A cold-sintered barium strontium titanate-based ceramic and a preparation method thereof

The preparation method of cold-sintered barium strontium titanate-based ceramics solves the problem of high sintering temperature of traditional barium titanate ceramics, achieves stable dielectric properties and low energy consumption at low and high frequencies, is suitable for low-temperature co-firing technology, and expands the Its scope of application.

CN117303889BActive Publication Date: 2024-10-01KYOCERA HIGH VOLTAGE (BEIJING) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311226651.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-21
Publication Date
2024-10-01
Estimated Expiration
2043-09-21

AI Technical Summary

Technical Problem

The high sintering temperature of barium titanate ceramics prepared by traditional solid-phase methods leads to reduced material performance, high electrode cost, and high energy consumption, which limits its further development in high-quality development and applications.

Method used

The preparation method of cold-sintered barium strontium titanate-based ceramics is adopted. The dielectric constant is obtained by mixing the pre-synthesized powder of barium strontium titanate, intermediate liquid source and dopant, uniaxial hot-pressing sintering, then pressure calcination and annealing. For ceramics with a dielectric loss of 1805 to 2582 and a dielectric loss of 0.01% to 0.02%, the sintering temperature is lower than that of traditional methods.

Benefits of technology

It achieves stable dielectric properties in the low and high frequency range, lowers the sintering temperature, reduces energy consumption, is suitable for low-temperature co-firing technology, opens up new uses for strontium barium titanate ceramics, and can be used with cheap electrodes .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117303889B_ABST
    Figure CN117303889B_ABST
Patent Text Reader

Abstract

The invention discloses a cold-sintered barium strontium titanate-based ceramic and a preparation method thereof. The cold-sintered barium strontium titanate-based ceramic has a relative density of 90.4% to 96.7%, a dielectric constant of 1805 to 2582 at 1 MHz, and a dielectric loss of 0.01% to 0.02%. In a frequency range of 1 MHz to 8 MHz and a temperature range of 20° C. to 85° C., the dielectric constant is greater than 1551, the change rate is less than 10%, the dielectric loss is less than 0.02%, and the change rate is less than 30%. Compared with ceramics prepared by a traditional solid phase method, the cold-sintered barium strontium titanate-based ceramic has comparable low-frequency performance and more excellent high-frequency characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic materials, and in particular relates to a cold-sintered barium strontium titanate-based ceramic and a preparation method thereof. Background Art

[0002] Barium titanate ceramics have excellent dielectric, piezoelectric and piezoresistive properties. They can be made into components such as capacitors, filters, and resonators. They are widely used in high-end equipment in high-tech fields such as electronics, communications, aerospace, nuclear energy, and oil well detection.

[0003] As a dielectric material with a high dielectric constant, barium titanate ceramics are often used in MLCC (Multilayer Ceramic Capacitor). Since the sintering temperature required to prepare barium titanate ceramics using the traditional solid phase method is as high as 1300°C, which is much higher than the melting point of the cheap and high-performance internal electrode copper (1083°C), the industry has to use expensive An / Pd electrodes and poor-performance nickel electrodes.

[0004] High sintering temperature will also bring other adverse results, such as high-temperature volatilization of doping elements leading to decreased material performance, inability to co-fire with components with lower melting points to prepare composite materials, easy interface diffusion when ceramics and internal electrodes are co-fired at high temperatures, affecting capacitor performance, and significantly increasing energy consumption, which is not conducive to carbon emission reduction. These problems have greatly restricted the further development and application of barium titanate ceramics in the context of high-quality development. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a cold-sintered barium strontium titanate-based ceramic and a preparation method thereof in view of the deficiencies of the above-mentioned prior art. The cold-sintered barium strontium titanate-based ceramic of the present invention has a dielectric constant of 1805-2582 at 1MHz and a dielectric loss of 0.01%-0.02%; in a frequency range of 1MHz-8MHz and a temperature range of 20℃-85℃, the dielectric constant is greater than 1551, the change rate is less than 10%, the dielectric loss is less than 0.02%, and the change rate is less than 30%. Compared with ceramics prepared by a traditional solid phase method, it has comparable low-frequency performance and better high-frequency characteristics.

[0006] To solve the above technical problems, the technical solution adopted by the present invention is: a cold-sintered barium strontium titanate-based ceramic, characterized in that the relative density of the cold-sintered barium strontium titanate-based ceramic is 90.4% to 96.7%; the dielectric constant is 1805 to 2582 at 1MHz, and the dielectric loss is 0.01% to 0.02%; the dielectric constant is greater than 1551 in the frequency range of 1MHz to 8MHz and the temperature range of 20℃ to 85℃, the change rate is less than 10%, the dielectric loss is less than 0.02%, and the change rate is less than 30%.

[0007] In addition, the present invention also provides a preparation method of cold-sintered barium strontium titanate-based ceramics, which is characterized in that it includes mixing raw materials of barium strontium titanate pre-synthesized powder, intermediate liquid source and dopant, uniaxial hot pressing sintering, re-pressure calcining and annealing to obtain cold-sintered barium strontium titanate-based ceramics; the temperature of the uniaxial hot pressing sintering is 180°C to 200°C, the pressure is 300MPa to 600MPa, and the temperature of the re-pressure calcining is 160°C to 180°C, and the pressure is 200MPa to 500MPa.

[0008] The above-mentioned method for preparing cold-sintered barium strontium titanate-based ceramics is characterized in that the mass of the intermediate liquid source is 15% to 25% of the mass of the barium strontium titanate pre-synthesized powder, the intermediate liquid source is magnesium hydroxide or magnesium oxalate, the mass of the dopant is 0.2% of the mass of the barium strontium titanate pre-synthesized powder, and the dopant is bismuth oxide.

[0009] The method for preparing the cold-sintered barium strontium titanate-based ceramics is characterized in that the temperature of uniaxial hot pressing sintering is greater than the temperature of re-pressurizing calcining; and the pressure of uniaxial hot pressing sintering is greater than the pressure of re-pressurizing calcining.

[0010] The above-mentioned method for preparing cold-sintered barium strontium titanate-based ceramics is characterized by comprising:

[0011] Step 1, mixing the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant uniformly to form a mixture; specifically comprising: adding the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant into a mortar in sequence, grinding for 2h to 3h, and adding deionized water dropwise during the grinding process to obtain a mixture;

[0012] Step 2, uniaxial hot pressing and sintering the mixture to obtain a sample after uniaxial hot pressing and sintering;

[0013] Step 3, pressurizing and calcining the sample after uniaxial hot pressing sintering to obtain a pressurized and calcined sample;

[0014] Step 4: annealing the sample after the pressurization and calcination to obtain cold-sintered barium strontium titanate-based ceramics.

[0015] The above-mentioned method for preparing cold-sintered barium strontium titanate-based ceramics is characterized in that, in step one, the mass of the intermediate liquid source is 15% to 25% of the mass of the barium strontium titanate pre-synthesized powder, the intermediate liquid source is magnesium hydroxide or magnesium oxalate, the mass of the dopant is 0.2% of the mass of the barium strontium titanate pre-synthesized powder, and the dopant is bismuth oxide; the mass of the deionized water is 15% to 25% of the mass of the barium strontium titanate pre-synthesized powder.

[0016] The preparation method of the above-mentioned cold-sintered barium strontium titanate-based ceramics is characterized in that step two specifically includes: placing the mixture in a hot pressing mold, placing the hot pressing mold in a hot press, applying a uniaxial pressure of 300MPa to 600MPa, heating to 180°C to 200°C at a heating rate of 2°C / min to 4°C / min, keeping warm for 30min to 90min, turning off the power, releasing the pressure, cooling, and obtaining a sample after uniaxial hot pressing sintering.

[0017] The preparation method of the above-mentioned cold-sintered barium strontium titanate-based ceramics is characterized in that, in step three, the uniaxial pressure of the re-pressurized calcination is 200MPa~500MPa, the heating rate is 2℃ / min~4℃ / min, the temperature of the re-pressurized calcination is 160℃~180℃, and the insulation time is 30min~90min.

[0018] The method for preparing the cold-sintered barium strontium titanate-based ceramics is characterized in that the temperature of uniaxial hot pressing sintering is greater than the temperature of re-pressurizing calcining; and the pressure of uniaxial hot pressing sintering is greater than the pressure of re-pressurizing calcining.

[0019] The method for preparing the cold-sintered barium strontium titanate-based ceramics is characterized in that, in step 4, the annealing temperature is 850° C. to 950° C., and the holding time is 3 h to 5 h.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] 1. The cold-sintered barium strontium titanate-based ceramic of the present invention has a dielectric constant of 1805-2582 at 1 MHz and a dielectric loss of 0.01%-0.02%; in the frequency range of 1 MHz to 8 MHz and the temperature range of 20°C to 85°C, the dielectric constant is >1551, the change rate is <10%, the dielectric loss is <0.02%, and the change rate is <30%. It can be stably applied in the frequency range of 1 MHz to 8 MHz and the temperature range of 20°C to 85°C. Compared with the ceramics prepared by the traditional solid phase method, it has comparable low-frequency performance and better high-frequency characteristics. It can be used in conjunction with cheaper electrodes such as Ag and Cu to prepare MLCC devices, or can be co-fired with other materials with lower melting points. It is expected to be used in LTCC (Low Temperature Co-fired Ceramic) technology to explore new uses for barium strontium titanate ceramics.

[0022] 2. The cold-sintered barium strontium titanate-based ceramics of the present invention have raw materials including pre-synthesized barium strontium titanate powder, an intermediate liquid source and a dopant, wherein the intermediate liquid source is magnesium hydroxide or magnesium oxalate, which can produce a liquid phase that can dissolve the main crystalline phase under a high temperature and high pressure environment, promote particle rearrangement, gas discharge, and material dissolution-precipitation, so that the grains grow fully and the ceramic microstructure reaches a densification.

[0023] 3. In the cold-sintered barium strontium titanate-based ceramic of the present invention, the dopant in the raw material is bismuth oxide, which can be used as a doping element in the crystal phase of the barium strontium titanate ceramic. Together with the magnesium ions generated by the decomposition of magnesium hydroxide or magnesium oxalate at high temperature, the bismuth oxide is fully dispersed in the grain boundaries of the barium strontium titanate ceramic, thereby increasing the grain boundary barrier, limiting the abnormal grain growth during the high-temperature annealing process, promoting uniform distribution of grains, increasing the dielectric constant, and reducing dielectric loss.

[0024] 4. The preparation method of the cold-sintered barium strontium titanate-based ceramics of the present invention comprises mixing the raw material barium strontium titanate pre-synthesized powder, the intermediate liquid source and the dopant, uniaxial hot pressing sintering, and then pressurizing calcining and annealing, wherein the temperature of the uniaxial hot pressing sintering is 180°C to 200°C, and the sintering temperature is much lower than the traditional solid phase sintering temperature, which is conducive to achieving carbon emission reduction.

[0025] 5. The preparation method of the cold-sintered barium strontium titanate-based ceramics of the present invention includes uniaxial hot pressing sintering, re-pressure calcination and annealing, and the temperature and pressure of the re-pressure calcination are lower than the temperature and pressure of the uniaxial hot pressing sintering, which can effectively eliminate residual stress, keep the ceramic structure dense, inhibit capillary action, promote ceramic sintering densification, and avoid gas and microcracks caused by single sintering and annealing.

[0026] 6. The preparation method of the cold-sintered barium strontium titanate-based ceramic of the present invention comprises adding the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant in sequence to the grinding process and then grinding, which is conducive to uniform grinding.

[0027] 7. The preparation method of the cold-sintered barium strontium titanate-based ceramics of the present invention has low cost and simple process.

[0028] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0029] Instruction Manual

[0030] Figure 1 The XRD patterns of Examples 1-7 and Comparative Examples of the present invention are shown in FIG.

[0031] Figure 2 The dielectric constant spectra of Examples 1-7 of the present invention and the comparative example are shown.

[0032] Figure 3 The dielectric loss spectrum diagram of Examples 1-7 of the present invention and the comparative example.

[0033] Figure 4 The dielectric constant temperature spectra of Examples 1-7 of the present invention and the comparative example are shown.

[0034] Figure 5 The dielectric loss thermograms of Examples 1-7 of the present invention and the comparative example.

[0035] Figure 6The scanning electron microscope photographs of Examples 1 and 5 of the present invention are shown.

[0036] Figure 7 The relative density diagram of Examples 1-7 of the present invention at different sintering temperatures. DETAILED DESCRIPTION

[0037] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the examples given are not intended to limit the present invention.

[0038] It should be noted that the experimental methods used in the following examples are all conventional methods unless otherwise specified.

[0039] Example 1

[0040] This embodiment provides a method for preparing a cold-sintered barium strontium titanate-based ceramic, comprising:

[0041] Step 1: Evenly mix the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant to form a mixture, specifically comprising: sequentially adding 20 g of the pre-synthesized barium strontium titanate powder, 5 g of magnesium hydroxide and 0.04 g of bismuth oxide into an agate mortar, grinding for 2 h, and dripping deionized water during the grinding process to obtain a mixture; the mass of the deionized water is 5 g; the pre-synthesized barium strontium titanate powder is a pre-synthesized barium strontium titanate powder obtained by a solid phase method commonly used in the art using barium carbonate, strontium carbonate and titanium dioxide as raw materials, and the solid phase synthesis includes ball milling, drying, calcining and grinding processes; the solid phase synthesis can be, for example: according to (Ba 0.7 Sr 0.3 ) TiO4 is prepared in a stoichiometric ratio, anhydrous ethanol is used as a grinding aid, zirconium oxide balls are used as ball milling media, and the mixture is ball milled in a planetary ball mill for 6 hours to obtain a ball milling slurry, the ball milling slurry is dried in an oven at 80° C., loaded into a zirconium oxide crucible, and placed in a muffle furnace at 1150° C. for calcination for 180 minutes, ground in a mortar for 2 hours, and passed through a 200-mesh sieve to obtain a pre-synthesized barium strontium titanate powder;

[0042] Step 2, uniaxial hot pressing and sintering the mixture, specifically comprising: placing the mixture in a hot pressing mold with a diameter of 13 mm, placing the hot pressing mold in a hot press, applying a uniaxial pressure of 300 MPa, heating to 180° C. at a heating rate of 3° C. / min, keeping the temperature for 30 min, turning off the power, removing the pressure, and naturally cooling to 50° C. to obtain a sample after uniaxial hot pressing and sintering;

[0043] Step 3, re-pressurizing and calcining the sample after uniaxial hot pressing sintering, specifically comprising: when the temperature of the hot press machine drops to 50°C, applying a uniaxial pressure of 200MPa, heating to 160°C at a heating rate of 3°C / min, keeping warm for 30min, turning off the power, removing the pressure, cooling naturally to room temperature, and drying until the residual water evaporates completely to obtain the sample after re-pressurizing and calcining; the drying temperature can be 120°C and the drying time can be 6h;

[0044] Step 4, annealing the sample after the re-pressurized calcination, specifically comprising: placing the sample after the re-pressurized calcination on a zirconia support plate, placing it in a muffle furnace, heating it to an annealing temperature of 850° C. at a heating rate of 10° C. / min, keeping it warm for 4 hours, and cooling it naturally after power off to obtain a cold-sintered barium strontium titanate-based ceramic;

[0045] Step 5: Evaluate the performance of the cold-sintered barium strontium titanate-based ceramic, including: grinding and polishing the surface of the cold-sintered barium strontium titanate-based ceramic with sandpaper, testing the volume density of the sample by the Archimedes method, and calculating that the relative density is 95.2%; characterizing its phase structure by an X-ray diffractometer, and the results are as follows: Figure 1 As shown, it can be seen that the diffraction peaks are clear and sharp, indicating that the phase is well crystallized. The appearance of the MgO diffraction peak indicates that the magnesium ions have not entered the lattice of the main crystal phase of barium strontium titanate, but exist independently at the grain boundary, which is conducive to improving the grain boundary barrier, limiting the abnormal growth of grains, making the grains evenly distributed, and reducing dielectric loss; the cross-sectional morphology was characterized by scanning electron microscopy, and the results are shown in Figure 6 As shown, it can be seen that after annealing, the grain size of the sample is larger, the organizational structure is dense, the grains are well crystallized and uniform in size, indicating that the presence of the low eutectic point of magnesium oxide and bismuth oxide during the annealing process will also promote further growth of the grains, which is beneficial to improving the dielectric constant of the ceramic; the cold-sintered barium strontium titanate-based ceramic is polished, and a conductive silver paste is evenly coated on the surface of the cold-sintered barium strontium titanate-based ceramic after polishing. After drying, the sample is heat-treated at 850°C for 5 hours to obtain a silver-coated sample, and the dielectric properties of the silver-coated sample are tested using an HP-4294A impedance analyzer. The results are as follows Figures 2 to 5 As shown, the results show that the dielectric constant at 1 MHz is 2516 and the dielectric loss is 0.016%. In the range of 1 MHz to 8 MHz, the dielectric constant is 2516 to 2415 and the dielectric loss is 0.016% to 0.011%.

[0046] Example 2

[0047] This embodiment provides a method for preparing a cold-sintered barium strontium titanate-based ceramic, comprising:

[0048] Step 1: Evenly mix the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant to form a mixture, specifically comprising: sequentially adding 20 g of the pre-synthesized barium strontium titanate powder, 4 g of magnesium hydroxide and 0.04 g of bismuth oxide into an agate mortar, grinding for 2 h, and dripping deionized water during the grinding process to obtain a mixture; the mass of the deionized water is 4 g; the pre-synthesized barium strontium titanate powder is a pre-synthesized barium strontium titanate powder obtained by a solid phase method commonly used in the art using barium carbonate, strontium carbonate and titanium dioxide as raw materials, and the solid phase synthesis includes ball milling, drying, calcining and grinding processes; the solid phase synthesis can be, for example: according to (Ba 0.7 Sr 0.3 ) TiO4 is prepared in a stoichiometric ratio, anhydrous ethanol is used as a grinding aid, zirconium oxide balls are used as ball milling media, and the mixture is ball milled in a planetary ball mill for 6 hours to obtain a ball milling slurry, the ball milling slurry is dried in an oven at 80° C., loaded into a zirconium oxide crucible, and placed in a muffle furnace at 1150° C. for calcination for 180 minutes, ground in a mortar for 2 hours, and passed through a 200-mesh sieve to obtain a pre-synthesized barium strontium titanate powder;

[0049] Step 2, uniaxial hot pressing and sintering the mixture, specifically comprising: placing the mixture in a hot pressing mold with a diameter of 13 mm, placing the hot pressing mold in a hot press, applying a uniaxial pressure of 400 MPa, heating to 200° C. at a heating rate of 3° C. / min, keeping the temperature for 60 min, turning off the power, removing the pressure, and naturally cooling to 50° C. to obtain a sample after uniaxial hot pressing and sintering;

[0050] Step 3, re-pressurizing and calcining the sample after uniaxial hot pressing sintering, specifically comprising: when the temperature of the hot press machine drops to 50°C, applying a uniaxial pressure of 300MPa, heating to 180°C at a heating rate of 3°C / min, keeping the temperature for 60min, turning off the power, removing the pressure, cooling naturally to room temperature, and drying until the residual water evaporates completely to obtain the sample after re-pressurizing and calcining; the drying temperature can be 120°C and the drying time can be 6h;

[0051] Step 4, annealing the sample after the re-pressurized calcination, specifically comprising: placing the sample after the re-pressurized calcination on a zirconia support plate, placing it in a muffle furnace, heating it to an annealing temperature of 900° C. at a heating rate of 10° C. / min, keeping it warm for 4 hours, and cooling it naturally after power off to obtain a cold-sintered barium strontium titanate-based ceramic;

[0052] Step 5: Evaluate the performance of the cold-sintered barium strontium titanate-based ceramic, including: grinding and polishing the surface of the cold-sintered barium strontium titanate-based ceramic with sandpaper, testing the volume density of the sample by the Archimedes method, and calculating that the relative density is 96.7%; characterizing its phase structure by an X-ray diffractometer, and the results are as follows: Figure 1As shown, it can be seen that the diffraction peaks are clear and sharp, indicating that the phase is well crystallized. The appearance of the MgO diffraction peak indicates that the magnesium ions have not entered the lattice of the main crystal phase of barium strontium titanate, but exist independently at the grain boundary, which is beneficial to improve the grain boundary barrier, limit the abnormal growth of grains, make the grains evenly distributed, and reduce dielectric loss; the cold-sintered barium strontium titanate-based ceramic is polished, and a conductive silver paste is evenly coated on the surface of the cold-sintered barium strontium titanate-based ceramic after polishing. After drying, it is heat-treated at 850°C for 5 hours to obtain a silver-coated sample, and the dielectric properties of the silver-coated sample are tested using an HP-4294A impedance analyzer. The results are as follows Figures 2 to 5 As shown, the results show that the dielectric constant at 1 MHz is 2583, and the dielectric loss is 0.017%. In the range of 1 MHz to 8 MHz, the dielectric constant is 2583 to 2460, and the dielectric loss is 0.017% to 0.012%.

[0053] Example 3

[0054] This embodiment provides a method for preparing a cold-sintered barium strontium titanate-based ceramic, comprising:

[0055] Step 1: Evenly mix the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant to form a mixture, specifically comprising: sequentially adding 25 g of the pre-synthesized barium strontium titanate powder, 3.75 g of magnesium hydroxide and 0.05 g of bismuth oxide to an agate mortar, grinding for 2 h, and dripping deionized water during the grinding process to obtain a mixture; the mass of the deionized water is 3.75 g; the pre-synthesized barium strontium titanate powder is a pre-synthesized barium strontium titanate powder obtained by a solid phase method commonly used in the art using barium carbonate, strontium carbonate and titanium dioxide as raw materials, and the solid phase synthesis includes ball milling, drying, calcining and grinding processes; the solid phase synthesis can be, for example: according to (Ba 0.7 Sr 0.3 ) TiO4 is prepared in a stoichiometric ratio, anhydrous ethanol is used as a grinding aid, zirconium oxide balls are used as ball milling media, and the mixture is ball milled in a planetary ball mill for 6 hours to obtain a ball milling slurry, the ball milling slurry is dried in an oven at 80° C., loaded into a zirconium oxide crucible, and placed in a muffle furnace at 1150° C. for calcination for 180 minutes, ground in a mortar for 2 hours, and passed through a 200-mesh sieve to obtain a pre-synthesized barium strontium titanate powder;

[0056] Step 2, uniaxial hot pressing and sintering the mixture, specifically comprising: placing the mixture in a hot pressing mold with a diameter of 13 mm, placing the hot pressing mold in a hot press, applying a uniaxial pressure of 500 MPa, heating to 190° C. at a heating rate of 3° C. / min, keeping the temperature for 90 min, turning off the power, removing the pressure, and naturally cooling to 50° C. to obtain a sample after uniaxial hot pressing and sintering;

[0057] Step 3, re-pressurizing and calcining the sample after uniaxial hot pressing sintering, specifically comprising: when the temperature of the hot press machine drops to 50°C, applying a uniaxial pressure of 400MPa, heating to 170°C at a heating rate of 3°C / min, keeping warm for 90min, turning off the power, removing the pressure, cooling naturally to room temperature, and drying until the residual water evaporates completely to obtain the sample after re-pressurizing and calcining; the drying temperature can be 120°C and the drying time can be 6h;

[0058] Step 4, annealing the sample after the re-pressurized calcination, specifically comprising: placing the sample after the re-pressurized calcination on a zirconia support plate, placing it in a muffle furnace, heating it to an annealing temperature of 950° C. at a heating rate of 10° C. / min, keeping it warm for 4 hours, and cooling it naturally after power off to obtain a cold-sintered barium strontium titanate-based ceramic;

[0059] Step 5: Evaluate the performance of the cold-sintered barium strontium titanate-based ceramic, including: grinding and polishing the surface of the cold-sintered barium strontium titanate-based ceramic with sandpaper, testing the volume density of the sample by the Archimedes method, and calculating that the relative density is 95.2%; characterizing its phase structure by an X-ray diffractometer, and the results are as follows: Figure 1 As shown, it can be seen that the diffraction peaks are clear and sharp, indicating that the phase is well crystallized. The appearance of the MgO diffraction peak indicates that the magnesium ions have not entered the lattice of the main crystal phase of barium strontium titanate, but exist independently at the grain boundary, which is beneficial to improve the grain boundary barrier, limit the abnormal growth of grains, make the grains evenly distributed, and reduce dielectric loss; the cold-sintered barium strontium titanate-based ceramic is polished, and a conductive silver paste is evenly coated on the surface of the cold-sintered barium strontium titanate-based ceramic after polishing. After drying, it is heat-treated at 850°C for 5 hours to obtain a silver-coated sample, and the dielectric properties of the silver-coated sample are tested using an HP-4294A impedance analyzer. The results are as follows Figures 2 to 5 As shown, the results show that the dielectric constant at 1 MHz is 2537, and the dielectric loss is 0.019%. In the range of 1 MHz to 8 MHz, the dielectric constant is 2537 to 2425, and the dielectric loss is 0.019% to 0.017%.

[0060] Example 4

[0061] This embodiment provides a method for preparing a cold-sintered barium strontium titanate-based ceramic, comprising:

[0062] Step 1: Evenly mix the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant to form a mixture, specifically comprising: sequentially adding 20 g of the pre-synthesized barium strontium titanate powder, 3 g of magnesium hydroxide and 0.04 g of bismuth oxide into an agate mortar, grinding for 2 h, and dripping deionized water during the grinding process to obtain a mixture; the mass of the deionized water is 3 g; the pre-synthesized barium strontium titanate powder is a pre-synthesized barium strontium titanate powder obtained by a solid phase method commonly used in the art using barium carbonate, strontium carbonate and titanium dioxide as raw materials, and the solid phase synthesis includes ball milling, drying, calcining and grinding; the solid phase synthesis can be, for example: according to (Ba 0.7 Sr 0.3 ) TiO4 is prepared in a stoichiometric ratio, anhydrous ethanol is used as a grinding aid, zirconium oxide balls are used as ball milling media, and the mixture is ball milled in a planetary ball mill for 6 hours to obtain a ball milling slurry, the ball milling slurry is dried in an oven at 80° C., loaded into a zirconium oxide crucible, and placed in a muffle furnace at 1150° C. for calcination for 180 minutes, ground in a mortar for 2 hours, and passed through a 200-mesh sieve to obtain a pre-synthesized barium strontium titanate powder;

[0063] Step 2, uniaxial hot pressing and sintering the mixture, specifically comprising: placing the mixture in a hot pressing mold with a diameter of 13 mm, placing the hot pressing mold in a hot press, applying a uniaxial pressure of 600 MPa, heating to 200° C. at a heating rate of 3° C. / min, keeping the temperature for 90 minutes, turning off the power, removing the pressure, and naturally cooling to 50° C. to obtain a sample after uniaxial hot pressing and sintering;

[0064] Step 3, re-pressurizing and calcining the sample after uniaxial hot pressing sintering, specifically comprising: when the temperature of the hot press machine drops to 50°C, applying a uniaxial pressure of 500MPa, heating to 180°C at a heating rate of 3°C / min, keeping the temperature for 60min, turning off the power, removing the pressure, cooling naturally to room temperature, and drying until the residual water evaporates completely to obtain the sample after re-pressurizing and calcining; the drying temperature can be 120°C and the drying time can be 6h;

[0065] Step 4, annealing the sample after the re-pressurized calcination, specifically comprising: placing the sample after the re-pressurized calcination on a zirconia support plate, placing it in a muffle furnace, heating it to an annealing temperature of 850° C. at a heating rate of 10° C. / min, keeping it warm for 4 hours, and cooling it naturally after power off to obtain a cold-sintered barium strontium titanate-based ceramic;

[0066] Step 5: Evaluate the performance of the cold-sintered barium strontium titanate-based ceramic, including: grinding and polishing the surface of the cold-sintered barium strontium titanate-based ceramic with sandpaper, testing the volume density of the sample by the Archimedes method, and calculating that the relative density is 94.9%; characterizing its phase structure by an X-ray diffractometer, and the results are as follows: Figure 1As shown, it can be seen that the diffraction peaks are clear and sharp, indicating that the phase is well crystallized. The appearance of the MgO diffraction peak indicates that the magnesium ions have not entered the lattice of the main crystal phase of barium strontium titanate, but exist independently at the grain boundary, which is beneficial to improve the grain boundary barrier, limit the abnormal growth of grains, make the grains evenly distributed, and reduce dielectric loss; the cold-sintered barium strontium titanate-based ceramic is polished, and a conductive silver paste is evenly coated on the surface of the cold-sintered barium strontium titanate-based ceramic after polishing. After drying, it is heat-treated at 850°C for 5 hours to obtain a silver-coated sample, and the dielectric properties of the silver-coated sample are tested using an HP-4294A impedance analyzer. The results are as follows Figures 2 to 5 As shown, the results show that the dielectric constant at 1 MHz is 2450, and the dielectric loss is 0.018%. In the range of 1 MHz to 8 MHz, the dielectric constant is 2450 to 2322, and the dielectric loss is 0.018% to 0.017%.

[0067] Example 5

[0068] This embodiment provides a method for preparing a cold-sintered barium strontium titanate-based ceramic, comprising:

[0069] Step 1: Evenly mix the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant to form a mixture, specifically comprising: sequentially adding 20 g of the pre-synthesized barium strontium titanate powder, 5 g of magnesium oxalate and 0.04 g of bismuth oxide into an agate mortar, grinding for 2 h, and dripping deionized water during the grinding process to obtain a mixture; the mass of the deionized water is 5 g; the pre-synthesized barium strontium titanate powder is a pre-synthesized barium strontium titanate powder obtained by a solid phase method commonly used in the art using barium carbonate, strontium carbonate and titanium dioxide as raw materials, and the solid phase synthesis includes ball milling, drying, calcining and grinding processes; the solid phase synthesis can be, for example: according to (Ba 0.7 Sr 0.3 ) TiO4 is prepared in a stoichiometric ratio, anhydrous ethanol is used as a grinding aid, zirconium oxide balls are used as ball milling media, and the mixture is ball milled in a planetary ball mill for 6 hours to obtain a ball milling slurry, the ball milling slurry is dried in an oven at 80° C., loaded into a zirconium oxide crucible, and placed in a muffle furnace at 1150° C. for calcination for 180 minutes, ground in a mortar for 2 hours, and passed through a 200-mesh sieve to obtain a pre-synthesized barium strontium titanate powder;

[0070] Step 2, uniaxial hot pressing and sintering the mixture, specifically comprising: placing the mixture in a hot pressing mold with a diameter of 13 mm, placing the hot pressing mold in a hot press, applying a uniaxial pressure of 300 MPa, heating to 180° C. at a heating rate of 3° C. / min, keeping the temperature for 30 min, turning off the power, removing the pressure, and naturally cooling to 50° C. to obtain a sample after uniaxial hot pressing and sintering;

[0071] Step 3, re-pressurizing and calcining the sample after uniaxial hot pressing sintering, specifically comprising: when the temperature of the hot press machine drops to 50°C, applying a uniaxial pressure of 200MPa, heating to 160°C at a heating rate of 3°C / min, keeping warm for 30min, turning off the power, removing the pressure, cooling naturally to room temperature, and drying until the residual water evaporates completely to obtain the sample after re-pressurizing and calcining; the drying temperature can be 120°C and the drying time can be 6h;

[0072] Step 4, annealing the sample after the re-pressurized calcination, specifically comprising: placing the sample after the re-pressurized calcination on a zirconia support plate, placing it in a muffle furnace, heating it to an annealing temperature of 950° C. at a heating rate of 10° C. / min, keeping it warm for 4 hours, and cooling it naturally after power off to obtain a cold-sintered barium strontium titanate-based ceramic;

[0073] Step 5: Evaluate the performance of the cold-sintered barium strontium titanate-based ceramic, including: grinding and polishing the surface of the cold-sintered barium strontium titanate-based ceramic with sandpaper, testing the volume density of the sample by the Archimedes method, and calculating that the relative density is 93.8%; characterizing its phase structure by an X-ray diffractometer, and the results are as follows: Figure 1 As shown, it can be seen that the diffraction peaks are clear and sharp, indicating that the phase is well crystallized. The appearance of the MgO diffraction peak indicates that the magnesium ions have not entered the lattice of the main crystal phase of barium strontium titanate, but exist independently at the grain boundary, which is conducive to improving the grain boundary barrier, limiting the abnormal growth of grains, making the grains evenly distributed, and reducing dielectric loss; the cross-sectional morphology was characterized by scanning electron microscopy, and the results are shown in Figure 6 As shown, it can be seen that after annealing, the grain size of the sample is larger, the organizational structure is denser, the grain crystallization is better and the size is uniform, indicating that during the annealing process, due to the presence of the low eutectic point of magnesium oxide and bismuth oxide, the grains will also be promoted to grow further, which is beneficial to further improve the dielectric constant of the ceramic; the cold-sintered barium strontium titanate-based ceramic is polished, and a conductive silver paste is evenly coated on the surface of the cold-sintered barium strontium titanate-based ceramic after polishing. After drying, the sample is heat-treated at 850°C for 5 hours to obtain a silver-coated sample, and the dielectric properties of the silver-coated sample are tested using an HP-4294A impedance analyzer. The results are as follows Figures 2 to 5 As shown, the results show that the dielectric constant at 1 MHz is 2193, and the dielectric loss is 0.0181%. In the range of 1 MHz to 8 MHz, the dielectric constant is 2193 to 2088, and the dielectric loss is 0.0181% to 0.0179%.

[0074] Example 6

[0075] This embodiment provides a method for preparing a cold-sintered barium strontium titanate-based ceramic, comprising:

[0076] Step 1: Evenly mix the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant to form a mixture, specifically comprising: sequentially adding 20 g of the pre-synthesized barium strontium titanate powder, 4 g of magnesium oxalate and 0.04 g of bismuth oxide to an agate mortar, grinding for 2 h, and dripping deionized water during the grinding process to obtain a mixture; the mass of the deionized water is 4 g; the pre-synthesized barium strontium titanate powder is a pre-synthesized barium strontium titanate powder obtained by a solid phase method commonly used in the art using barium carbonate, strontium carbonate and titanium dioxide as raw materials, and the solid phase synthesis includes ball milling, drying, calcining and grinding processes; the solid phase synthesis can be, for example: according to (Ba 0.7 Sr 0.3 ) TiO4 is prepared in a stoichiometric ratio, anhydrous ethanol is used as a grinding aid, zirconium oxide balls are used as ball milling media, and the mixture is ball milled in a planetary ball mill for 6 hours to obtain a ball milling slurry, the ball milling slurry is dried in an oven at 80° C., loaded into a zirconium oxide crucible, and placed in a muffle furnace at 1150° C. for calcination for 180 minutes, ground in a mortar for 2 hours, and passed through a 200-mesh sieve to obtain a pre-synthesized barium strontium titanate powder;

[0077] Step 2, uniaxial hot pressing and sintering the mixture, specifically comprising: placing the mixture in a hot pressing mold with a diameter of 13 mm, placing the hot pressing mold in a hot press, applying a uniaxial pressure of 400 MPa, heating to 200° C. at a heating rate of 3° C. / min, keeping the temperature for 60 min, turning off the power, removing the pressure, and naturally cooling to 50° C. to obtain a sample after uniaxial hot pressing and sintering;

[0078] Step 3, re-pressurizing and calcining the sample after uniaxial hot pressing sintering, specifically comprising: when the temperature of the hot press machine drops to 50°C, applying a uniaxial pressure of 300MPa, heating to 180°C at a heating rate of 3°C / min, keeping the temperature for 60min, turning off the power, removing the pressure, cooling naturally to room temperature, and drying until the residual water evaporates completely to obtain the sample after re-pressurizing and calcining; the drying temperature can be 120°C and the drying time can be 6h;

[0079] Step 4, annealing the sample after the re-pressurized calcination, specifically comprising: placing the sample after the re-pressurized calcination on a zirconia support plate, placing it in a muffle furnace, heating it to an annealing temperature of 900° C. at a heating rate of 10° C. / min, keeping it warm for 4 hours, and cooling it naturally after power off to obtain a cold-sintered barium strontium titanate-based ceramic;

[0080] Step 5: Evaluate the performance of the cold-sintered barium strontium titanate-based ceramic, including: grinding and polishing the surface of the cold-sintered barium strontium titanate-based ceramic with sandpaper, testing the volume density of the sample by the Archimedes method, and calculating that the relative density is 90.4%; characterizing its phase structure by an X-ray diffractometer, and the results are as follows: Figure 1As shown, it can be seen that the diffraction peaks are clear and sharp, indicating that the phase is well crystallized. The appearance of the MgO diffraction peak indicates that the magnesium ions have not entered the lattice of the main crystal phase of barium strontium titanate, but exist independently at the grain boundary, which is beneficial to improve the grain boundary barrier, limit the abnormal growth of grains, make the grains evenly distributed, and reduce dielectric loss; the cold-sintered barium strontium titanate-based ceramic is polished, and a conductive silver paste is evenly coated on the surface of the cold-sintered barium strontium titanate-based ceramic after polishing. After drying, it is heat-treated at 850°C for 5 hours to obtain a silver-coated sample, and the dielectric properties of the silver-coated sample are tested using an HP-4294A impedance analyzer. The results are as follows Figures 2 to 5 As shown, the results show that the dielectric constant at 1 MHz is 1823, and the dielectric loss is 0.0173%. In the range of 1 MHz to 8 MHz, the dielectric constant is 1823 to 1647, and the dielectric loss is 0.0173% to 0.0167%.

[0081] Example 7

[0082] This embodiment provides a method for preparing a cold-sintered barium strontium titanate-based ceramic, comprising:

[0083] Step 1: Evenly mix the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant to form a mixture, specifically comprising: sequentially adding 20 g of the pre-synthesized barium strontium titanate powder, 3 g of magnesium oxalate and 0.04 g of bismuth oxide into an agate mortar, grinding for 2 h, and dripping deionized water during the grinding process to obtain a mixture; the mass of the deionized water is 3 g; the pre-synthesized barium strontium titanate powder is a pre-synthesized barium strontium titanate powder obtained by a solid phase method commonly used in the art using barium carbonate, strontium carbonate and titanium dioxide as raw materials, and the solid phase synthesis includes ball milling, drying, calcining and grinding processes; the solid phase synthesis can be, for example: according to (Ba 0.7 Sr 0.3 ) TiO4 is prepared in a stoichiometric ratio, anhydrous ethanol is used as a grinding aid, zirconium oxide balls are used as ball milling media, and the mixture is ball milled in a planetary ball mill for 6 hours to obtain a ball milling slurry, the ball milling slurry is dried in an oven at 80° C., loaded into a zirconium oxide crucible, and placed in a muffle furnace at 1150° C. for calcination for 180 minutes, ground in a mortar for 2 hours, and passed through a 200-mesh sieve to obtain a pre-synthesized barium strontium titanate powder;

[0084] Step 2, uniaxial hot pressing and sintering the mixture, specifically comprising: placing the mixture in a hot pressing mold with a diameter of 13 mm, placing the hot pressing mold in a hot press, applying a uniaxial pressure of 600 MPa, heating to 200° C. at a heating rate of 3° C. / min, keeping the temperature for 90 minutes, turning off the power, removing the pressure, and naturally cooling to 50° C. to obtain a sample after uniaxial hot pressing and sintering;

[0085] Step 3, re-pressurizing and calcining the sample after uniaxial hot pressing sintering, specifically comprising: when the temperature of the hot press machine drops to 50°C, applying a uniaxial pressure of 500MPa, heating to 180°C at a heating rate of 3°C / min, keeping the temperature for 60min, turning off the power, removing the pressure, cooling naturally to room temperature, and drying until the residual water evaporates completely to obtain the sample after re-pressurizing and calcining; the drying temperature can be 120°C and the drying time can be 6h;

[0086] Step 4, annealing the sample after the re-pressurized calcination, specifically comprising: placing the sample after the re-pressurized calcination on a zirconia support plate, placing it in a muffle furnace, heating it to an annealing temperature of 850° C. at a heating rate of 10° C. / min, keeping it warm for 4 hours, and cooling it naturally after power off to obtain a cold-sintered barium strontium titanate-based ceramic;

[0087] Step 5: Evaluate the performance of the cold-sintered barium strontium titanate-based ceramic, including: grinding and polishing the surface of the cold-sintered barium strontium titanate-based ceramic with sandpaper, testing the volume density of the sample by the Archimedes method, and calculating that the relative density is 92.7%; characterizing its phase structure by an X-ray diffractometer, and the results are as follows: Figure 1 As shown, it can be seen that the diffraction peaks are clear and sharp, indicating that the phase is well crystallized. The appearance of the MgO diffraction peak indicates that the magnesium ions have not entered the lattice of the main crystal phase of barium strontium titanate, but exist independently at the grain boundary, which is beneficial to improve the grain boundary barrier, limit the abnormal growth of grains, make the grains evenly distributed, and reduce dielectric loss; the cold-sintered barium strontium titanate-based ceramic is polished, and a conductive silver paste is evenly coated on the surface of the cold-sintered barium strontium titanate-based ceramic after polishing. After drying, it is heat-treated at 850°C for 5 hours to obtain a silver-coated sample, and the dielectric properties of the silver-coated sample are tested using an HP-4294A impedance analyzer. The results are as follows Figures 2 to 5 As shown, the results show that the dielectric constant at 1 MHz is 1805 and the dielectric loss is 0.0150%. In the range of 1 MHz to 8 MHz, the dielectric constant is 1805 to 1551 and the dielectric loss is 0.0150% to 0.0152%.

[0088] Comparative Example 1

[0089] This comparative example provides a method for preparing magnesium ion and bismuth ion co-doped barium strontium titanate ceramics according to a traditional solid phase method, comprising:

[0090] Step 1, weigh 20g of pre-synthesized barium strontium titanate powder, 4g of magnesium hydroxide and 0.04g of bismuth oxide respectively, add them into an agate mortar in turn, grind for 2h, add PVA with a mass concentration of 5% during the grinding process to obtain a powder, and pass the powder through a 200-mesh sieve to obtain a mixture; the molecular weight of the PVA is 22000;

[0091] Step 2, uniaxial hot pressing and sintering the mixture, specifically comprising: placing the mixture in a hot pressing mold with a diameter of 13 mm, dry pressing at 120 MPa, debinding at 550° C., and obtaining a debinding sample;

[0092] Step 3: Place the debinding sample on a zirconia sintering plate, put it into a muffle furnace, heat it to 1250°C at a heating rate of 10°C / min, keep it warm for 4 hours for sintering, and cool it naturally after power off to obtain barium strontium titanate ceramics.

[0093] Step 5, the performance of the barium strontium titanate ceramic is evaluated, including: grinding and polishing the surface of the barium strontium titanate ceramic with sandpaper, testing the volume density of the sample by the Archimedes method, and calculating that its relative density is 96.5%; using an X-ray diffractometer to characterize its phase structure, the results are as follows Figure 1 As shown, it can be seen that the diffraction peaks are clear and sharp, indicating that the phase is well crystallized; the barium strontium titanate ceramic is polished, and a conductive silver paste is evenly coated on the surface of the barium strontium titanate ceramic after polishing. After drying, the ceramic is heat-treated at 850°C for 5 hours to obtain a silver-coated sample. The dielectric properties of the silver-coated sample are tested using an HP-4294A impedance analyzer. The results are as follows Figures 2 to 5 As shown, the results show that the dielectric constant at 1 MHz is 2060, and the dielectric loss is 0.0150%. In the range of 1 MHz to 8 MHz, the dielectric constant is 2060 to 813, and the dielectric loss is 0.084% to 0.082%.

[0094] Combining Examples 1 to 7 with Comparative Example 1, it can be seen that the low-frequency performance of the cold-sintered barium strontium titanate-based ceramics is comparable to that of the barium strontium titanate ceramics prepared by the conventional method, but the cold-sintered barium strontium titanate-based ceramics have better high-frequency performance. In the frequency range of 1 MHz to 8 MHz and the temperature range of 20° C. to 85° C., the dielectric constant is >1551, and the change rate is <10%, the dielectric loss is <0.02%, and the change rate is <30%; in addition, the sintering temperature of the cold-sintered ceramics is greatly reduced, such as Figure 7 As shown, it is shown that the energy consumption of cold-sintered ceramics prepared by the method of the present invention is greatly reduced, which is beneficial to achieving carbon emission reduction. When preparing MLCC devices, cheaper electrodes such as Ag and Cu can be used, and co-firing with other materials with lower melting points can be achieved. It is expected to be used in LTCC (Low Temperature Co-fired Ceramic) technology to explore new uses of barium strontium titanate ceramics.

[0095] Example 8

[0096] This embodiment provides a method for preparing a cold-sintered barium strontium titanate-based ceramic, comprising:

[0097] Step 1: Evenly mix the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant to form a mixture, specifically comprising: sequentially adding 20 g of the pre-synthesized barium strontium titanate powder, 5 g of magnesium hydroxide and 0.04 g of bismuth oxide into an agate mortar, grinding for 3 h, and dripping deionized water during the grinding process to obtain a mixture; the mass of the deionized water is 5 g; the pre-synthesized barium strontium titanate powder is a pre-synthesized barium strontium titanate powder obtained by a solid phase method commonly used in the art using barium carbonate, strontium carbonate and titanium dioxide as raw materials, and the solid phase synthesis includes processes such as ball milling, drying, calcining and grinding; the solid phase synthesis can be, for example: according to (Ba 0.7 Sr 0.3 ) TiO4 is prepared in a stoichiometric ratio, anhydrous ethanol is used as a grinding aid, zirconium oxide balls are used as ball milling media, and the mixture is ball milled in a planetary ball mill for 6 hours to obtain a ball milling slurry, the ball milling slurry is dried in an oven at 80° C., loaded into a zirconium oxide crucible, and placed in a muffle furnace at 1150° C. for calcination for 180 minutes, ground in a mortar for 2 hours, and passed through a 200-mesh sieve to obtain a pre-synthesized barium strontium titanate powder;

[0098] Step 2, uniaxial hot pressing and sintering the mixture, specifically comprising: placing the mixture in a hot pressing mold with a diameter of 13 mm, placing the hot pressing mold in a hot press, applying a uniaxial pressure of 400 MPa, heating to 200° C. at a heating rate of 2° C. / min, keeping the temperature for 30 minutes, turning off the power, removing the pressure, and naturally cooling to 50° C. to obtain a sample after uniaxial hot pressing and sintering;

[0099] Step 3, re-pressurizing and calcining the sample after uniaxial hot pressing sintering, specifically comprising: when the temperature of the hot press machine drops to 50°C, applying a uniaxial pressure of 300MPa, heating to 180°C at a heating rate of 2°C / min, keeping the temperature for 60min, turning off the power, removing the pressure, cooling naturally to room temperature, and drying until the residual water evaporates completely to obtain the sample after re-pressurizing and calcining; the drying temperature can be 120°C and the drying time can be 6h;

[0100] Step 4: annealing the sample after re-pressurization calcination, specifically comprising: placing the sample after re-pressurization calcination on a zirconia support plate, putting it into a muffle furnace, heating it to an annealing temperature of 900°C at a heating rate of 10°C / min, keeping it warm for 3 hours, and cooling it naturally after power off to obtain a cold-sintered barium strontium titanate-based ceramic.

[0101] The performance of the cold-sintered barium strontium titanate-based ceramic obtained in this example is basically consistent with that in Example 1.

[0102] Example 9

[0103] This embodiment provides a method for preparing a cold-sintered barium strontium titanate-based ceramic, comprising:

[0104] Step 1: Evenly mix the pre-synthesized barium strontium titanate powder, the intermediate liquid source and the dopant to form a mixture, specifically comprising: sequentially adding 20 g of the pre-synthesized barium strontium titanate powder, 5 g of magnesium hydroxide and 0.04 g of bismuth oxide to an agate mortar, grinding for 2.5 h, and dripping deionized water during the grinding process to obtain a mixture; the mass of the deionized water is 5 g; the pre-synthesized barium strontium titanate powder is a pre-synthesized barium strontium titanate powder obtained by a solid phase method commonly used in the art using barium carbonate, strontium carbonate and titanium dioxide as raw materials, and the solid phase synthesis includes ball milling, drying, calcining and grinding; the solid phase synthesis can be, for example: according to (Ba 0.7 Sr 0.3 ) TiO4 is prepared in a stoichiometric ratio, anhydrous ethanol is used as a grinding aid, zirconium oxide balls are used as ball milling media, and the mixture is ball milled in a planetary ball mill for 6 hours to obtain a ball milling slurry, the ball milling slurry is dried in an oven at 80° C., loaded into a zirconium oxide crucible, and placed in a muffle furnace at 1150° C. for calcination for 180 minutes, ground in a mortar for 2 hours, and passed through a 200-mesh sieve to obtain a pre-synthesized barium strontium titanate powder;

[0105] Step 2, uniaxial hot pressing and sintering the mixture, specifically comprising: placing the mixture in a hot pressing mold with a diameter of 13 mm, placing the hot pressing mold in a hot press, applying a uniaxial pressure of 600 MPa, heating to 180° C. at a heating rate of 4° C. / min, keeping the temperature for 60 min, turning off the power, removing the pressure, and naturally cooling to 50° C. to obtain a sample after uniaxial hot pressing and sintering;

[0106] Step 3, re-pressurizing and calcining the sample after uniaxial hot pressing sintering, specifically comprising: when the temperature of the hot press machine drops to 50°C, applying a uniaxial pressure of 500MPa, heating to 160°C at a heating rate of 4°C / min, keeping warm for 60min, turning off the power, removing the pressure, cooling naturally to room temperature, and drying until the residual water evaporates completely to obtain the sample after re-pressurizing and calcining; the drying temperature can be 120°C and the drying time can be 6h;

[0107] Step 4: annealing the sample after re-pressurization calcination, specifically comprising: placing the sample after re-pressurization calcination on a zirconia support plate, putting it into a muffle furnace, heating it to an annealing temperature of 850°C at a heating rate of 10°C / min, keeping it warm for 5 hours, and cooling it naturally after power off to obtain a cold-sintered barium strontium titanate-based ceramic.

[0108] The performance of the cold-sintered barium strontium titanate-based ceramic obtained in this example is basically consistent with that in Example 1.

[0109] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing cold-sintered barium strontium titanate-based ceramics, characterized in that: The cold-sintered barium strontium titanate-based ceramic has a relative density of 90.4% to 96.7%; a dielectric constant of 1805 to 2582 at 1 MHz, and a dielectric loss of 0.01% to 0.02%; a dielectric constant greater than 1551 with a variation rate of less than 10% and a dielectric loss of less than 0.02% with a variation rate of less than 30% within a frequency range of 1 MHz to 8 MHz and a temperature range of 20° C. to 85° C.; the method comprises mixing a raw material of pre-synthesized barium strontium titanate powder, an intermediate liquid source, and a dopant, uniaxially hot-pressing and sintering, then pressurizing and annealing to obtain the cold-sintered barium strontium titanate-based ceramic; the uniaxial hot-pressing and sintering temperature is 180° C. to 200° C. and the pressure is 300 MPa to 600 MPa, and the pressurizing and annealing temperature is 160° C. to 180° C. and the pressure is 200 MPa to 500 MPa; the intermediate liquid source is magnesium hydroxide or magnesium oxalate, and the dopant is bismuth oxide.

2. The method for preparing cold-sintered barium strontium titanate-based ceramics according to claim 1, characterized in that: The mass of the intermediate liquid source is 15% to 25% of the mass of the pre-synthesized barium strontium titanate powder, and the mass of the dopant is 0.2% of the mass of the pre-synthesized barium strontium titanate powder.

3. The method for preparing cold-sintered barium strontium titanate-based ceramics according to claim 1, characterized in that: The temperature of uniaxial hot pressing sintering is greater than the temperature of re-pressurizing calcining; the pressure of uniaxial hot pressing sintering is greater than the pressure of re-pressurizing calcining.

4. The method for preparing cold-sintered barium strontium titanate-based ceramics according to claim 1, wherein: Specifically include: Step 1: uniformly mixing the pre-synthesized barium strontium titanate powder, the intermediate liquid source, and the dopant to form a mixture; specifically, adding the pre-synthesized barium strontium titanate powder, the intermediate liquid source, and the dopant to a mortar in sequence, grinding for 2 to 3 hours, and adding deionized water dropwise during the grinding process to obtain a mixture; Step 2: uniaxially hot pressing and sintering the mixture to obtain a uniaxially hot pressed and sintered sample; Step 3, pressurizing and calcining the sample after uniaxial hot pressing to obtain a pressurized and calcined sample; Step 4: Annealing the sample after pressurized calcination to obtain cold-sintered barium strontium titanate-based ceramics.

5. The method for preparing cold-sintered barium strontium titanate-based ceramics according to claim 4, characterized in that: In step 1, the mass of the deionized water is 15% to 25% of the mass of the pre-synthesized barium strontium titanate powder.

6. The method for preparing cold-sintered barium strontium titanate-based ceramics according to claim 4, characterized in that: Step 2 specifically includes: placing the mixed material in a hot pressing mold, placing the hot pressing mold in a hot press, applying 300MPa~600MPa uniaxial pressure, heating to 180℃~200℃ at a heating rate of 2℃ / min~4℃ / min, keeping warm for 30min~90min, turning off the power, releasing the pressure, and cooling to obtain a sample after uniaxial hot pressing sintering.

7. The method for preparing the cold-sintered barium strontium titanate-based ceramic according to any one of claims 4 to 6, characterized in that: In step three, the uniaxial pressure of the re-pressurized calcination is 200 MPa~500 MPa, the heating rate is 2°C / min~4°C / min, the temperature of the re-pressurized calcination is 160°C~180°C, and the holding time is 30min~90min.

8. The method for preparing cold-sintered barium strontium titanate-based ceramics according to claim 7, characterized in that: The temperature of uniaxial hot pressing sintering is greater than the temperature of re-pressurizing calcining; the pressure of uniaxial hot pressing sintering is greater than the pressure of re-pressurizing calcining.

9. The method for preparing cold-sintered barium strontium titanate-based ceramics according to claim 4, characterized in that: In step 4, the annealing temperature is 850°C to 950°C, and the holding time is 3h to 5h.