Interface transition layer of metal lithium negative electrode and solid electrolyte and preparation method of interface transition layer

By using a liquid alloy transition layer between the metal lithium negative electrode and the solid electrolyte, the problem of poor interface contact is solved, the interface impedance is reduced, the lithium ion transmission efficiency and interface stability are improved, and the battery charging and discharging process is adapted to the battery and the solid state is significantly improved Battery performance.

CN119009188APending Publication Date: 2024-11-22HEFEI INSTITUTE OF PHYSICAL SCIENCE CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411235217.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

There is a large wetting angle between the interface between the metal lithium negative electrode and the solid electrolyte, resulting in poor interface contact and a high-impedance interface, which affects the rate performance and cycle stability of the battery, and the stability and electrochemistry of the transition layer in the prior art. Inadequate compatibility affects lithium ion transmission efficiency.

Method used

The liquid alloy formed by mixing metal element elements such as lithium, gallium, tin, indium, aluminum, zinc and other metal oxides as the interface transition layer. The alloy suspension is prepared by melting and ultrasonic dispersion method, and the method is applied to the dropwise addition or coating method. The solid electrolyte surface forms an interface transition layer to achieve a close fit between the metal lithium negative electrode and the solid electrolyte.

Benefits of technology

Reduces interface impedance, improves lithium ion transmission efficiency and interface stability, enhances the wetting and self-repairing ability of the interface, adapts to changes in electrode volume during battery charging and discharging, maintains continuous interface contact, and significantly improves the solid-state battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009188A_ABST
    Figure CN119009188A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to an interface transition layer of a metal lithium negative electrode and a solid electrolyte and a preparation method of the interface transition layer. The interface transition layer is a liquid alloy formed by mixing at least two of metal simple substances of lithium, gallium, tin, indium, aluminum and zinc and oxides thereof, and the preparation method of the interface transition layer comprises the following steps: S1, weighing raw materials of the interface transition layer according to a mass ratio, and preparing an alloy suspension through a melting method and ultrasonic dispersion; and S2, the alloy suspension liquid is solidified and attached to the solid electrolyte and the lithium negative electrode, so that an interface transition layer is formed between the solid electrolyte and the lithium negative electrode. According to the invention, a plurality of metal elementary substances and oxides thereof are mixed to form the liquid alloy as the interface transition layer, the alloy suspension is prepared by combining a melting method and an ultrasonic dispersion method, and interface fitting is realized by adopting methods such as dropwise adding and coating, so that the interface contact between the metal lithium negative electrode and the solid electrolyte is effectively improved, and the interface impedance is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an interface transition layer between a metal lithium negative electrode and a solid electrolyte and a preparation method thereof. Background Art

[0002] All-solid-state batteries based on metal lithium anodes are the forefront of the current development of lithium-ion battery technology. They have advantages such as high energy density and high safety, and are expected to become the mainstream technology for the next generation of power batteries. However, the interface problem between the metal lithium anode and the solid electrolyte has always been one of the key bottlenecks restricting the commercial application of all-solid-state batteries. However, there is a large wetting angle between metal lithium and most solid electrolyte materials, resulting in poor interface contact and the formation of a high-impedance interface. This high-impedance interface will not only reduce the rate performance and cycle stability of the battery, but also cause safety hazards.

[0003] In order to solve this problem, researchers proposed to construct a third phase transition layer between the interface of metallic lithium and the solid electrolyte to achieve the purpose of improving the interface bonding effect and reducing the contact resistance. Chinese patent CN201910711413.3 discloses a transition layer design method between an inorganic solid electrolyte and a positive electrode, which includes: firstly, the positive electrode active material and the inorganic electrolyte material are ball-milled and mixed according to a set ratio, and configured into transition layer slurries of different proportions; then, these transition layer slurries of different proportions are applied to the positive electrode surface in a gradient order; finally, the positive electrode sheet coated with the gradient transition layer is tightly attached to the inorganic solid electrolyte sheet, and the gradient transition layer is between the positive electrode sheet and the inorganic solid electrolyte. The above scheme introduces a gradient transition layer between the positive electrode and the inorganic electrolyte to provide an effective path for the transmission of lithium ions, thereby reducing the interface transmission resistance of ions and improving the cycle stability of the all-solid-state battery. However, in the above technical solution, the slurry formed by the positive electrode material and the electrolyte material is used as the transition layer. The contact between the particles in the slurry transition layer may form a complex ion conduction path, increasing the conduction resistance; during the battery charging and discharging process, problems such as stratification and shedding may occur, making it difficult to maintain long-term interface stability; at the same time, there may also be electrochemical compatibility problems with the metallic lithium negative electrode, thereby affecting the interfacial lithium ion transmission efficiency. Summary of the invention

[0004] In view of this, the present invention proposes an interface transition layer between a metal lithium negative electrode and a solid electrolyte and a preparation method thereof to solve the problem of uneven interface contact in the prior art, thereby affecting the interface lithium ion transmission efficiency and interface resistance.

[0005] The technical solution of the present invention is achieved in this way: In a first aspect, the present invention provides an interface transition layer between a metallic lithium negative electrode and a solid electrolyte, wherein the interface transition layer is a liquid alloy formed by mixing at least two substances selected from metallic single substances of lithium, gallium, tin, indium, aluminum, zinc and their oxides.

[0006] On the basis of the above technical solution, preferably, in the liquid alloy, the gallium content is 30-80 wt.%, the indium and tin contents are both 0-30 wt.%, the lithium, aluminum and zinc contents are both 0-20 wt.%, and the oxide content of the metal element is 0-10wt.%.

[0007] Further preferably, the interface transition layer is composed of gallium, indium and tin, or of lithium, gallium and indium, or of lithium, gallium and tin. The melting point of gallium is close to room temperature, and the combination of gallium with any of indium, tin or lithium can reduce the melting point of the mixed metal.

[0008] Specifically, in the present invention, by combining metal elements and their oxides, a low-temperature liquid alloy transition layer having both ionic and electronic conductivity is formed, thereby improving the interface contact effect between the metal lithium negative electrode and the solid electrolyte and reducing the interface impedance. Specifically, lithium, gallium, tin, indium, aluminum, and zinc are all metal elements with excellent electronic conductivity, and their free electrons can move freely in the liquid alloy, providing a good electronic conduction channel; at least two substances in the metal elements of lithium, gallium, tin, indium, aluminum, and zinc and their oxides are mixed to form an alloy, and the metal elements can work synergistically to enhance the transmission capacity of lithium ions. In addition, in the present invention, by forming a liquid alloy, in the liquid state, the arrangement of each metal atom is looser, and the movement of electrons between atoms is easier, further improving the mobility and conductivity of electrons; when the liquid metal alloy is attached to the lithium negative electrode, it can dissolve a certain amount of lithium, and when lithium dissolves from the negative electrode into the liquid alloy, a lithium ion transmission channel is formed; the liquid characteristics also bring excellent interface wettability, dynamic balance ability and self-repairing ability, further enhancing the conductive performance.

[0009] In a second aspect, the present invention provides a method for preparing an interface transition layer between a metal lithium negative electrode and a solid electrolyte, comprising the following steps: S1. Weigh the raw materials of the interface transition layer according to the mass ratio, prepare a uniform alloy by a melting method, and prepare an alloy suspension by ultrasonic dispersion in a volatile solvent with a temperature exceeding the melting point; S2. Add the alloy suspension dropwise onto the surface of the solid electrolyte and dry it, and then solidify and bond it to the lithium negative electrode to form an interface transition layer between the solid electrolyte and the lithium negative electrode.

[0010] On the basis of the above technical solution, preferably, step S1 specifically includes: heating and melting the raw materials of the interface transition layer to obtain a uniform alloy, and then placing the alloy in a solvent for ultrasonic dispersion to obtain an alloy suspension.

[0011] On the basis of the above technical solution, preferably, in step S1, the melting temperature is 25-250° C., the melting time is 0.1-2 h; the frequency of ultrasonic dispersion is 20-40 kHz, and the time is 5-60 min.

[0012] On the basis of the above technical scheme, preferably, the solvent is one or a mixed liquid of ethanol, dimethyl carbonate, N-methylpyrrolidone, diethylene glycol, acetamide, ethylene glycol, N,N-dimethylformamide, octane, isopropanol, and hexane.

[0013] On the basis of the above technical solution, preferably, in step S2, the prepared alloy suspension is dripped and coated on the surface of the solid electrolyte to achieve the bonding of the interface transition layer and the solid electrolyte.

[0014] Specifically, in step S1, the melting method uses temperature to melt and mix the components to form a uniform liquid alloy. The selection of temperature and time ensures sufficient melting and mixing while avoiding excessive oxidation or volatilization of the components. The cavitation effect of ultrasound is used to disperse the molten alloy into nano-scale particles. The high-frequency vibration generated by ultrasound in the liquid causes the formation, growth and rupture of tiny bubbles, which can break the alloy into extremely small particles.

[0015] In step S2, the dripping or coating method utilizes the liquid properties and good fluidity of the alloy suspension to enable it to be evenly spread on the surface of the solid electrolyte; at the same time, the surface tension of the liquid alloy helps to form a continuous film, and the self-leveling ability can fill the tiny surface bumps and increase the contact area. This method is simple to operate and easy to control, suitable for laboratories and small-scale production, and the thickness of the interface transition layer can be adjusted by controlling the dripping amount or the number of coatings.

[0016] On the basis of the above technical solution, preferably, the material of the solid electrolyte is NASICON type LiTi2(PO3)3 based electrolyte, LiGe2(PO3)3 based electrolyte and Garnet type Li7La3Zr2O 12 One of the base electrolytes.

[0017] On the basis of the above technical solution, preferably, the thickness of the interface transition layer is 10 nm-5 μm.

[0018] In a third aspect, the present invention provides a solid-state battery, comprising an interface transition layer between a metal lithium negative electrode and a solid electrolyte as described above.

[0019] The interface transition layer between a metal lithium negative electrode and a solid electrolyte and the preparation method thereof of the present invention have the following beneficial effects compared with the prior art: (1) The interface transition layer between the metal lithium negative electrode and the solid electrolyte and the preparation method thereof provided by the present invention, by using a plurality of metal elements and their oxides to form a liquid alloy as the interface transition layer, combining the melting method and the ultrasonic dispersion method to prepare the alloy suspension, and using the dripping, coating and other methods to achieve interface bonding, effectively improves the interface contact between the metal lithium negative electrode and the solid electrolyte, reduces the interface impedance, improves the lithium ion transmission efficiency, and enhances the stability and safety of the interface; (2) The liquid alloy interface transition layer used in the present invention, especially the gallium content is 30-80wt.%, the indium and tin content is 0-30wt.%, and the lithium, aluminum, and zinc content is 0-20wt.%, so that the interface transition layer remains in a liquid or semi-liquid state at room temperature, has good fluidity and self-repairing ability, can adapt to the volume change of the electrode during the battery charging and discharging process, and maintain continuous interface contact. At the same time, this component also has excellent ionic conductivity and electronic conductivity, which greatly reduces the interface impedance. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 is a flow chart for preparing the interface transition layer in Example 1 of the present invention; Figure 2 This is a SEM image of the lithium metal / transition layer / solid electrolyte three-layer structure prepared in Example 1 of the present invention; Figure 3 This is a picture of the metallic lithium prepared in Comparative Example 1 melted on the surface of the solid electrolyte. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0023] This embodiment provides an interface transition layer between a metal lithium negative electrode and a solid electrolyte and a preparation method thereof, comprising the following steps: S1. 6.8 g of metal gallium, 2.2 g of indium and 1.0 g of tin were weighed and mixed. Under the protection of an argon inert atmosphere, the mixture was heated and stirred at 100 °C for 1 h to achieve uniform mixing of the three. The alloy was then placed in ethanol and ultrasonically dispersed at a frequency of 30 kHz for 40 min to obtain an alloy suspension. S2, add the alloy suspension dropwise to the Ca / Ta co-doped garnet-type Li 6.55 (La 2.95 Ca 0.05 )(Zr 1.5 Ta)O 12 After the surface of the (LLZTO) solid electrolyte block is dried, the interface transition layer and the solid electrolyte are closely fitted; then, under heating conditions at 180°C, the metal lithium sheet is melted on the surface of the interface transition layer to achieve close fitting between the lithium negative electrode, the interface transition layer and the solid electrolyte. Example 2

[0024] This embodiment provides an interface transition layer between a metal lithium negative electrode and a solid electrolyte and a preparation method thereof, comprising the following steps: S1. 1.0 g of metallic lithium, 7.0 g of gallium and 2.0 g of tin were weighed and mixed. Under the protection of an argon inert atmosphere, the mixture was heated and stirred at 150° C. for 1 h to achieve uniform mixing of the three. The alloy was then placed in a dimethyl carbonate solvent and ultrasonically dispersed at a frequency of 30 kHz for 40 min to obtain an alloy suspension. S2, add the alloy suspension dropwise to the Ta-doped garnet-type Li 6.5 Ln3Z 1.5 Ta 0.5 O 12 After the surface of the solid electrolyte block is dried, close contact between the liquid alloy transition layer and the solid electrolyte can be achieved; then, under heating conditions at 180°C, the metal lithium sheet is melted on the surface of the interface transition layer to achieve close fitting between the lithium negative electrode, the interface transition layer and the solid electrolyte. Example 3

[0025] This embodiment provides an interface transition layer between a metal lithium negative electrode and a solid electrolyte and a preparation method thereof, comprising the following steps: S1. 1.0 g of metallic lithium, 8.0 g of gallium and 1.0 g of indium were weighed and mixed. Under the protection of an argon inert atmosphere, the mixture was heated and stirred at 150 °C for 1 h to achieve uniform mixing of the three. The alloy was placed in an N-methylpyrrolidone (NMP) solvent and ultrasonically dispersed at a frequency of 30 kHz for 40 min to obtain an alloy suspension. S2, add the alloy suspension dropwise to the Nb-doped garnet-type Li 6.5 Ln3Z 1.5 Nb 0.5 O 12 After the surface of the solid electrolyte block is dried, close contact between the liquid alloy transition layer and the solid electrolyte can be achieved; then, under heating conditions at 180°C, the metal lithium sheet is melted on the surface of the interface transition layer to achieve close fitting between the lithium negative electrode, the interface transition layer and the solid electrolyte. Example 4

[0026] This embodiment provides an interface transition layer between a metal lithium negative electrode and a solid electrolyte and a preparation method thereof, comprising the following steps: S1. 8.0 g of metal gallium, 1.0 g of indium and 1.0 g of aluminum were weighed and mixed. Under the protection of an argon inert atmosphere, the mixture was heated and stirred at 50° C. for 2 h to achieve uniform mixing of the three. The alloy was then placed in diethylene glycol and ultrasonically dispersed at a frequency of 20 kHz for 60 min to obtain an alloy suspension. S2, add the alloy suspension dropwise to the Al-doped NASICON type Li 1.3 Al 0.3 Ti 1.7 After the (PO4)3 solid electrolyte block is dried, the interface transition layer and the solid electrolyte are tightly fitted together. Then, the metal lithium sheet is melted on the surface of the interface transition layer under heating conditions at 160°C to achieve a tight fit between the lithium negative electrode, the interface transition layer and the solid electrolyte. Example 5

[0027] This embodiment provides an interface transition layer between a metal lithium negative electrode and a solid electrolyte and a preparation method thereof, comprising the following steps: S1. 3.0 g of metal gallium, 3.0 g of indium, 2.0 g of zinc and 2.0 g of lithium were weighed and mixed. Under the protection of an argon inert atmosphere, the mixture was heated and stirred at 250° C. for 0.1 h to achieve uniform mixing of the three. The alloy was then placed in acetamide and ultrasonically dispersed at a frequency of 40 kHz for 5 min to obtain an alloy suspension. S2, add the alloy suspension dropwise to the Ca / Ta co-doped garnet-type Li 6.55 (La 2.95 Ca 0.05)(Zr 1.5 Ta 0.5 ) 12 After the surface of the (LLZTO) solid electrolyte block is dried, the interface transition layer and the solid electrolyte are closely fitted; then, under heating conditions of 200°C, the metal lithium sheet is melted on the surface of the interface transition layer to achieve close fitting between the lithium negative electrode, the interface transition layer and the solid electrolyte.

[0028] Comparative Example 1 The metallic lithium was heated and melted in the Ca / Ta co-doped garnet-type Li 6.55 (La 2.95 Ca 0.05 )(Zr 1.5 Ta 0.5 ) 12 (LLZTO) solid electrolyte block surface and cooling.

[0029] Comparative Example 2 S1. 10 g of metal gallium was placed in ethanol and ultrasonically dispersed at a frequency of 30 kHz for 40 min to obtain an alloy suspension. S2, drop the suspension onto the Ca / Ta co-doped garnet-type Li 6.55 (La 2.95 Ca 0.05 )(Zr 1.5 Ta 0.5 ) 12 After the surface of the (LLZTO) solid electrolyte block is dried, the metal lithium sheet is melted on the surface of the interface transition layer under heating conditions at 180°C to achieve a close fit between the lithium negative electrode, the interface transition layer and the solid electrolyte.

[0030] Performance Testing The interface transition layer prepared in the embodiment and the comparative example was assembled into a pole core in the order of lithium negative electrode, interface transition layer, solid electrolyte, and positive electrode sheet, and then aluminum-plastic film encapsulation-liquid injection-chemical composition was made into a solid-state lithium battery. The above solid-state lithium battery was tested for impedance performance, and the test results are shown in Table 1.

[0031] Table 1 Performance test It can be seen from Table 1 that the interface transition layer prepared by the present invention is applied to solid-state batteries to reduce interface resistance.

[0032] Figure 1 The preparation flow chart of the interface transition layer in Example 1 of the present invention is shown, wherein: Figure 1 (a) is an LLZTO-type solid electrolyte without coating layer. Figure 1(b) is a LLZTO-type solid electrolyte coated with a gallium-indium-tin alloy. Figure 1 (c) shows the metal lithium layer melt-coated on the gallium-indium-tin coating layer. As can be seen from the figure, the liquid alloy transition layer can be evenly distributed on the surface of the solid electrolyte and is tightly bonded. The metal lithium sheet is melted on the surface of the transition layer to achieve a tight bond between the three.

[0033] Figure 2 This is an SEM image of the lithium metal / transition layer / solid electrolyte three-layer structure prepared in Example 1 of the present invention. It can be seen from the figure that from top to bottom are the lithium metal layer, the transition layer and the LLZTO electrolyte layer, and the interface transition layer is tightly attached to the lithium metal layer and the LLZTO electrolyte layer.

[0034] Figure 3 This is a diagram of the metal lithium prepared in Comparative Example 1 of the present invention melted on the surface of the solid electrolyte. As can be seen from the figure, due to the large wetting angle between the metal lithium and the LLZTO type solid electrolyte, the melted metal lithium spontaneously shrinks into a sphere, and separates from the solid electrolyte after cooling, and close contact between the two cannot be achieved.

[0035] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An interface transition layer between a metallic lithium negative electrode and a solid electrolyte, characterized in that: The interface transition layer is a liquid alloy formed by mixing at least two substances selected from metal elements of lithium, gallium, tin, indium, aluminum, zinc and their oxides.

2. The interface transition layer between a metal lithium negative electrode and a solid electrolyte according to claim 1, characterized in that: In the liquid alloy, the gallium content is 30-80 wt.%, the indium and tin contents are both 0-30 wt.%, the lithium, aluminum and zinc contents are both 0-20 wt.%, and the oxide content of the metal element is 0-10 wt.%.

3. A method for preparing an interface transition layer between a metal lithium negative electrode and a solid electrolyte according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1. Weigh the raw materials of the interface transition layer according to the mass ratio, prepare a uniform alloy by a melting method, and prepare an alloy suspension by ultrasonic dispersion in a volatile solvent with a temperature exceeding the melting point; S2. Add the alloy suspension dropwise onto the surface of the solid electrolyte and dry it, and then solidify and bond it to the lithium negative electrode to form an interface transition layer between the solid electrolyte and the lithium negative electrode.

4. The method for preparing an interface transition layer between a metal lithium negative electrode and a solid electrolyte according to claim 3, characterized in that: Step S1 specifically includes: heating and melting the raw materials of the interface transition layer to obtain a uniform alloy, and then placing the alloy in a solvent for ultrasonic dispersion to obtain an alloy suspension.

5. The method for preparing an interface transition layer between a metal lithium negative electrode and a solid electrolyte according to claim 4, characterized in that: In step S1, the melting temperature is 25-250° C., the melting time is 0.1-2 h; the ultrasonic dispersion frequency is 20-40 kHz, and the time is 5-60 min.

6. The method for preparing an interface transition layer between a metal lithium negative electrode and a solid electrolyte according to claim 4, characterized in that: The solvent is one or a mixed liquid of ethanol, dimethyl carbonate, N-methylpyrrolidone, diethylene glycol, acetamide, ethylene glycol, N,N-dimethylformamide, octane, isopropanol and hexane.

7. The method for preparing an interface transition layer between a metal lithium negative electrode and a solid electrolyte according to claim 3, characterized in that: In step S2, the prepared alloy suspension is dripped and coated on the surface of the solid electrolyte to achieve bonding between the interface transition layer and the solid electrolyte.

8. The method for preparing an interface transition layer between a metal lithium negative electrode and a solid electrolyte according to claim 3, characterized in that: The solid electrolyte material is NASICON type LiTi2(PO3)3 based electrolyte, LiGe2(PO3)3 based electrolyte and Garnet type Li7La3Zr2O 12 One of the base electrolytes.

9. The method for preparing an interface transition layer between a metal lithium negative electrode and a solid electrolyte according to claim 3, characterized in that: The thickness of the interface transition layer is 10 nm-5 μm.

10. A solid-state battery, characterized in that: The solid-state battery comprises an interface transition layer between a metal lithium negative electrode and a solid electrolyte as described in any one of claims 1 to 2.

Citation Information

Cited By

  • Combination method for enhancing solid-state battery electrolyte and electrode interface

    CN122291707A

  • Composite structure of negative electrode and solid-state electrolyte for battery, and preparation method therefor and use thereof

    WO2026208195A1