A method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings

By employing reduction roasting, magnetic separation, gravity separation, acid leaching, and precipitation processes, the problem of unrecovered metals in copper smelting slag flotation tailings has been solved, achieving efficient and comprehensive utilization of copper smelting slag flotation tailings, producing a variety of high-quality products, reducing environmental pressure, and improving economic benefits.

CN117299348BActive Publication Date: 2026-11-17GANSU KANGXING TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311242627.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-25
Publication Date
2026-11-17
Estimated Expiration
2043-09-25

AI Technical Summary

Technical Problem

In existing technologies, copper smelting slag flotation tailings contain lead, zinc, iron and other metals that can be comprehensively recovered but cannot be effectively recovered, resulting in resource waste and increased environmental pressure.

Method used

By employing processes such as reduction roasting, magnetic separation, gravity separation, acid leaching, precipitation, and concentration crystallization, metals such as copper, iron, lead, and zinc are separated and recovered to produce high-quality iron concentrate, lead concentrate, copper sulfate, zinc sulfate, and other products. Weakly magnetic iron minerals and silicate minerals are then used to manufacture cement and building materials.

Benefits of technology

This technology enables the efficient and comprehensive recycling of copper smelting slag flotation tailings, reducing resource waste, minimizing environmental pollution, improving economic efficiency, and producing a variety of high-quality products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117299348B_ABST
    Figure CN117299348B_ABST
Patent Text Reader

Abstract

This invention discloses a method for the efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings. The method employs a reduction roasting and magnetic-gravity combined separation process to first recover iron and lead, producing high-quality iron and lead concentrates, while simultaneously yielding three intermediate products: weakly magnetic iron minerals, copper-zinc metallic minerals, and silicate minerals. Then, copper and zinc are separated and recovered using chemical leaching, precipitation separation, and concentration crystallization, producing industrial copper sulfate and industrial zinc sulfate products. Finally, the weakly magnetic iron minerals and silicate minerals are used as additives in cement production to produce silicate cement. The method disclosed in this invention has advantages such as simple process, low operating cost, and high comprehensive recovery and utilization rate, which not only brings good economic benefits but also solves environmental protection and mine environmental management problems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of mineral processing technology, specifically relating to a method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings. Background Technology

[0002] During the smelting process of copper ore containing mainly copper sulfide, a large amount of copper smelting slag is generated. Due to the limitations of copper smelting technology, the copper smelting slag still contains a large amount of copper metal, resulting in the waste of copper.

[0003] With the continuous advancement of mining processing technology, copper metal in copper smelting slag is typically recovered secondary through flotation recovery technology, ensuring full utilization of the copper metal in the smelting slag. The main chemical components of copper smelting flotation tailings are: Cu 0.1%–0.6%, S 0.5%–1.5%, Fe 30.0%–46%, Pb 0.4%–1.1%, Zn 1.5%–3.5%, Co 0.01%–0.1%, MgO 1.0%–1.5%, CaO 0.8%–3.0%, Al₂O₃ 0.5%–2.0%, and SiO₂ 28%–40%. The main mineral composition of copper smelting slag flotation tailings is as follows: 0.11%–0.25% porphyritic chalcopyrite, 0.08%–0.12% copper-lead sulfides, 0.05%–1.10% copper-zinc sulfides, 0.05%–2.0% zinc-copper sulfides, 3.0%–7.0% iron oxides, 0.10%–0.50% galena, 0.02%–1.50% pyrrhotite, 7.0%–18.0% ferrophosphate, 60%–70% fir olivine, and 1.0%–3.0% other minerals.

[0004] It can be seen that the tailings after copper smelting slag flotation and recycling still contain metals such as lead, zinc, and iron that can be comprehensively recycled but have not been comprehensively recovered. This not only wastes resources, but also puts great pressure on environmental governance due to the long-term stockpiling of copper smelting slag flotation tailings. Summary of the Invention

[0005] To address the problems existing in the prior art, this invention provides a method for the efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings, specifically including the following:

[0006] A method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings includes the following steps:

[0007] (1) Reduction roasting: The copper smelting slag flotation tailings and reducing agent are roasted at a temperature of 600-800℃ (e.g., 620℃, 650℃, 680℃, 700℃, 750℃, 780℃, etc.) to obtain roasted sand;

[0008] (2) Magnetic separation: Cool the roasted sand and perform at least one magnetic separation to obtain iron-containing materials and the first tailings;

[0009] (3) Re-separation: The first tailings are subjected to at least one re-separation to obtain concentrate and second tailings;

[0010] (4) First acid leaching: The concentrate is leached in a dilute sulfuric acid solution with a mass concentration of 10-20% (e.g., 12%, 14%, 16%, 18%), and the leaching liquid-solid ratio is controlled at (1-2):1 (e.g., 1.2:1, 1.4:1, 1.6:1, 1.8:1). After leaching, the solid and liquid are separated to obtain the first filtrate and the first filter residue.

[0011] (5) Primary precipitation: Adjust the pH of the first filtrate to 7-10 (e.g., 7.5, 8, 8.5, 9, 9.5, etc.) to carry out the precipitation reaction. After the reaction is completed, the solid and liquid are separated to obtain the second filtrate and the second filter residue.

[0012] (6) Copper-zinc separation: Add sodium hydroxide solution with a mass concentration of 25%-40% (e.g., 26%, 30%, 34%, 36%, 38%, etc.) to the second filter residue to carry out a dissolution reaction. After the reaction is completed, the solid and liquid are separated to obtain the third filtrate and the third filter residue.

[0013] (7) Secondary precipitation: Adjust the pH of the third filtrate to 7-10 (e.g., 7.5, 8, 8.5, 9, 9.5, etc.) to carry out the precipitation reaction. After the reaction is completed, the solid and liquid are separated to obtain the fourth filtrate and the fourth filter residue.

[0014] Preferably, the copper smelting slag flotation tailings in step (1) are 80% or more (e.g., 82%, 85%, 90%, 95%, etc.) of particles with a particle size of less than 400 mesh, and the reducing agent is coke.

[0015] Preferably, the magnetic separation in step (2) includes:

[0016] Primary magnetic separation: After the roasted sand is cooled, it is subjected to primary magnetic separation in a magnetic field with a magnetic induction intensity of 1000-2000 Gauss (e.g., 1200 Gauss, 1400 Gauss, 1600 Gauss, 1800 Gauss, etc.) to obtain iron concentrate with an iron content of >60% and tailings.

[0017] Secondary magnetic separation: The tailings are subjected to secondary magnetic separation in a magnetic field with a magnetic induction intensity of 4000-14000 Gauss (e.g., 5000 Gauss, 6000 Gauss, 8000 Gauss, 10000 Gauss, 12000 Gauss, 13000 Gauss, etc.) to obtain weakly magnetic iron-bearing minerals and the first tailings.

[0018] Preferably, the reselection in step (3) includes:

[0019] Primary gravity separation: The first tailings are subjected to primary gravity separation to obtain heavy metal concentrate and primary tailings; the primary gravity separation is preferably carried out by a shaking table; the heavy metal concentrate contains Pb, Zn and Cu heavy metals, and the primary tailings are silicate minerals.

[0020] Secondary gravity separation: The heavy metal concentrate is subjected to secondary gravity separation to obtain lead concentrate with a lead content >40% and secondary tailings; the primary gravity separation is preferably carried out by shaking table.

[0021] Three-stage gravity separation: The secondary tailings are subjected to three-stage gravity separation to obtain a concentrate containing Zn and Cu and a second tailings. The primary gravity separation is preferably carried out by a centrifugal concentrator. The second tailings are silicate minerals.

[0022] Preferably, the method further includes: combining weakly magnetic iron-bearing minerals, primary tailings, and secondary tailings to produce cement.

[0023] Preferably, the method for producing cement is as follows: combining weakly magnetic iron-containing minerals, primary tailings, and secondary tailings, adding limestone and clay, and grinding until more than 65% (e.g., 70%, 74%, 76%, 78%, 80%, etc.) of the particles have a particle size of less than 400 mesh; then calcining at a temperature of 400-1200℃ (e.g., 600℃, 700℃, 800℃, 900℃, 1000℃, 1100℃, etc.) to obtain cement clinker; adding gypsum to the cement clinker and grinding until more than 85% (e.g., 86%, 88%, 90%, 92%, 95%, etc.) of the particles have a particle size of less than 400 mesh to obtain silicate cement product.

[0024] Preferably, the heavy metal concentrate and concentrate produced by the gravity separation can also be sold as raw materials and intermediate products; the primary tailings and the second tailings are silicate minerals, which can also be used to make bricks and general building materials; the weakly magnetic iron minerals can be used to make thermal insulation materials.

[0025] Preferably, the method for adjusting the pH of the first filtrate to alkaline in step (5) is to add sodium hydroxide solution to the first filtrate.

[0026] Preferably, step (6) further includes: adding dilute sulfuric acid solution to the third filter residue, and obtaining copper sulfate solution after reaction; concentrating and crystallizing the copper sulfate solution to obtain (industrial) copper sulfate.

[0027] Preferably, the method further includes step (8) secondary acid dissolution: sulfuric acid solution is added to the fourth filter residue, and zinc sulfate solution is obtained after reaction, and then concentrated and crystallized to obtain (industrial) zinc sulfate.

[0028] The beneficial effects of this invention are:

[0029] This invention discloses a method for the efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings. The material processed is the tailings produced after copper smelting slag has undergone mineral processing to recover copper metal minerals (i.e., copper smelting slag flotation tailings). This tailings contains a small amount of copper and a certain amount of iron, lead, zinc, and a large amount of silicate minerals, thus possessing value for mineral resource recycling. Based on the physicochemical properties of these minerals, this invention employs a reduction roasting and magnetic-gravity combined separation process to first recover iron and lead, producing high-quality iron concentrate and lead concentrate, while simultaneously producing three intermediate products: weakly magnetic iron minerals, copper-zinc metal minerals, and silicate minerals. Then, copper and zinc are separated and recovered using chemical leaching, precipitation separation, and concentration crystallization methods, producing industrial copper sulfate and industrial zinc sulfate products. Finally, the produced weakly magnetic iron minerals and silicate minerals are used as raw materials for cement production, producing silicate cement. Furthermore, depending on production, operation, and market conditions, the copper-, lead-, and zinc-containing minerals produced by gravity separation can be sold as raw materials and intermediate products; the silicate minerals produced by gravity separation can be used for brick making and general building materials; and the weakly magnetic iron minerals produced by magnetic separation can be used to make insulation materials, thereby improving the economic benefits of their processing and utilization. The method disclosed in this invention produces eight products: iron concentrate with an iron content >60%, lead concentrate with a lead content >40%, industrial copper sulfate, industrial zinc sulfate, silicate cement, building bricks, general building materials, and insulation materials.

[0030] This invention discloses a method for the efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings. Utilizing mineral processing and chemical methods, it achieves efficient and comprehensive recovery and utilization of copper smelting slag tailings, reducing smelting waste emissions, mitigating environmental pollution, and promoting sustainable economic development. This method has advantages such as simple process, low operating cost, and high comprehensive recovery and utilization rate, not only bringing good economic benefits but also solving environmental protection and mine environmental management issues. Attached Figure Description

[0031] Figure 1 This is a simplified process flow diagram of the method disclosed in the embodiments of the present invention;

[0032] Figure 2 This is a simplified process flow diagram of the method disclosed in the embodiments of the present invention. Detailed Implementation

[0033] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. The embodiments shown below do not limit the scope of the invention as described in the claims. Furthermore, the complete contents of the configurations illustrated in the following embodiments are not limited to those necessary for the solution of the invention as described in the claims.

[0034] Reference Appendix Figure 1 A method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings includes the following steps:

[0035] (1) Reduction roasting: The copper smelting slag flotation tailings and reducing agent are roasted at a temperature of 600-800℃ to obtain roasted sand; the copper smelting slag flotation tailings are more than 80% particles with a particle size of less than 400 mesh, and the reducing agent is coke.

[0036] (2) Magnetic separation:

[0037] Primary magnetic separation: After cooling the roasted sand, it is subjected to primary magnetic separation in a magnetic field with a magnetic induction intensity of 1000-2000 Gauss to obtain iron concentrate with an iron content of >60% and tailings.

[0038] Secondary magnetic separation: The tailings are subjected to secondary magnetic separation in a magnetic field with a magnetic induction intensity of 4000 to 14000 Gauss to obtain weakly magnetic iron-bearing minerals and the first tailings.

[0039] (1) Reselect:

[0040] Primary gravity separation: The first tailings are subjected to primary gravity separation to obtain heavy metal concentrate and primary tailings; the primary gravity separation is preferably carried out by a shaking table; the heavy metal concentrate contains Pb, Zn and Cu heavy metals, and the primary tailings are silicate minerals.

[0041] Secondary gravity separation: The heavy metal concentrate is subjected to secondary gravity separation to obtain lead concentrate with a lead content >40% and secondary tailings; the primary gravity separation is preferably carried out by shaking table.

[0042] Three-stage gravity separation: The secondary tailings are subjected to three-stage gravity separation to obtain a concentrate containing Zn and Cu and a second tailings. The primary gravity separation is preferably carried out by a centrifugal concentrator. The second tailings are silicate minerals.

[0043] Cement is produced by combining weakly magnetic iron-bearing minerals, primary tailings, and secondary tailings. The weakly magnetic iron-bearing minerals, primary tailings, and secondary tailings are combined, and cement raw materials are added. The mixture is then ground until more than 65% of the particles have a diameter less than 400 mesh. This is followed by calcination at 400-1200℃ to obtain cement clinker. Gypsum is then added to the cement clinker and ground until more than 85% of the particles have a diameter less than 400 mesh to obtain silicate cement products. Furthermore, the primary and secondary tailings, being silicate minerals, can also be used to make bricks and general building materials; the weakly magnetic iron minerals can be used to make thermal insulation materials.

[0044] (4) First acid leaching: The concentrate is leached in a dilute sulfuric acid solution with a mass concentration of 10-20%, and the solid-solid ratio of the leaching solution is controlled to be (1-2):1. After leaching, the solid and liquid are separated to obtain the first filtrate and the first filter residue.

[0045] (5) Primary precipitation: Add sodium hydroxide solution to the first filtrate to adjust the pH of the first filtrate to alkaline and carry out the precipitation reaction. After the reaction is completed, the solid and liquid are separated to obtain the second filtrate and the second filter residue.

[0046] (6) Copper-zinc separation: Sodium hydroxide solution is added to the second filter residue to carry out a dissolution reaction. After the reaction is completed, the solid and liquid are separated to obtain the third filtrate and the third filter residue. Dilute sulfuric acid solution is added to the third filter residue to obtain copper sulfate solution after the reaction. The copper sulfate solution is concentrated and crystallized to obtain (industrial) copper sulfate.

[0047] (7) Secondary precipitation: Adjust the pH of the third filtrate to alkaline and carry out the precipitation reaction. After the reaction is completed, the solid and liquid are separated to obtain the fourth filtrate and the fourth filter residue.

[0048] (8) Secondary acid dissolution: Add sulfuric acid solution to the fourth filter residue, and after the reaction, zinc sulfate solution is obtained. Then concentrate and crystallize to obtain (industrial) zinc sulfate.

[0049] Reference Appendix Figure 2 The method disclosed in this invention is used to comprehensively recover and utilize the tailings from copper smelting slag beneficiation in a company's mine. The process includes the following steps:

[0050] (1) The copper smelting slag flotation tailings are uniformly fed into the roasting furnace for reduction roasting. The roasting temperature is controlled at 600℃~800℃, the reducing agent is coke, and the roasted sand produced is cooled naturally.

[0051] (2) The naturally cooled roasted sand is fed into a two-stage magnetic separation operation. The first stage of magnetic separation is a weak magnetic separator with a magnetic induction intensity of 1000-2000 Gauss. The produced concentrate is iron concentrate with an iron content of >60%. The tailings from the first stage of magnetic separation are fed into the second stage of magnetic separation operation. The second stage of magnetic separation is a strong magnetic separator with a magnetic induction intensity of 4000-14000 Gauss. The produced magnetic concentrate is a weak magnetic iron mineral, which can be used as an auxiliary material and raw material for cement production. The produced tailings are then fed into a gravity separation operation.

[0052] (3) The tailings produced by the second stage magnetic separation are fed into the third stage gravity separation operation. The first stage gravity separation operation uses a shaking table, and the produced concentrate is copper-lead-zinc heavy metal minerals, while the produced tailings are silicate minerals, which can be used as auxiliary materials and raw materials for cement production. The concentrate produced by the first stage gravity separation enters the second stage gravity separation operation, which uses a shaking table, and the produced concentrate is lead concentrate with a lead content of >40%. The produced tailings enter the third stage gravity separation operation, which uses a centrifugal concentrator, and the produced concentrate is copper-zinc minerals, while the produced tailings are silicate minerals, which can be used as auxiliary materials and raw materials for cement production.

[0053] (4) The concentrate produced by the third stage gravity separation is leached with dilute sulfuric acid with a leaching liquid-solid ratio of 1 to 2:1. The leaching liquid is then subjected to solid-liquid separation. The resulting leaching residue is sent to the cement production process. The resulting leaching liquid is a copper-zinc sulfate solution.

[0054] (5) Add sodium hydroxide to the leachate to adjust the pH of the solution to weakly alkaline. Copper sulfate and zinc sulfate in the solution react to produce copper hydroxide and zinc hydroxide precipitates. After filtering the solution, the filter residue produced is copper hydroxide and zinc hydroxide. The filtrate is returned to the precipitation operation for reuse.

[0055] (6) Add sodium hydroxide solution to the filter residue containing copper hydroxide and zinc hydroxide. The zinc hydroxide dissolves to form sodium zincate. After filtration, the filter residue is copper hydroxide and the filtrate is sodium zincate solution.

[0056] (7) Add dilute sulfuric acid to the filter residue containing copper hydroxide to dissolve it. After the copper hydroxide precipitate dissolves, copper sulfate solution is generated. Then, after concentration and crystallization, industrial copper sulfate product is generated.

[0057] (8) Add sulfuric acid to the sodium zincate filtrate to adjust the pH to weak alkalinity, react to produce zinc hydroxide precipitate, filter and filter residue is zinc hydroxide precipitate, and return the filtrate to the sodium zincate precipitation operation for reuse.

[0058] (9) Add sulfuric acid to the filter residue containing zinc hydroxide to react. After the zinc hydroxide precipitate dissolves, zinc sulfate solution is generated. After concentration and crystallization, industrial zinc sulfate product is generated.

[0059] (10) After combining the silicate minerals produced by gravity separation and the weakly magnetic iron minerals produced by magnetic separation, a certain amount of cement raw materials are added, and after mixing evenly, the mixture is finely ground and calcined at high temperature. Then, a certain amount of gypsum is added to the calcined material and finely ground again. After fine grinding, silicate cement products are produced.

[0060] (11) The silicate minerals produced by gravity separation can also be used to make bricks and general building materials; the weakly magnetic iron minerals produced by magnetic separation can also be used to make thermal insulation materials.

[0061] After the above processing steps, eight products were obtained: iron concentrate containing 58%–65% iron, lead concentrate containing 40%–50% lead, industrial copper sulfate, industrial zinc sulfate, silicate cement, building bricks, general building materials, and thermal insulation materials. The iron concentrate produced can meet the needs of steel production; the lead concentrate can be used to extract high-purity lead metal; the industrial copper sulfate and industrial zinc sulfate can meet industrial production needs; and the silicate cement can meet the needs of mine backfilling and general building materials. The main technical indicators of these products are shown in Table 1-4.

[0062] Table 1. Statistical Table of Technical Indicators for Iron Concentrate (%)

[0063]

[0064] Table 2. Statistical Table of Technical Indicators for Lead Concentrate (%)

[0065]

[0066] Table 3. Statistical Table of Technical Indicators for Industrial Copper Sulfate (%)

[0067]

[0068] Table 4. Statistical Table of Technical Indicators for Industrial Zinc Sulfate (%)

[0069]

[0070] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings, characterized in that, Includes the following steps: (1) Reduction roasting: The copper smelting slag flotation tailings and reducing agent are roasted at a temperature of 600-800℃ to obtain roasted sand; (2) Magnetic separation: including primary magnetic separation and secondary magnetic separation; the primary magnetic separation is to cool the roasted sand and then perform a primary magnetic separation in a magnetic field with a magnetic induction intensity of 1000-2000 Gauss to obtain iron concentrate with iron content >60% and tailings; the secondary magnetic separation is to perform a secondary magnetic separation in a magnetic field with a magnetic induction intensity of 4000-14000 Gauss to obtain weakly magnetic iron-bearing minerals and first tailings; (3) Gravity separation: The first tailings are subjected to at least one gravity separation to obtain concentrate and second tailings; (4) Primary acid leaching: The concentrate is subjected to acid leaching in a magnetic field with a mass concentration of 10 (5) First precipitation: Adjust the pH of the first filtrate to 7-10 and carry out the precipitation reaction. After the reaction is completed, separate the solid and liquid to obtain the second filtrate and the second filter residue. (6) Copper-zinc separation: Add sodium hydroxide solution with a mass concentration of 25%-40% to the second filter residue and carry out the dissolution reaction. After the reaction is completed, separate the solid and liquid to obtain the third filtrate and the third filter residue. (7) Second precipitation: Adjust the pH of the third filtrate to 7-10 and carry out the precipitation reaction. After the reaction is completed, separate the solid and liquid to obtain the fourth filtrate and the fourth filter residue.

2. The method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings according to claim 1, characterized in that, The copper smelting slag flotation tailings in step (1) consist of more than 80% particles with a particle size of less than 400 mesh, and the reducing agent is coke.

3. The method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings according to claim 1, characterized in that, The re-separation in step (3) includes: primary re-separation: performing primary re-separation on the first tailings to obtain heavy metal concentrate and primary tailings; secondary re-separation: performing secondary re-separation on the heavy metal concentrate to obtain lead concentrate and secondary tailings; tertiary re-separation: performing tertiary re-separation on the secondary tailings to obtain concentrate and secondary tailings.

4. The method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings according to claim 3, characterized in that, The method also includes: combining weakly magnetic iron-bearing minerals, primary tailings, and secondary tailings to produce cement.

5. The method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings according to claim 4, characterized in that, The method for producing cement is as follows: weakly magnetic iron-containing minerals, primary tailings, and secondary tailings are combined, and limestone and clay are added to them. The mixture is then ground until more than 65% of the particles have a particle size of less than 400 mesh. The mixture is then calcined at a temperature of 400-1200℃ to obtain cement clinker. Gypsum is added to the cement clinker and ground until more than 85% of the particles have a particle size of less than 400 mesh to obtain silicate cement product.

6. The method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings according to claim 3, characterized in that, The method further includes: selling the heavy metal concentrate and concentrate obtained by gravity separation as raw materials and intermediate products; using the primary tailings and the second tailings to make bricks and general building materials, wherein the primary tailings and the second tailings are both silicate minerals; and using the weakly magnetic iron-bearing minerals to make thermal insulation materials.

7. The method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings according to claim 1, characterized in that, The method for adjusting the pH of the first filtrate to alkaline in step (5) is to add sodium hydroxide solution to the first filtrate.

8. The method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings according to claim 1, characterized in that, Step (6) also includes: adding dilute sulfuric acid solution to the third filter residue, and obtaining copper sulfate solution after reaction; concentrating and crystallizing the copper sulfate solution to obtain industrial copper sulfate.

9. The method for efficient and comprehensive recovery and utilization of copper smelting slag flotation tailings according to any one of claims 1-8, characterized in that, The method further includes step (8) secondary acid dissolution: sulfuric acid solution is added to the fourth filter residue, and after reaction, zinc sulfate solution is obtained. Then, it is concentrated and crystallized to obtain industrial zinc sulfate.

Citation Information

Patent Citations

  • Integrated utilization technique for multi-metal ore containing gold and silver by chlorine carrier chlorination method

    CN101215633A

  • Beneficiation and metallurgy combined process for processing refractory copper and zinc ores

    CN106345607A

  • Recycling method of fine-grained tailing sand

    CN111302680A

  • Process for comprehensively recovering valuable metals from solid dangerous waste residues through wet smelting

    CN113399107A

  • Method for recovering iron from copper smelting slag flotation tailings

    CN115254914A