A 3D printed composite solid electrolyte and its preparation method and application
The preparation of porous composite solid electrolytes through 3D printing technology solves the brittleness and interface resistance problems of traditional ceramic solid-state lithium batteries, achieves 3D contact of electrodes/electrolytes, and improves the energy density and cycle stability of lithium batteries.
Patent Information
- Application Number
- CN202311525273.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-11-15
AI Technical Summary
Traditional ceramic solid-state lithium batteries have problems such as high brittleness, difficulty in processing, and high interfacial resistance at the solid-solid interface, which affects their cycle life and energy density. Moreover, the solid electrolyte with a planar structure is difficult to adapt to the volume expansion of the electrode.
A composite solid electrolyte with a symmetrical porous structure is prepared through 3D printing technology. Lithium bistrifluoromethanesulfonyl imide, photosensitive resin and inorganic oxide ceramic nanoparticles are used to construct a printing slurry, which is cured by UV light to form a solid structure in the middle layer and The upper and lower layers of porous structure realize 3D contact of electrode/electrolyte, increasing the contact area and active material loading capacity.
It improves the energy density and ion migration capability of solid-state lithium batteries, reduces the interface impedance, and enhances the cycle stability and Coulombic efficiency of the battery.
Smart Images

Figure CN117374385B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid electrolytes, and in particular to a 3D printed composite solid electrolyte and a preparation method and application thereof. Background Art
[0002] As an important part of the development of clean energy, electrochemical energy storage systems such as lithium batteries are of great significance to promoting the green transformation of energy and helping to achieve the "dual carbon" goals. Due to the risks of traditional liquid lithium batteries, the development of solid-state lithium batteries with high energy density and high safety has become an inevitable trend. Solid electrolytes are the core components of solid-state lithium batteries. Among the solid electrolytes currently studied, ceramic solid electrolytes represented by garnet-type LLZO have attracted much attention due to their high ionic conductivity, wide electrochemical window and simple preparation methods. However, traditional ceramic solid electrolytes have problems such as high brittleness and difficulty in processing, and the contact with the electrode changes from a solid-liquid interface to a solid-solid interface, which will cause a large interface resistance between the electrolyte and the electrode, hindering the ion transport at the interface, making it difficult to adapt to the volume expansion of the electrode during the cycle, and the stability is poor.
[0003] At the same time, traditional solid electrolytes are mostly planar structures, so the contact between the electrode and the electrolyte is planar contact, which will also cause high interface resistance at the solid-solid interface, which will greatly affect the cycle life and energy density of solid-state lithium batteries. Among various solid electrolyte preparation technologies, 3D printing technology has the advantages of low cost, rapid prototyping, controllable geometric structure, and simple process. It is an important means of preparing 3D structural materials and has injected new vitality into the development of the energy storage field.
[0004] In recent years, ionic liquids have attracted much attention due to their unique advantages such as high conductivity, high thermal stability, low volatility and non-flammability. Immobilizing ionic liquids on a solid matrix to construct ion gel electrolytes has also become an important way to solve interface problems. Therefore, preparing ion gel-encapsulated ceramic electrolytes with symmetrical 3D structures through 3D printing technology is one of the effective ways to obtain high-performance solid-state lithium batteries. Summary of the invention
[0005] The purpose of the present invention is to provide a 3D printed composite solid electrolyte and its preparation method and application. The electrode / electrolyte in the battery prepared by the porous composite solid electrolyte is in 3D contact, which provides an open space for electrode filling, greatly increases the contact area between the electrolyte and the electrode, increases the active material loading, reduces the interface impedance, and realizes precise regulation of the interface structure and performance, thereby effectively improving the energy density of the solid-state lithium battery.
[0006] To achieve the above object, the present invention provides a method for preparing a 3D printed composite solid electrolyte, comprising the following steps:
[0007] S1. Adding lithium bis(trifluoromethanesulfonyl)imide into the ionic liquid solution and stirring evenly to obtain a mixed solution A with a concentration of 0.5 to 3 mol / L;
[0008] S2, adding the photosensitive resin and the initiator into the mixed solution A in S1 at a mass ratio of 100:1, and stirring to obtain a mixed solution B;
[0009] S3, adding inorganic oxide ceramic nanoparticles into the mixed solution B in S2 three times, and mixing them evenly to obtain a printing slurry;
[0010] S4: Place the printing paste in S3 into the printing tank, and use the UV laser power of 500-3000mW / cm 2 Under the condition of light-curing 3D printing, layer by layer is carried out, and a composite solid electrolyte with a symmetrical porous structure is obtained after cleaning.
[0011] Preferably, in S1, the ionic liquid is one or more of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide, 1-methyl-1-propylpyrrolidine bis(trifluoromethanesulfonyl)imide, 1-n-butyl-1-methylpyrrolidine di(trifluoromethylsulfonyl)imide and 1-butyl-1-methylpyrrolidine bis(trifluoromethanesulfonyl)imide.
[0012] Preferably, in S2, the photosensitive resin is at least one of ethoxylated trimethylolpropane triacrylate, 1,6-hexanediol diacrylate and polyethylene glycol diacrylate.
[0013] Preferably, in S2, the initiator is one or more of 2-hydroxy-2-methyl-1-phenylacetone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide.
[0014] Preferably, in S2, the amount of the photosensitive resin used is 5-40 wt % of the mixed solution A.
[0015] Preferably, in S3, the inorganic oxide ceramic nanoparticles are one or more of lithium lanthanum zirconium oxide ceramic nanoparticles, tantalum-doped lithium lanthanum zirconium oxide ceramic nanoparticles, aluminum-doped lithium lanthanum zirconium oxide ceramic nanoparticles, niobium-doped lithium lanthanum zirconium oxide ceramic nanoparticles, lithium aluminum titanium phosphate ceramic nanoparticles and lanthanum lithium titanate ceramic nanoparticles.
[0016] Preferably, in S3, the amount of inorganic oxide ceramic nanoparticles used is 5 to 40 wt % of the mixed solution B.
[0017] The composite solid electrolyte prepared by the above-mentioned method for preparing a 3D printed composite solid electrolyte: the structure of the composite solid electrolyte printed by photocuring 3D printing is that the middle layer is a solid structure, and the upper and lower layers are symmetrical porous structures.
[0018] Application of the above composite solid electrolyte: The composite solid electrolyte is used in the preparation of batteries.
[0019] Therefore, the beneficial effects of the present invention are:
[0020] 1. Personalized customization of composite solid electrolyte microstructure is achieved through photocuring 3D printing technology, including parameters such as thickness of each electrolyte layer, pore shape, pore size, and pore spacing. Porous composite solid electrolytes can transform the planar contact of electrode / electrolyte into 3D contact, thereby providing an open space for electrode filling, greatly increasing the contact area between electrolyte and electrode, increasing the loading amount of active substances, reducing interface impedance, achieving precise regulation of interface structure and performance, and improving the energy density of solid-state lithium batteries;
[0021] 2. Ionic liquids themselves have excellent ion transport properties. The ion gel-ceramic composite solid electrolyte composed of them can also achieve strong interaction between ion gel and inorganic oxide nanoparticles. This unique composite solid electrolyte structure can increase the number of freely moving lithium ions and promote ion transport, thereby improving the ion migration and transport capabilities of solid-state lithium batteries.
[0022] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is an optical image of the porous composite solid electrolyte prepared in Example 1 of the present invention;
[0024] Figure 2 is a scanning electron microscope image of the porous composite solid electrolyte prepared in Example 1 of the present invention;
[0025] Figure 3 is a scanning electron microscope image of the non-porous composite solid electrolyte prepared in Comparative Example 1 of the present invention;
[0026] Figure 4 It is a charge and discharge test chart of the porous composite solid electrolyte prepared in Example 4 of the present invention and the non-porous composite solid electrolyte prepared in Comparative Example 1 at 0.5C. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.
[0028] The present invention can be explained in more detail by the following examples. The purpose of disclosing the present invention is to protect all changes and improvements within the scope of the present invention. The present invention is not limited to the following examples.
[0029] Example 1
[0030] S1. Add lithium bis(trifluoromethanesulfonyl imide) to 1-ethyl-3-methylimidazole bis(trifluoromethanesulfonyl imide) salt, stir at room temperature for 3 hours, and after stirring evenly, obtain a mixed solution A with a concentration of 0.5 mol / L.
[0031] S2. Add ethoxylated trimethylolpropane triacrylate and 2-hydroxy-2-methyl-1-phenylacetone into the mixed solution A in S1 at a mass ratio of 100:1, and stir evenly at room temperature to obtain a mixed solution B.
[0032] The amount of ethoxylated trimethylolpropane triacrylate used is 5 wt % of the mixed solution A.
[0033] S3, adding lithium lanthanum zirconium oxide ceramic nanoparticles into the mixed solution B in S2 three times, stirring at room temperature, and mixing evenly to obtain a printing slurry.
[0034] The amount of lithium lanthanum zirconium oxide ceramic nanoparticles used is 5wt% of the mixed solution B.
[0035] S4: Place the printing paste in S3 into the printing tank, and use a UV laser power of 500mW / cm 2 The model is built according to the needs and light-curing 3D printing is performed layer by layer. After printing, the porous composite solid electrolyte is removed and the uncured printing slurry on the surface is cleaned. After cleaning, a composite solid electrolyte with a symmetrical porous structure is obtained.
[0036] like Figure 1 As shown, the composite solid electrolyte prepared in this embodiment has good flexibility. Figure 2 As shown, the honeycomb-shaped composite solid electrolyte has a uniformly distributed pore structure, which can serve as a 3D space for filling electrodes.
[0037] Example 2
[0038] S1. Add lithium bis(trifluoromethanesulfonyl)imide to 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide salt, stir at room temperature for 3 hours, and after stirring evenly, obtain a mixed solution A with a concentration of 1 mol / L.
[0039] S2. Add 1,6-hexanediol diacrylate and diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide into the mixed solution A in S1 at a mass ratio of 100:1, and stir evenly at room temperature to obtain a mixed solution B.
[0040] The amount of 1,6-hexanediol diacrylate used is 10 wt % of the mixed solution A.
[0041] S3, adding aluminum-doped lithium lanthanum zirconium oxide ceramic nanoparticles into the mixed solution B in S2 three times, stirring at room temperature, and mixing evenly to obtain a printing slurry.
[0042] The amount of aluminum-doped lithium lanthanum zirconium oxide ceramic nanoparticles used is 10 wt % of the mixed solution B.
[0043] S4: Place the printing paste in S3 into the printing tank, and use a UV laser power of 1000mW / cm 2 The model is built according to the needs and light-curing 3D printing is performed layer by layer. After printing, the porous composite solid electrolyte is removed and the uncured printing slurry on the surface is cleaned. After cleaning, a composite solid electrolyte with a symmetrical porous structure is obtained.
[0044] Example 3
[0045] S1. Add lithium bis(trifluoromethanesulfonyl)imide to 1-methyl-1-propylpyrrolidine bis(trifluoromethanesulfonyl)imide salt, stir at room temperature for 3 h, and after stirring evenly, obtain a mixed solution A with a concentration of 2 mol / L.
[0046] S2. Add polyethylene glycol diacrylate and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide into the mixed solution A in S1 at a mass ratio of 100:1, and stir evenly at room temperature to obtain a mixed solution B.
[0047] The amount of polyethylene glycol diacrylate used is 25 wt % of the mixed solution A.
[0048] S3, adding lithium aluminum titanium phosphate ceramic nanoparticles into the mixed solution B in S2 three times, stirring at room temperature, and mixing evenly to obtain a printing slurry.
[0049] The amount of lithium aluminum titanium phosphate ceramic nanoparticles used is 30wt% of the mixed solution B.
[0050] S4: Place the printing paste in S3 into the printing tank, and use a UV laser power of 2000mW / cm 2 The model is built according to the needs and light-curing 3D printing is performed layer by layer. After printing, the porous composite solid electrolyte is removed and the uncured printing slurry on the surface is cleaned. After cleaning, a composite solid electrolyte with a symmetrical porous structure is obtained.
[0051] Example 4
[0052] S1. Add lithium bis(trifluoromethanesulfonyl)imide to 1-n-butyl-1-methylpyrrolidine bis(trifluoromethylsulfonyl)imide, and stir at room temperature for 3 h. After stirring evenly, a mixed solution A with a concentration of 3 mol / L is obtained.
[0053] S2. Add ethoxylated trimethylolpropane triacrylate and 2-hydroxy-2-methyl-1-phenylacetone into the mixed solution A in S1 at a mass ratio of 100:1, and stir evenly at room temperature to obtain a mixed solution B.
[0054] The amount of ethoxylated trimethylolpropane triacrylate used is 40 wt % of the mixed solution A.
[0055] S3, adding lanthanum lithium titanate ceramic nanoparticles into the mixed solution B in S2 three times, stirring at room temperature, and mixing evenly to obtain a printing slurry.
[0056] The amount of lanthanum lithium titanate ceramic nanoparticles used is 40wt% of the mixed solution B.
[0057] S4: Place the printing paste in S3 into the printing tank, and use a UV laser power of 3000mW / cm 2 The model is built according to the needs and light-curing 3D printing is performed layer by layer. After printing, the porous composite solid electrolyte is removed and the uncured printing slurry on the surface is cleaned. After cleaning, a composite solid electrolyte with a symmetrical porous structure is obtained.
[0058] Comparative Example 1
[0059] S1. Add lithium bis(trifluoromethanesulfonyl)imide to 1-n-butyl-1-methylpyrrolidine bis(trifluoromethylsulfonyl)imide, and stir at room temperature for 3 h. After stirring evenly, a mixed solution A with a concentration of 3 mol / L is obtained.
[0060] S2. Add ethoxylated trimethylolpropane triacrylate and 2-hydroxy-2-methyl-1-phenylacetone into the mixed solution A in S1 at a mass ratio of 100:1, and stir evenly at room temperature to obtain a mixed solution B.
[0061] The amount of ethoxylated trimethylolpropane triacrylate used is 40 wt % of the mixed solution A.
[0062] S3, adding lanthanum lithium titanate ceramic nanoparticles into the mixed solution B in S2 three times, stirring at room temperature, and mixing evenly to obtain a printing slurry.
[0063] The amount of lanthanum lithium titanate ceramic nanoparticles used is 40wt% of the mixed solution B.
[0064] S4: Place the printing paste in S3 into the printing tank, and use a UV laser power of 3000mW / cm 2 Under the condition of modeling according to the needs and performing light-curing 3D printing layer by layer, after printing, the non-porous composite solid electrolyte is removed and the uncured printing slurry on the surface is cleaned, and a non-porous composite solid electrolyte is obtained after cleaning, such as Figure 3 shown.
[0065] a. Verification method for composite solid electrolyte performance
[0066] Lithium iron phosphate (LiFePO4) positive electrode slurry was poured onto one side of the porous composite solid electrolyte printed in Example 4, and metallic lithium was filled into the other side of the porous composite solid electrolyte by melt lithium filling technology to assemble a CR2025 battery.
[0067] Lithium iron phosphate (LiFePO4) positive electrode slurry was poured onto one side of the non-porous composite solid electrolyte printed in Comparative Example 1, and metallic lithium was filled into the other side of the non-porous composite solid electrolyte by melt-filling lithium technology to assemble into CR2025 battery 2.
[0068] Use CT-4000 Xinwei battery tester to perform constant current charge and discharge test on CR2025 battery 1 and CR2025 battery 2 in the voltage range of 2.5-3.8V. The constant current charge and discharge test results are as follows: Figure 4 As shown, it can be seen that the printed porous composite solid electrolyte has good cycle stability and coulombic efficiency relative to the non-porous composite solid electrolyte.
[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a 3D printed composite solid electrolyte, Features: The method comprises the following steps: S1, adding lithium bis(trifluoromethanesulfonyl imide) into an ionic liquid, and stirring evenly to obtain a mixed solution A with a concentration of 0.5 to 3 mol / L; S2, adding the photosensitive resin and the initiator into the mixed solution A in S1 at a mass ratio of 100:1, and stirring to obtain a mixed solution B; S3, adding inorganic oxide ceramic nanoparticles into the mixed solution B in S2 three times, and mixing them evenly to obtain a printing slurry; S4, placing the printing slurry in S3 into a printing tank, performing photocuring 3D printing layer by layer at a UV laser power of 500-3000 mW / cm2, and obtaining a composite solid electrolyte with a symmetrical porous structure after cleaning; The structure of the composite solid electrolyte printed by photocuring 3D printing is that the middle layer is a solid structure, and the upper and lower layers are symmetrical porous structures; The ionic liquid is one or more of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium bis(fluoromethanesulfonyl)imide, 1-methyl-1-propylpyrrolidine bis(trifluoromethanesulfonyl)imide, 1-n-butyl-1-methylpyrrolidine bis(trifluoromethanesulfonyl)imide and 1-butyl-1-methylpyrrolidine bis(trifluoromethanesulfonyl)imide; The photosensitive resin is at least one of ethoxylated trimethylolpropane triacrylate, 1,6-hexanediol diacrylate and polyethylene glycol diacrylate; The initiator is one or more of 2-hydroxy-2-methyl-1-phenylacetone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide; The amount of photosensitive resin used is 5-40wt% of the mixed solution A; The inorganic oxide ceramic nanoparticles are one or more of lithium lanthanum zirconium oxide ceramic nanoparticles, tantalum-doped lithium lanthanum zirconium oxide ceramic nanoparticles, aluminum-doped lithium lanthanum zirconium oxide ceramic nanoparticles, niobium-doped lithium lanthanum zirconium oxide ceramic nanoparticles, lithium aluminum titanium phosphate ceramic nanoparticles and lanthanum lithium titanate ceramic nanoparticles; The amount of the inorganic oxide ceramic nanoparticles used is 5-40wt% of the mixed solution B.
2. The composite solid electrolyte prepared by the method for preparing a 3D printed composite solid electrolyte according to claim 1, Features: The structure of the composite solid electrolyte printed by photocuring 3D printing is that the middle layer is a solid structure, and the upper and lower layers are symmetrical porous structures.
3. Application of the composite solid electrolyte according to claim 2, Features: The composite solid electrolyte is used in the preparation of batteries.
Citation Information
Patent Citations
Electrode for solid-state batteries and preparation method thereof and solid-state battery
CN110224107A
Composite solid electrolyte having three-dimensional through structure and all-solid-state lithium ion battery
CN111326786A
Ordered porous solid electrolyte structures, electrochemical device with same, and methods of making sam
CN111886090A
Solid polymer electrolyte as well as preparation method and application thereof
CN114069035A
Method for preparing solid-state lithium ion battery by utilizing 3D printing and obtained lithium ion battery
CN114865096A