the aforementioned polarizing lens manufacturing method, such as when hot bending or injection molding is performed with accompanying heat treatment, the formation of these bubbles can be frequently observed when the polarizing sheet is exposed to high temperatures. Moreover, the inventors' research has clarified that this is due to the presence of isocyanate groups derived from isocyanate compounds remaining in the first bonding layer 16, which react with water, such as in the air, to generate carbon dioxide during the heat treatment.
[0134] In contrast, in this invention, according to JIS K 7136:2000, after immersing the polarizer 10 in distilled water at 80°C for 15 minutes, the haze value of the polarizer 10 is measured, satisfying the condition that the haze value is 0.05% or more and 1.00% or less. Thus, in this invention, satisfying the condition that the haze value is 0.05% or more and 1.00% or less ensures that the decrease in transparency of the first protective film 11 caused by exposure to high temperatures, such as the heat treatment, can be reliably suppressed, and the generation of bubbles in the first bonding layer 16 of the polarizer 10 can be reliably suppressed or prevented.
[0135] Furthermore, depending on the type of urethane adhesive contained in the first bonding layer 16, i.e., whether the urethane adhesive is a two-liquid crosslinking type or a single-liquid moisture crosslinking type, the generation of bubbles in the first bonding layer 16 can be suppressed, for example, as follows.
[0136] That is, when the urethane adhesive is a two-liquid crosslinked urethane adhesive containing a polyisocyanate compound and a polyol, the polyisocyanate compound reacts with the polyol to form urethane bonds between them, thereby curing the adhesive. In this two-liquid crosslinked urethane adhesive, it is generally assumed that the polyisocyanate compound reacts with moisture in the air and becomes deactivated, and that the polyisocyanate compound is contained in the adhesive at an equivalent amount of approximately 1.2 times the functional groups of the polyol. However, if the urethane adhesive contains a large amount of polyisocyanate compound relative to the polyol at such an equivalent amount of functional groups, then there is a tendency for unreacted isocyanate groups to remain in the bonding layer formed by the urethane adhesive. Therefore, if a polarizer having such a bonding layer is subjected to hot bending or injection molding with heat treatment, and the polarizer is exposed to high temperatures, bubbles caused by the generation of carbon dioxide will be generated in the bonding layer. In contrast, in this invention, the polyisocyanate compound is contained in the adhesive at approximately 1.0 times the amount of functional groups as the polyol, thereby suppressing the retention of unreacted isocyanate groups in the first bonding layer 16. Therefore, even when the polarizer 10 is exposed to high temperatures, as in the case of hot bending or injection molding accompanied by heat treatment, the generation of bubbles in the first bonding layer 16 can be reliably suppressed. Thus, the haze value can be set in the range of 0.05% or more and 1.00% or less.
[0137] Furthermore, when the urethane adhesive is a single-liquid, moisture-crosslinking urethane adhesive that contains di-terminated diisocyanates as polyisocyanates but not polyols, the di-terminated diisocyanates react with water, such as in the air, to generate carbon dioxide and an amino-containing compound. Then, the other di-terminated diisocyanates react with this amino-containing compound to form urea bonds, thereby curing the adhesive. Thus, in single-liquid, moisture-crosslinking urethane adhesives, carbon dioxide is typically generated by the reaction of di-terminated diisocyanates with water. Therefore, if a polarizer having a bonding layer derived from such a single-liquid, moisture-crosslinking urethane adhesive is subjected to heat bending or injection molding with accompanying heat treatment, and the polarizer is exposed to high temperatures, the di-terminated diisocyanates remaining in the bonding layer react with water, thereby generating bubbles in the bonding layer due to the generation of carbon dioxide. In contrast, in this invention, the first bonding layer 16 is configured to contain trifunctional isocyanates in addition to di-terminated diisocyanates. Therefore, in the first bonding layer 16, a compound with a six-membered ring is formed by the reaction of three isocyanate groups, which hinders the reaction between the two terminal diisocyanates and water. Thus, even when the polarizer 10 is exposed to high temperatures, as in the case of hot bending or injection molding accompanied by heat treatment, the generation of bubbles in the first bonding layer 16 can be reliably suppressed. As a result, the haze value can be set in the range of 0.05% or more and 1.00% or less.
[0138] Furthermore, according to JIS K 7136:2000, when measuring the haze value of the polarizer 10 after immersing it in distilled water at 80°C for 15 minutes, it is sufficient to meet the condition that the haze value is 0.05% or more and 1.00% or less. However, it is preferable that the haze value is 0.05% or more and 0.50% or less, and more preferably 0.05% or more and 0.20% or less. Therefore, it can be said that the generation of bubbles in the first bonding layer 16 of the polarizer 10 is more reliably suppressed or prevented.
[0139] Furthermore, in the polarizing lens 30 equipped with a polarizer 10 that satisfies this haze value, when the haze value of the polarizing lens 30 is measured after immersing it in distilled water at 80°C for 15 minutes according to JIS K7136:2000, the haze value is preferably 0.05% or more and 1.00% or less, more preferably 0.05% or more and 0.50% or less. Therefore, it can be said that the generation of air bubbles in the first bonding layer 16 of the polarizer 10 of the polarizing lens 30 is more reliably suppressed or prevented.
[0140] Furthermore, when measuring the adhesion force of polarizer 10 after immersing it in distilled water at 80°C for 15 minutes according to JIS K 7136:2000, the adhesion force preferably satisfies the following requirement A.
[0141] That is, for the polarizer 10, according to JIS K 6854-2, the polarizer 10 is cut into a size of 200mm in length and 25mm in width. Then, in an environment of 140°, holding one end of the first protective sheet 11 of the polarizer 10, and peeling it to a length of 10mm at a speed of 10mm / min in a 180° direction, the adhesion force of the first protective sheet 11 to the polarizer 13 is preferably 40N / 25mm or more and 500N / 25mm or less, more preferably 50N / 25mm or more and 300N / 25mm or less, and even more preferably 80N / 25mm or more and 250N / 25mm or less (Requirement A).
[0142] When bubbles are generated on the polarizer 10, as described above, there is a tendency for the transparency of the polarizer 10 to decrease, and furthermore, there is a tendency for the adhesion of the first bonding layer 16 to decrease. In contrast, in this invention, since the polarizer 10 can be made to meet requirement A more easily, cracks can be reliably suppressed or prevented on the polarizer 10 during hot bending or injection molding with accompanying heat treatment, and the decrease in the adhesion of the first bonding layer 16 can be reliably suppressed or prevented. Therefore, it can be said that the generation of bubbles in the first bonding layer 16 is reliably suppressed.
[0143] Furthermore, the thickness of the first bonding layer 16 is not particularly limited, but is preferably 5 μm or more and 60 μm or less, and more preferably 10 μm or more and 40 μm or less. This allows the first bonding layer 16 to reliably perform its function.
[0144] (Second bonding layer 17)
[0145] The second bonding layer 17 (second adhesive layer) has the function of bonding the polarizing film 13 and the second protective sheet 12, thereby improving the durability of the polarizing film 10.
[0146] The adhesive (or binder) constituting the second bonding layer 17 is not particularly limited, and examples include water-soluble adhesives such as acrylic adhesives, urethane adhesives, epoxy adhesives, silicone adhesives, and polyvinyl alcohol adhesives. Among these, urethane adhesives are preferred. This further improves the transparency, adhesive strength, and durability of the second bonding layer 17, and provides particularly excellent adaptability to shape changes.
[0147] Furthermore, as mentioned above, the birefringence of the second protective sheet 12 is lower than that of the first protective sheet 11. If it is mainly composed of resin materials such as cellulose esters (especially triacetyl cellulose), the second protective sheet 12 exhibits excellent air permeability. Therefore, even if a urethane-based adhesive is used as the adhesive constituting the second bonding layer 17, and carbon dioxide is generated in the second bonding layer 17, the carbon dioxide can be discharged to the outside of the polarizer 10 via the second protective sheet 12. Therefore, the generation of air bubbles in the second bonding layer 17 can be reliably suppressed or prevented. However, from the viewpoint of more reliably preventing the generation of air bubbles in the second bonding layer 17, when using a urethane-based adhesive as the adhesive constituting the second bonding layer 17, it is preferable to use the same or similar urethane-based adhesive as the one described in the first bonding layer 16. This allows for a more significant effect in preventing the generation of air bubbles in the second bonding layer 17.
[0148] The thickness of the second bonding layer 17 is not particularly limited, but is preferably 5 μm or more and 60 μm or less, and more preferably 10 μm or more and 40 μm or less. This reliably imparts the function of the second bonding layer 17.
[0149] Furthermore, the total thickness of the polarizer 10 is preferably 0.1 mm or more and 2 mm or less.
[0150] In addition, apart from the case of hot bending or injection molding accompanied by heat treatment, in order to make the polarizing lens 30 have a hard coating as its outermost layer, even if a hard coating is formed on the polarizer 10 or in the case of envisioning the sunglasses 100 being placed in a high-temperature space such as the dashboard of a car for a long time, in the present invention, the generation of bubbles in the first bonding layer 16 of the polarizer 10 can be reliably suppressed as described above, so that the haze value can be set in the range of 0.05% or more and 1.00% or less.
[0151] The polarizer, polarizing lens, and optical components of the present invention have been described above, but the present invention is not limited thereto.
[0152] For example, the various parts constituting the polarizer of the present invention can be replaced by any structure that can perform the same function.
[0153] Furthermore, in addition to the structure described above, the polarizer of the present invention can also be fitted with any additional structures.
[0154] More specifically, for example, the polarizer of the present invention may also include an intermediate layer and a diopter adjustment layer for adjusting the diopter of the lens.
[0155] [Example]
[0156] The present invention will now be described in detail with reference to embodiments, but the present invention is not limited thereto.
[0157] 1. Manufacturing of polarizers
[0158] (Example 1)
[0159] First, a polyvinyl alcohol (PVA) film was stretched in a water bath while being dyed with an aqueous solution containing dissolved dye, and then treated with boric acid. The treated PVA film was then washed with water and dried. This yielded a polarizing film 13 with a thickness of 35 μm.
[0160] On the other hand, using polycarbonate resin (manufactured by Mitsubishi Gas Chemical Company, Inc., "Iupilon E-2000"), a sheet-like first protective sheet 11 with a thickness of 0.2 mm and a delay of 100 nm was obtained by extrusion molding using a vented single-screw extruder.
[0161] Furthermore, as the second protective sheet 12, which is mainly composed of triacetyl cellulose, FUJITAC (manufactured by Fujifilm Investment Co., Ltd., “TD80UL”, 80mm thick) was prepared.
[0162] Next, on one side of the first protective sheet 11, a two-liquid moisture-curing polyurethane adhesive (main agent (polyol): "TAKELAC A-520" manufactured by Mitsui Chemicals, Inc., curing agent (polyisocyanate compound): "TAKENATE A-50" manufactured by Mitsui Chemicals, Inc., functional group equivalents, main agent: curing agent = 1.0:1.0) was applied using a bar coater, so that the thickness of the first bonding layer 16 after drying is 20 μm. Furthermore, on one side of the second protective sheet 12, a two-liquid moisture-curing polyurethane adhesive (main agent (polyol): manufactured by Mitsui Chemicals, Inc., "TAKELAC A-520", curing agent (polyisocyanate compound): manufactured by Mitsui Chemicals, Inc., "TAKENATE A-50", functional group equivalents, main agent: curing agent = 1.0:1.0) was applied using a bar coater, so that the thickness of the second bonding layer 17 after drying is 20 μm.
[0163] Next, the first protective sheet 11 coated with the first adhesive and the second protective sheet 12 coated with the second adhesive are placed in an oven and heated until the solvent components in the first adhesive and the second adhesive are dried. Thus, a first laminate with a first bonding layer 16 (first adhesive layer) laminated on one side of the first protective sheet 11 is obtained, and a second laminate with a second bonding layer 17 (second adhesive layer) laminated on one side of the second protective sheet 12 is obtained.
[0164] Then, on one side of the polarizing film 13, the first laminate is stacked on the polarizing film 13 in such a way that the first bonding layer 16 contacts it, and on the other side of the polarizing film 13, the second laminate is stacked on the polarizing film 13 in such a way that the second bonding layer 17 contacts it, thereby obtaining the polarizer 10 of Example 1. At this time, the rubber roller of the laminator is used to press the first laminate, the polarizing film 13 and the second laminate respectively, so that the total thickness of the polarizer 10 is 0.75 mm. In addition, after obtaining the polarizer 10, it is cured at 30°C for 1 week to completely cure the first adhesive contained in the first bonding layer 16 and the second adhesive contained in the second bonding layer 17.
[0165] (Examples 2-6, Comparative Examples 1-3)
[0166] As the urethane-based adhesive used to form the first bonding layer 16 of the polarizer 10, an adhesive with functional group equivalence relationships shown in Table 1 was used. Otherwise, similar to Example 1, polarizers 10 of Examples 2 to 6 and Comparative Examples 1 to 3 were obtained.
[0167] In addition, as a single-liquid moisture-crosslinking polyurethane adhesive, an adhesive containing a two-terminal diisocyanate (Mitsui Chemicals, Inc., "LA2355") and a trifunctional isocyanate (DIC Corporation, "DN-902S") was used.
[0168] 2. Evaluation
[0169] The polarizers of each embodiment and each comparative example were evaluated using the following methods.
[0170] <1> Determination of the haze value of polarizer
[0171] First, the polarizers of each embodiment and each comparative example were immersed in distilled water at 80°C for 15 minutes according to JIS K 7136:2000. Then, the haze value of the polarizer was measured using a haze meter (NIPPON DENSHOKUINDUSTRIES CO.,LTD., “NDH4000”).
[0172] <2> Determination of the sealing force of the first protective film in a polarizer
[0173] First, the polarizers of each embodiment and comparative example were immersed in distilled water at 80°C for 15 minutes according to JIS K 7136:2000. Then, the adhesion force of the first protective sheet to the polarizing film was measured using a tensile testing machine (Shimadzu Corporation, "AG-10kNXplus") when the polarizer was cut into pieces of 200mm in length and 25mm in width according to JIS K 6854-2, and then peeled to a length of 10mm at a speed of 10mm / min in a 180° direction while holding one end of the first protective sheet of the polarizer at 140°C.
[0174] <3> Determination of haze value of polarizing lens
[0175] First, for the polarizers of each embodiment and each comparative example, protective films made of polyolefin were laminated on both sides of the polarizer, namely the side of the first protective film opposite to the polarizing film and the side of the second protective film opposite to the polarizing film, respectively.
[0176] Next, the polarizer is punched to a diameter of 8cm and then hot-bent at 150°C for 10 minutes using a REMA (vacuum forming machine) (CR-32 type) to produce a polarizer with a radius of curvature R1 of 80.5mm on the MD and a radius of curvature R2 of 87.2mm on the TD.
[0177] Next, after peeling off the protective film from the heat-bent polarizer 10, the following steps are taken: Figure 2 (d) The mold 40 is used to form a resin layer made of injection molding optical resin (manufactured by Mitsubishi Gas Chemical Company, Inc., "H-3000") on the curved concave side (first protective sheet) of the polarizer 10 by injection molding, thereby obtaining a polarizing lens.
[0178] Then, the obtained polarizing lenses were immersed in distilled water at 80°C for 15 minutes according to JIS K 7136:2000. The haze value of the polarizing lenses was then measured using a haze meter (NIPPON DENSHOKU INDUSTRIES CO.,LTD., “NDH4000”).
[0179] <4> Evaluation of whether air bubbles are generated in the polarizing lens
[0180] First, for the polarizers of each embodiment and each comparative example, protective films made of polyolefin were laminated on both sides of the polarizer, namely the side of the first protective film opposite to the polarizing film and the side of the second protective film opposite to the polarizing film, respectively.
[0181] Next, the polarizer is punched to a diameter of 8cm and then hot-bent at 150°C for 10 minutes using a REMA (vacuum forming machine) (CR-32 type) to produce a polarizer with a radius of curvature R1 of 80.5mm on the MD and a radius of curvature R2 of 87.2mm on the TD.
[0182] Next, after peeling off the protective film from the heat-bent polarizer 10, the following steps are taken: Figure 2 (d) The mold 40 is used to form a resin layer made of injection molding optical resin (manufactured by Mitsubishi Gas Chemical Company, Inc., "H-3000") on the curved concave side (first protective sheet) of the polarizer 10 by injection molding, thereby obtaining a polarizing lens.
[0183] Then, visually observe whether there are bubbles in the polarizing lens. The case where no bubbles are confirmed is rated as A, the case where some bubbles are confirmed is rated as B, the case where bubbles are definitely confirmed is rated as C, and the case where bubbles are more obviously confirmed is rated as D.
[0184] The evaluation results of the polarizers of each embodiment and comparative example obtained as described above are shown in Table 1 below.
[0185] [Table 1]
[0186]
[0187] As shown in Table 1, in each embodiment, the haze value in the polarizer is satisfied to be 0.05% or more and 1.00% or less. Thus, it is shown that when a polarizing lens is obtained, the generation of bubbles can be reliably suppressed or prevented in the polarizer of the polarizing lens.
[0188] In contrast, in each comparative example, the condition that the haze value in the polarizer is more than 0.05% and less than 1.00% cannot be met. As a result, it is shown that when a polarizing lens is obtained, the generation of bubbles is confirmed in the polarizer of the polarizing lens.
[0189] Industrial availability
[0190] According to the present invention, when the haze value of a polarizer is measured after immersing it in distilled water at 80°C for 15 minutes in accordance with JIS 7136:2000, the haze value satisfies the condition of being 0.05% or more and 1.00% or less. Therefore, for example, in cases such as hot bending of the polarizer under heating for manufacturing a polarizing lens or injection molding of an optical lens, even when the polarizer is exposed to high temperatures, it can be said that the reduction in the transparency of the polarizer is reliably suppressed or prevented. Therefore, it is possible to manufacture polarizing lenses and optical components with excellent reliability. Therefore, the present invention has industrial applicability.
Claims
1. A polarizer comprising: a polarizing film uniaxially stretched and having an absorption axis in the direction of the uniaxial stretching; a first protective sheet stacked on one side of the polarizing film and having birefringence; a second protective sheet stacked on the other side of the polarizing film and having lower birefringence than the first protective sheet; a first bonding layer bonding the polarizing film and the first protective sheet; and a second bonding layer bonding the polarizing film and the second protective sheet, characterized in that... The first bonding layer and the second bonding layer are bonding layers constructed primarily of polyurethane adhesives. The polyurethane adhesive used as the main material of the first bonding layer is either a two-liquid crosslinking polyurethane adhesive containing a polyisocyanate compound and a polyol, or a single-liquid moisture crosslinking polyurethane adhesive containing two-terminated diisocyanates as polyisocyanates without polyols. The polyurethane adhesive used as the main material of the second bonding layer is a two-liquid crosslinking polyurethane adhesive comprising a polyisocyanate compound and a polyol. The dual-liquid crosslinking polyurethane adhesive comprises the polyol and the polyisocyanate compound in a functional group equivalence ratio of 1.0:1.3 to 1.3:1.
0. The single-liquid moisture-crosslinking polyurethane adhesive contains the two-terminal diisocyanate and trifunctional isocyanate in a functional group equivalence ratio of 1.0:1.3 to 1.3:1.
0. According to JIS K 7136:2000, after immersing the polarizer in distilled water at 80°C for 15 minutes, the haze value of the polarizer is measured to be above 0.05% and below 1.00%.
2. The polarizer according to claim 1, wherein, According to JIS K 7136:2000, after immersing the polarizer in distilled water at 80°C for 15 minutes, the adhesion force of the polarizer is measured, and the adhesion force satisfies the following requirement A. Requirement A: According to JIS K 6854-2, the polarizer is cut into pieces with a length of 200mm and a width of 25mm. Then, at 140°C, one end of the first protective sheet of the polarizer is grasped and peeled at a speed of 10mm / min in a 180° direction to a length of 10mm. The adhesion force of the first protective sheet to the polarizing film is measured to be more than 40N / 25mm and less than 500N / 25mm.
3. The polarizer according to claim 1 or 2, wherein, The first protective sheet is a protective sheet made primarily of polycarbonate resin or polyamide resin, and the second protective sheet is a protective sheet made primarily of cellulose resin.
4. The polarizer according to claim 1 or 2, wherein, The polarizing film is made primarily of polyvinyl alcohol resin or its derivatives, and contains dichroic dyes and is uniaxially stretched.
5. The polarizer according to claim 1 or 2, wherein, The polarizer is formed into a curved plate shape with the first protective sheet forming a concave surface and the second protective sheet forming a convex surface. The polarizer is placed in the cavity of the mold of the injection molding machine with the convex side of the polarizer becoming the mold side of the injection molding machine and the concave side exposed, so as to form an optical lens made of injection molding optical resin as the main material and bonded to the first protective sheet by injection molding.
6. A polarizing lens, characterized in that, The polarizing lens comprises: The polarizer according to claim 1 or 2, wherein the polarizer is formed into a curved plate shape by means that the first protective sheet forms a concave surface and the second protective sheet forms a convex surface; and An optical lens is formed by joining the concave surface to the first protective sheet and by injection molding.
7. The polarizing lens according to claim 6, wherein, According to JIS K 7136:2000, after immersing the polarizing lens in distilled water at 80°C for 15 minutes, the haze value of the polarizing lens is measured to be above 0.05% and below 1.00%.
8. The polarizing lens according to claim 6, wherein, When using the polarizing lens, the concave surface of the first protective sheet side of the polarizing film faces the user's eye side.
9. The polarizing lens according to claim 6, wherein, In the polarizing lens, the difference between the radian on MD and the radian on TD is greater than 0.05 and less than 0.
5.
10. An optical component, characterized in that, The optical component includes the polarizing lens as described in claim 6.
Citation Information
Patent Citations
Polarizing layer laminate and its manufacturing method
JP2009294445A
Polarizing laminate and process for producing the same
CN101598831A