A Low-Temperature Metal-Air Battery Catalyst, Its Preparation Method and Application
By preparing an N-doped C-layer-coated FeCo alloy catalyst, the problem of poor discharge performance of metal-air batteries at low temperatures was solved, achieving efficient low-temperature oxygen reduction reaction and long-life battery performance.
Patent Information
- Application Number
- CN202311482356.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-08
AI Technical Summary
The lack of effective low-temperature oxygen reduction reaction catalysts in current technologies results in poor discharge performance of metal-air batteries at low temperatures.
A nitrogen-doped carbon-coated FeCo alloy catalyst, abbreviated as FeCo@NC, was prepared by calcining and acid washing after mixing polyvinylpyrrolidone, melamine, iron salt and cobalt salt. The electronic structure of the catalyst was adjusted to improve its low-temperature activity.
Under low-temperature conditions, the FeCo@NC catalyst exhibits highly efficient 4-electron oxygen reduction reaction activity, and the assembled metal-air battery achieves a power density of up to 117.6 mW/cm2 at -40℃ and a cycle life of up to 300 hours.
Smart Images

Figure CN117317263B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery catalyst technology, and in particular to a low-temperature metal-air battery catalyst, its preparation method, and its application. Background Technology
[0002] Electrical energy is an economical, practical, clean, and easily controlled and converted form of energy. Metal-air batteries are a common type of energy conversion device, offering advantages such as no pollution, stable discharge, high specific energy, and low price, making them an ideal alternative to traditional batteries. Metal-air batteries use metal and oxygen as fuel, converting their chemical energy into electrical energy. They have low raw material costs, a relatively simple battery structure, and their active material is derived from oxygen in the air, with a specific energy exceeding 1000 Wh / kg. Therefore, metal-air batteries have broad development prospects in the energy storage field.
[0003] However, metal-air batteries exhibit poor discharge performance at low temperatures, and there is still a lack of research on the reaction kinetics of slow oxygen reduction reaction (ORR) at low temperatures, as well as a lack of effective low-temperature ORR catalysts. Therefore, it is urgent to explore the reaction kinetics at low temperatures and develop high-performance low-temperature ORR catalysts. To address these issues, previous researchers have conducted extensive studies, including vacancy modulation of perovskite oxides, where the introduced oxygen vacancies reduce the oxidation state of the metal, decrease the coordination number, and increase the coordination bond length (Adv. Mater., 2023, 35, 2303109); constructing Fe-Se diatomic dispersed catalysts, where the electronic hybridization of asymmetrically coordinated Fe-Se sites optimizes the adsorption / desorption behavior between the active site and the intermediate (Angew. Chem. Int. Ed. 2023, e202219191); and electronic modulation based on adjacent metal nanoclusters, where the electron enrichment of adjacent Fe nanoclusters reduces the magnetic moment of Fe single atoms, enhancing catalytic activity (Appl. Cata. B, 2023, 323, 122163). To date, there is still no clear method for preparing high-efficiency low-temperature metal-air battery catalysts using transition metal alloys and nitrogen-doped carbon layers. Therefore, developing a highly active and inexpensive low-temperature metal-air battery catalyst to address the poor performance of metal-air batteries at low temperatures is a problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0004] The purpose of this invention is to provide a low-temperature metal-air battery catalyst, its preparation method, and its application, so as to solve the problem of poor discharge performance of metal-air batteries under low-temperature conditions.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0006] This invention provides a method for preparing a low-temperature metal-air battery catalyst, comprising the following steps:
[0007] 1) Mix polyvinylpyrrolidone, melamine, iron salt, cobalt salt and water, and then dry to obtain the precursor;
[0008] 2) The precursor was calcined and acid-washed to obtain a low-temperature metal-air battery catalyst.
[0009] Preferably, the ferric salt in step 1) comprises one or more of ferric nitrate, ferric sulfate, and ferric chloride;
[0010] The cobalt salt comprises one or more of cobalt nitrate, cobalt sulfate, and cobalt chloride.
[0011] Preferably, in step 1), the mass ratio of polyvinylpyrrolidone, melamine, iron salt, cobalt salt and water is 0.3-0.8:0.3-0.8:0.3-0.8:0.3-0.8:30-60.
[0012] Preferably, the calcination temperature in step 2) is 750–850°C, the calcination time is 1–3 h, and the calcination atmosphere is an inert atmosphere.
[0013] Preferably, the pickling temperature in step 2) is 90-110°C, and the pickling time is 12-36 hours.
[0014] The present invention also provides a low-temperature metal-air battery catalyst prepared by the above-described method for preparing a low-temperature metal-air battery catalyst.
[0015] The present invention also provides an application of the above-mentioned low-temperature metal-air battery catalyst in an air-metal battery.
[0016] The present invention has at least the following beneficial effects:
[0017] 1. This invention provides a synthetic route for preparing low-temperature metal-air battery catalysts. The target product is obtained using a simple one-step method. The preparation process is simple and easy to mass-produce. Furthermore, the electronic structure of the catalyst is adjusted during the preparation process, enabling it to maintain excellent electrochemical performance at low temperatures (-40℃).
[0018] 2. Electrocatalytic 4-electron oxygen reduction reaction (4e - ORR (Ortho-Ortho-Reaction) is the most important cathode reaction in metal-air batteries, and a crucial element in designing metal-air batteries with high energy density and long cycle life. However, 4e -ORR (Orthogonal Orthogonal Reaction) is limited by the slowed molecular thermal motion at low temperatures, leading to a reduced rate of intermediate formation and becoming a decisive step affecting the overall reaction rate. The formation of the *OOH intermediate and its further protonation or dissociation are the main determinants of the ORR reaction rate. The ORR reaction rate is closely related to the power density of metal-air batteries; a limited reaction rate prevents the achievement of high power densities. The low-temperature metal-air battery catalyst prepared in this invention is an N-doped C-layer-coated FeCo alloy catalyst (FeCo@NC), which exhibits highly efficient 4e⁻ regeneration. - ORR activity was observed, and the metal-air battery assembled at -40°C exhibited a power density as high as 117.6 mW / cm². Variations in the FeCo alloy ratio modulated the electronic structure at the N site, leading to charge accumulation at the N element driven by the work function difference, thereby modulating the catalyst's adsorption and conversion behavior for oxygen. Attached Figure Description
[0019] Figure 1 The images shown are transmission electron microscope (TEM) images of the low-temperature metal-air battery catalyst prepared in Example 1, where a and b are TEM images at different magnifications.
[0020] Figure 2 The images shown are high-angle annular dark-field transmission electron microscope (HAADF-TEM) images of the low-temperature metal-air battery catalyst prepared in Example 1, where a is a transmission electron microscope image, b is a C elemental mapping image, c is a N elemental mapping image, d is a Fe elemental mapping image, e is a Co elemental mapping image, and f is a C, N, Fe and Co elemental mapping image.
[0021] Figure 3 The X-ray diffraction (XRD) patterns of the low-temperature metal-air battery catalysts prepared in Example 1 and Comparative Examples 1-2 are shown.
[0022] Figure 4 The electronic structure regulation characterization diagrams of the low-temperature metal-air battery catalysts prepared in Example 1 and Comparative Examples 1-2 are shown, where a is an X-ray photoelectron spectroscopy (XPS) diagram and b is a statistical diagram of different N species.
[0023] Figure 5 The graphs show the electrochemical performance test results of the low-temperature metal-air battery catalysts prepared in Example 1 and Comparative Examples 1-2, where a is the polarization curve, b is the Tafel slope graph, c is the power density graph, and d is the recycling curve. Detailed Implementation
[0024] This invention provides a method for preparing a low-temperature metal-air battery catalyst, comprising the following steps:
[0025] 1) Mix polyvinylpyrrolidone, melamine, iron salt, cobalt salt and water, and then dry to obtain the precursor;
[0026] 2) The precursor was calcined and acid-washed to obtain a low-temperature metal-air battery catalyst.
[0027] In this invention, the ferric salt in step 1) includes one or more of ferric nitrate, ferric sulfate, and ferric chloride;
[0028] The cobalt salt comprises one or more of cobalt nitrate, cobalt sulfate, and cobalt chloride.
[0029] In this invention, the mass ratio of polyvinylpyrrolidone, melamine, iron salt, cobalt salt and water in step 1) is 0.3-0.8:0.3-0.8:0.3-0.8:0.3-0.8:30-60, preferably 0.4-0.7:0.4-0.7:0.4-0.7:0.4-0.7:35-55, more preferably 0.5-0.6:0.5-0.6:0.5-0.6:0.5-0.6:40-50, and even more preferably 0.5:0.5:0.5:0.5:45.
[0030] In this invention, the mixing temperature in step 1) is preferably 75-85°C, more preferably 78-82°C, and even more preferably 80°C; the mixing time is preferably 12-36h, more preferably 15-30h, even more preferably 18-28h, and even more preferably 20-24h.
[0031] In this invention, the drying in step 1) is preferably carried out under vacuum conditions, the drying temperature is preferably 50-70°C, more preferably 55-65°C, even more preferably 58-63°C, and even more preferably 60°C; the drying time is preferably 24-48h, more preferably 28-42h, even more preferably 32-38h, and even more preferably 34-36h.
[0032] In this invention, the calcination temperature in step 2) is 750–850°C, preferably 770–830°C, more preferably 780–810°C, and even more preferably 790–800°C; the calcination time is 1–3 h, preferably 1.5–2.5 h, more preferably 1.8–2.2 h, and even more preferably 2 h; the calcination atmosphere is an inert atmosphere, which can specifically be one or more of nitrogen, helium, neon, and argon.
[0033] In this invention, the heating rate of the calcination is preferably 3-10°C / min, more preferably 4-9°C, even more preferably 5-8°C / min, and even more preferably 6-7°C.
[0034] In this invention, the pickling temperature in step 2) is 90-110°C, preferably 93-108°C, more preferably 95-105°C, and even more preferably 98-102°C; the pickling time is 12-36 hours, preferably 14-35 hours, even more preferably 18-32 hours, more preferably 22-28 hours, and even more preferably 24-26 hours.
[0035] In this invention, the pickling is preferably performed using a hydrochloric acid solution, wherein the concentration of the hydrochloric acid solution is preferably 1-3 mol / L, more preferably 1.5-2.5 mol / L, and even more preferably 1.8-2.2 mol / L.
[0036] In this invention, after acid washing, the low-temperature metal-air battery catalyst is preferably washed and dried with deionized water, wherein the washing is performed with deionized water until neutral; the drying temperature is 50-70°C, preferably 55-65°C, more preferably 58-62°C, and even more preferably 60°C.
[0037] The present invention also provides a low-temperature metal-air battery catalyst prepared by the above-described method for preparing a low-temperature metal-air battery catalyst.
[0038] The present invention also provides an application of the above-mentioned low-temperature metal-air battery catalyst in an air-metal battery.
[0039] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0040] Example 1
[0041] Dissolve 0.6 g of polyvinylpyrrolidone in 40 mL of deionized water, then add 0.6 g of melamine and stir until completely dispersed to obtain a mixed solution. Add 0.5 g of ferric nitrate nonahydrate and 0.5 g of cobalt nitrate hexahydrate to the above mixed solution and stir until completely dispersed. Then, magnetically stir in an oil bath at 80 °C for 24 h until the solvent is completely evaporated. Transfer the solution to a vacuum drying oven and dry at 60 °C for 36 h to obtain the precursor.
[0042] The precursor was ground into powder and placed in a calcination apparatus with argon as a protective gas. The temperature was increased to 800℃ at a rate of 5℃ / min and calcined for 2 hours. The powder was then removed and acid-washed with 3mol / L hydrochloric acid at 100℃ for 24 hours. After acid washing, it was washed four times with deionized water until the washing solution was neutral. The powder was then dried in a vacuum drying oven at 60℃ for 24 hours to obtain the low-temperature metal-air battery catalyst.
[0043] The low-temperature metal-air battery catalyst prepared in this example was characterized using transmission electron microscopy, and the results are as follows: Figures 1-2As shown. Figure 1 In the image, 'a' is a TEM image of the catalyst magnified 100k times, and 'b' is a TEM image of the catalyst magnified 400k times. Figure 2 The images show HAADF-TEM images of the catalysts described above, where a is a transmission electron microscope image of the catalyst magnified 45kx, b is the elemental mapping map of C, c is the elemental mapping map of N, d is the elemental mapping map of Fe, e is the elemental mapping map of Co, and f is the elemental mapping map of C, N, Fe, and Co. Combined with... Figure 1 and Figure 2 It can be seen that the catalyst is an ultrathin nanosheet structure with defects, and the carbon matrix is uniformly doped with C and N elements, forming a structure of metal particles loaded on layered graphene.
[0044] Example 2
[0045] Dissolve 0.3g of polyvinylpyrrolidone in 40mL of deionized water, then add 0.4g of melamine and stir until completely dispersed to obtain a mixed solution. Add 0.5g of ferric nitrate nonahydrate and 0.5g of cobalt nitrate hexahydrate to the above mixed solution and stir until completely dispersed. Then, magnetically stir in an oil bath at 75℃ for 28h until the solvent is completely evaporated. Transfer the solution to a vacuum drying oven and dry at 50℃ for 42h to obtain the precursor.
[0046] The precursor was ground into powder and placed in a calcination apparatus with helium as a protective gas. The temperature was increased to 780°C at a rate of 6°C / min and calcined for 2.2 h. The powder was then removed and acid-washed with 1 mol / L hydrochloric acid at 110°C for 20 h. After acid washing, it was washed three times with deionized water until the washing solution was neutral. The powder was then dried in a vacuum drying oven at 65°C for 24 h to obtain the low-temperature metal-air battery catalyst.
[0047] Example 3
[0048] Dissolve 0.8 g of polyvinylpyrrolidone in 40 mL of deionized water, then add 0.8 g of melamine and stir until completely dispersed to obtain a mixed solution. Add 0.4 g of ferric nitrate nonahydrate and 0.4 g of cobalt nitrate hexahydrate to the above mixed solution and stir until completely dispersed. Then, magnetically stir in an oil bath at 85 °C for 15 h until the solvent is completely evaporated. Transfer the solution to a vacuum drying oven and dry at 50 °C for 48 h to obtain the precursor.
[0049] The precursor was ground into powder and placed in a calcination apparatus with argon as a protective gas. The temperature was increased to 830°C at a rate of 7°C / min and calcined for 1.8 h. The powder was then removed and acid-washed with 2 mol / L hydrochloric acid at 90°C for 18 h. After acid washing, it was washed four times with deionized water until the washing solution was neutral. The powder was then dried in a vacuum drying oven at 60°C for 24 h to obtain the low-temperature metal-air battery catalyst.
[0050] Example 4
[0051] Dissolve 0.5g of polyvinylpyrrolidone in 40mL of deionized water, then add 0.6g of melamine and stir until completely dispersed to obtain a mixed solution. Add 0.3g of ferric nitrate nonahydrate and 0.4g of cobalt nitrate hexahydrate to the above mixed solution and stir until completely dispersed. Then, magnetically stir in an oil bath at 80℃ for 24h until the solvent is completely evaporated. Transfer the solution to a vacuum drying oven and dry at 65℃ for 36h to obtain the precursor.
[0052] The precursor was ground into powder and placed in a calcination apparatus with argon as a protective gas. The temperature was increased to 850°C at a rate of 10°C / min and calcined for 1.5 h. The powder was then removed and acid-washed with 3 mol / L hydrochloric acid at 95°C for 24 h. After acid washing, it was washed five times with deionized water until the washing solution was neutral. The powder was then dried in a vacuum drying oven at 65°C for 28 h to obtain the low-temperature metal-air battery catalyst.
[0053] Example 5
[0054] Dissolve 0.6 g of polyvinylpyrrolidone in 40 mL of deionized water, then add 0.6 g of melamine and stir until completely dispersed to obtain a mixed solution. Add 0.6 g of ferric nitrate nonahydrate and 0.6 g of cobalt nitrate hexahydrate to the above mixed solution and stir until completely dispersed. Then, magnetically stir in an oil bath at 82 °C for 28 h until the solvent is completely evaporated. Transfer the solution to a vacuum drying oven and dry at 60 °C for 40 h to obtain the precursor.
[0055] The precursor was ground into powder and placed in a calcination apparatus with nitrogen as a protective gas. The temperature was increased to 750°C at a rate of 3°C / min and calcined for 2 hours. The powder was then removed and acid-washed with 3 mol / L hydrochloric acid at 90°C for 20 hours. After acid washing, it was washed four times with deionized water until the washing solution was neutral. The powder was then dried in a vacuum drying oven at 60°C for 24 hours to obtain the low-temperature metal-air battery catalyst.
[0056] Compare with Example 1
[0057] The only difference between this comparative example and Example 1 is that the amount of ferric nitrate nonahydrate added is 0.1g and the amount of cobalt nitrate hexahydrate added is 0.9g; the other operating steps and parameters are the same.
[0058] Compare with Example 2
[0059] The only difference between this comparative example and Example 1 is that the amount of ferric nitrate nonahydrate added is 0.9g and the amount of cobalt nitrate hexahydrate added is 0.1g. All other operating steps and parameters are the same.
[0060] X-ray diffraction experiments were performed on the low-temperature metal-air battery catalysts prepared in Example 1, Comparative Example 1, and Comparative Example 2. The results are as follows: Figure 3 As shown, from Figure 3 As can be seen from the data, the material prepared in Example 1 shows two XRD diffraction peaks at 44.82° and 65.37°, which represent the (110) and (002) crystal planes of the FeCo alloy, respectively.
[0061] X-ray photoelectron spectroscopy (XPS) experiments were conducted on the low-temperature metal-air battery catalysts prepared in Example 1, Comparative Example 1, and Comparative Example 2. Figure 4 In the spectrum 'a', the area of each peak represents the content of each N species, and the position of each peak represents the energy level of that N species. It can be found that by comparing the energy levels of Example 1, Comparative Example 1 and Comparative Example 2, the peak position of Example 1 shows a significant shift, indicating that the present invention effectively adjusts the charge structure by adjusting the addition ratio of cobalt and iron elements. Figure 4 b in the text is a pair Figure 4 By statistically analyzing the integral results of the peak areas in the spectrum of 'a', the relative contents of different N species were obtained.
[0062] The low-temperature metal-air battery catalysts prepared in Example 1, Comparative Example 1, and Comparative Example 2 were subjected to rotating disk annular electrode (RRDE) testing, using a 0.1M KOH solution containing saturated O2 as the electrolyte. The rotation speed was 1600 rpm, and ORR current polarization curves were obtained on the disk electrode. The results are as follows. Figure 5 As shown in a. Test results show that the half-wave potential of Example 1 is 0.904V vs. RHE, the half-wave potential of Control Example 1 is 0.790V vs. RHE, and the half-wave potential of Control Example 2 is 0.802V vs. RHE. It can be seen that the half-wave potential of Example 1 is significantly higher than that of Control Example 1 and Control Example 2. Figure 5 In the figure, b represents the calculated Tafel slope, which shows that the catalyst prepared in Example 1 is more conducive to the ORR process.
[0063] The low-temperature metal-air battery catalyst prepared in Example 1 was used as the cathode catalyst to assemble a metal-air battery. The specific assembly method is as follows: 5.0 mg of catalyst was dispersed in a mixed solution of 480 μL deionized water / isopropanol (volume ratio 3:7) and 20 μL naphthol to obtain a catalyst slurry; the catalyst slurry was uniformly coated on carbon paper and then dried at 80 °C for 2 h to obtain the cathode of the air electrode, with a catalyst composite amount of 0.2 mg / cm³. 2 A zinc-air battery was assembled using a zinc plate as the anode and a catalyst supported on carbon paper as the cathode in a 0.1 MkOH solution. The power density of this self-made zinc-air battery was tested in constant temperature chambers at different temperatures (e.g.,...). Figure 5 (as shown in c) and cycle life (as shown in c) Figure 5 (as shown in d), from Figure 5 It can be seen that this metal-air battery still exhibits a power output of 117.6 mW / cm² at -40℃. 2 Power density, compared to the power density at room temperature (25℃, 145.2 mW / cm³). 2 The degradation rate was only 18.7%; and the battery has a cycle life of over 300 hours at -40°C, demonstrating excellent low-temperature operating life.
[0064] The above experimental results show that the low-temperature metal-air battery catalyst material of this invention is prepared by a one-step method, and its structure is an N-doped carbon layer encapsulating an FeCo alloy (FeCo@NC). This catalyst has high efficiency in 4e-ionization. - The catalyst exhibits excellent ORR activity and good low-temperature stability after being assembled into a metal-air battery. The change in the Fe / Co ratio modulates the controllable alteration of its charge structure; driven by the difference in work function, charge accumulation at the N element regulates the catalyst's oxygen adsorption and conversion behavior. The FeCo@NC catalyst possesses excellent 4e... - The catalytic activity of ORR was demonstrated in the RRDE current polarization curve tests compared with Control Examples 1 and 2, showing an excellent reaction half-wave potential (0.904 V vs. RHE). The FeCo@NC catalyst achieved a 68 mV / dec reaction in Tafel tests. -1 The test results show that it exhibits optimal reaction kinetics. Furthermore, when the FeCo@NC catalyst was applied as a cathode catalyst in a metal-air battery, its peak power density exceeded 117.6 mW / cm² in a low-temperature (-40℃) metal-air battery. 2 The cycle time can reach 300 h. Experimental and characterization results show that FeCo@NC is a promising new type of low-temperature metal-air battery cathode catalyst, which is expected to exhibit superior performance in practical production. This work not only provides a simple strategy for developing N-doped carbon-coated alloys, but also offers a new approach to the design of low-temperature metal-air battery catalysts.
[0065] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for producing a catalyst for a low temperature metal-air battery, characterized by, Includes the following steps: 1) Mix polyvinylpyrrolidone, melamine, iron salt, cobalt salt and water, and then dry to obtain the precursor; 2) The precursor was calcined and acid-washed to obtain a low-temperature metal-air battery catalyst; In step 1), the mass ratio of polyvinylpyrrolidone, melamine, iron salt, cobalt salt, and water is 0.3~0.8:0.3~0.8:0.3~0.8:30~60. In step 2), the calcination temperature is 750~850℃, the calcination time is 1~3h, and the calcination atmosphere is an inert atmosphere.
2. The method for preparing a low-temperature metal-air battery catalyst according to claim 1, characterized in that, In step 1), the iron salt contains one or more of ferric nitrate, ferric sulfate, and ferric chloride. The cobalt salt comprises one or more of cobalt nitrate, cobalt sulfate, and cobalt chloride.
3. The method for preparing a low-temperature metal-air battery catalyst according to claim 2, characterized in that, In step 2), the pickling temperature is 90~110℃ and the pickling time is 12~36h.
4. The low-temperature metal-air battery catalyst prepared by the method described in any one of claims 1 to 3.
5. The application of the low-temperature metal-air battery catalyst according to claim 4 in air-metal batteries.
Citation Information
Patent Citations
Bifunctional oxygen evolution-oxygen reduction catalytic material CoFe@NC, and preparation method and application thereof
CN110354884A
FeCo-coated NC core-shell structure catalyst, preparation method and application of FeCo-coated NC core-shell structure catalyst in seawater electrolysis hydrogen production
CN114561651A