A blowing method for a Consteel electric arc furnace

By employing an asymmetrical distribution of six oxygen lances and flow rate regulation in the Consteel electric arc furnace, the problem of slow scrap melting speed was solved, achieving rapid melting and efficient smelting, while reducing power consumption and smelting cycle.

CN117385125BActive Publication Date: 2026-11-10HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311193799.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-15
Publication Date
2026-11-10
Estimated Expiration
2043-09-15

AI Technical Summary

Technical Problem

The Consteel electric arc furnace has a low preheating temperature for scrap steel, which leads to the accumulation of scrap steel in the connecting trolley, resulting in a slow melting speed, increased difficulty in smelting operations and power consumption, and a longer smelting cycle.

Method used

The system employs six oxygen lances asymmetrically distributed and angled downwards, with the oxygen lance flow rate adjusted at different stages. Combined with carbon powder injection, it achieves rapid melting of scrap steel and creation of foamy slag.

Benefits of technology

By using a rationally distributed oxygen lance system and flow regulation, scrap steel can be melted quickly, shortening the smelting cycle, reducing power consumption, and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117385125B_ABST
    Figure CN117385125B_ABST
Patent Text Reader

Abstract

This invention discloses an oxygen lance distribution configuration and blowing method for a Consteel electric arc furnace. The furnace is equipped with six oxygen lances: Lance 1 and Lance 2 asymmetrically positioned on both sides of the connecting trolley; Lance 3 and Lance 4 asymmetrically positioned on both sides of the furnace door; and Lance 5 and Lance 6 asymmetrically positioned on both sides of the eccentric furnace bottom taphole. The angles between Lance 1 and Lance 2 and the centerline of the connecting trolley are 20–40° and 40–60°, respectively; the angles between Lance 3 and Lance 4 and the centerline of the furnace door are 20–40° and 40–60°, respectively; and the angles between Lance 5 and Lance 6 and the centerline of the eccentric furnace bottom taphole are 20–40° and 40–60°, respectively. This invention allows oxygen to be delivered to different locations within the furnace, resulting in a more rational oxygen distribution. This enables rapid melting of scrap steel, rapid foam slag formation, and rapid heating of molten steel, thereby improving production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electric arc furnace metallurgical technology, and in particular to a oxygen lance distribution configuration and blowing method for a Consteel electric arc furnace. Background Technology

[0002] Currently, over 95% of global electric arc furnace steel production is produced using electric arc furnaces, and short-process steelmaking, with electric arc furnace steelmaking at its core, has become one of the most important processes in the entire steel production process.

[0003] Consteel electric arc furnaces are widely used due to their advantages such as smooth production operation, low grid impact, and reliable and controllable feeding. However, because of their low scrap preheating temperature and large amount of scrap added to the connecting trolley, scrap tends to accumulate at the connection between the connecting trolley and the furnace body, resulting in slow melting speed, increased difficulty in smelting operation, increased power consumption in steelmaking, and longer smelting cycle. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide an oxygen lance distribution configuration for a Consteel electric arc furnace that can rapidly melt scrap steel; the present invention also provides a blowing method for a Consteel electric arc furnace that can rapidly melt scrap steel.

[0005] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: the electric arc furnace is equipped with six oxygen lances, namely, oxygen lances No. 1 and No. 2 asymmetrically arranged on both sides of the connecting trolley, oxygen lances No. 3 and No. 4 asymmetrically arranged on both sides of the furnace door, and oxygen lances No. 5 and No. 6 asymmetrically arranged on both sides of the eccentric furnace bottom taphole; the angles between oxygen lances No. 1 and No. 2 and the center line of the connecting trolley are 20-40° and 40-60° respectively, the angles between oxygen lances No. 3 and No. 4 and the center line of the furnace door are 20-40° and 40-60° respectively, and the angles between oxygen lances No. 5 and No. 6 and the center line of the eccentric furnace bottom taphole are 20-40° and 40-60° respectively.

[0006] Furthermore, all six oxygen lances are positioned at an angle downwards, with an angle of 30 to 45 degrees to the horizontal.

[0007] Furthermore, the horizontal distance between the No. 1, No. 3, and No. 5 oxygen lances extending into the furnace is 70-100cm, and the horizontal distance between the No. 2, No. 4, and No. 6 oxygen lances extending into the furnace is 40-70cm.

[0008] Furthermore, the oxygen lances No. 1, No. 4, No. 3, No. 5, No. 6, and No. 2 are arranged in a counterclockwise direction.

[0009] The method of the present invention uses the above-described oxygen lance distribution and comprises the following steps: 1) After tapping steel from the eccentric bottom of the electric arc furnace, the steel retention ratio is ≥50%. After the electric arc furnace returns to the horizontal position, the electrodes are energized for heating, and scrap steel is added. At the same time, the oxygen lance is started for oxygen blowing and the carbon lance is started for carbon powder injection. The flow rates of the first and second oxygen lances are both 2500-3000 Nm³. 3 / h, the flow rate of the remaining oxygen lances is 500-1000 Nm³ / h. 3 / h; 2) Add lime and lightly calcined dolomite during the time periods when the scrap steel content in the furnace reaches 0-30%, 30-50%, and 50-80%, respectively. After the scrap steel content in the furnace exceeds 50%, adjust the flow rates of oxygen lances No. 3, No. 4, No. 5, and No. 6 to 1000-1500 Nm³. 3 / h; After the amount of scrap steel added into the furnace exceeds 80%, the flow rates of oxygen lances No. 3, No. 4, No. 5, and No. 6 should be adjusted to 1500-2000 Nm³. 3 / h; 3) After all the scrap steel has been added to the furnace, adjust the flow rates of oxygen lances No. 1 and No. 2 to 1500–2000 Nm³. 3 / h; After all the scrap steel is added, the temperature is measured and a steel sample is taken 4 minutes later. If the [C] content in the steel sample is high, the oxygen lance flow rate is adjusted to 2000-3000 Nm. 3 If the [C] content in the steel sample is low, add carbon powder and adjust the oxygen lance flow rate to 500–1500 Nm / h. 3 / h; When the temperature and composition meet the requirements, prepare to tap the steel.

[0010] Furthermore, in steps 1) and 2), the amount of carbon powder added is 60-120 kg / min, the total amount of lime added is 20-30 kg / t, and the total amount of lightly calcined dolomite added is 15-25 kg / t.

[0011] The beneficial effects of adopting the above technical solution are as follows: the present invention uses six oxygen lances to supply oxygen in a coordinated manner and adopts an asymmetrical distribution, which can deliver oxygen to different positions in the furnace, making the oxygen distribution in the furnace more reasonable. This enables rapid melting of scrap steel, rapid foam slag formation, and rapid heating of molten steel, thereby improving production efficiency.

[0012] The method of this invention utilizes a high oxygen flow rate in the oxygen lances on both sides of the connecting trolley before all scrap steel is added, achieving rapid melting of the scrap steel. The oxygen flow rates of the oxygen lances on both sides of the furnace door and the tapping port are adjusted according to the heating and melting of the scrap steel, facilitating heating, melting, and rapid foaming slag formation. By coordinating the oxygen supply from six oxygen lances and adjusting the oxygen flow rates at different stages of scrap steel addition, rapid melting of scrap steel, rapid foaming slag formation, and rapid heating of molten steel are achieved. The rapid heating during the smelting process can quickly and effectively meet the tapping requirements, avoiding the problem of slow melting speed due to scrap steel accumulation near the connecting trolley caused by a large amount of scrap steel added to the Consteel electric arc furnace. This is beneficial for electric arc furnace smelting and operation, reduces smelting power consumption, shortens the smelting cycle, reduces the average smelting cycle per furnace by 3-5 minutes, and greatly improves production efficiency and economic benefits. Attached Figure Description

[0013] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.

[0014] Figure 1 This is a top view schematic diagram of the oxygen lance distribution configuration described in this invention; Figure 2 This is a cross-sectional schematic diagram of the Consteel electric arc furnace described in this invention.

[0015] In the diagram: 1. Electrode; 2. Furnace door; 3. Eccentric furnace bottom taphole; 4. Connecting trolley; 5. Oxygen lance No. 1; 6. Oxygen lance No. 2; 7. Oxygen lance No. 3; 8. Oxygen lance No. 4; 9. Oxygen lance No. 6; 10. Feeding device; 11. Carbon lance; 12. Molten steel; 13. Slag; 14. Detailed Implementation

[0016] Figure 1 , Figure 2 As shown, the Consteel electric arc furnace is equipped with electrodes 1 for heating, a feeding device 11 on one side of the furnace top for adding slag-forming auxiliary materials, a furnace door 2 on the furnace side for slag discharge, an eccentric furnace bottom taphole 3 on one side of the furnace bottom for tapping steel, and a connecting trolley 4 in the middle of the furnace body for continuously adding scrap steel. It also has oxygen lances and carbon lances 12 that pass through the furnace body and extend into the furnace. During smelting, scrap steel is continuously added into the furnace body via the connecting trolley 4, slag-forming auxiliary materials are added via the furnace top feeding device 11, electrodes 1 are energized for heating, and oxygen lances and carbon lances 12 blow steel. The scrap steel and slag-forming auxiliary materials melt into molten steel 13 and slag 14 attached to the top of the molten steel. This Consteel electric arc furnace has a capacity of 150t and above.

[0017] Figure 1 , Figure 2As shown, the oxygen lances of this Consteel electric arc furnace are distributed as follows: the furnace is equipped with six oxygen lances, namely oxygen lance 5 (No. 1), oxygen lance 6 (No. 2), oxygen lance 7 (No. 3), oxygen lance 8 (No. 4), oxygen lance 9 (No. 5), and oxygen lance 10 (No. 6). Oxygen lance 5 and oxygen lance 6 are asymmetrically positioned on both sides of the connecting trolley 4, with the angle between oxygen lance 5 and the center line of the connecting trolley being α1 = 20–40°, and the angle between oxygen lance 6 and the center line of the connecting trolley being α2 = 40–60°. Oxygen lance 7 and oxygen lance 8 are asymmetrically positioned on both sides of the furnace door 2, with the angle between oxygen lance 7 and the center line of the furnace door being α1 = 20–40°, and the angle between oxygen lance 8 and the center line of the furnace door being α2 = 40–60°. Oxygen lances 9 (No. 5) and 10 (No. 6) are asymmetrically positioned on either side of the eccentric furnace bottom taphole 3. The angle between oxygen lance 9 and the center line of the eccentric furnace bottom taphole is α1 = 20–40°, and the angle between oxygen lance 10 and the center line of the eccentric furnace bottom taphole is α2 = 40–60°. All oxygen lances are connected to the electric arc furnace body at the same horizontal level, and oxygen lances 5 (No. 1), 8 (No. 4), 7 (No. 3), 9 (No. 5), 10 (No. 6), and 6 (No. 2) are arranged counterclockwise. All oxygen lances are angled downwards, with angles between them and the horizontal direction ranging from 30° to 45°. The horizontal insertion distance of oxygen lances 5 (No. 1), 7 (No. 3), and 9 (No. 5) into the furnace is 70–100 cm, while the horizontal insertion distance of oxygen lances 6 (No. 2), 8 (No. 4), and 10 (No. 6) into the furnace is 40–70 cm. These insertion distances are particularly suitable for the 150t Consteel electric arc furnace. The flow rate of each oxygen lance is individually controlled, with an adjustment range of 500–3000 Nm³ for each lance. 3 / h.

[0018] Figure 1 , Figure 2 As shown, the blowing method of this Consteel electric arc furnace adopts the following steps: (1) After the electric arc furnace adopts eccentric bottom tapping, the steel retention ratio is ≥50%. After the electric arc furnace returns to the horizontal position, the electrodes are energized for heating, and scrap steel is added. At the same time, the oxygen lance is started to blow oxygen and the carbon lance is started to inject carbon powder. The carbon powder injection rate is 60-120 kg / min. The flow rate of oxygen lance 5 and oxygen lance 6 located on both sides of the connecting trolley 4 is 2500-3000 Nm. 3 / h, to cut scrap steel; the flow rates of oxygen lances 7 and 8 located on both sides of furnace door 2, and oxygen lances 9 and 10 located on both sides of eccentric furnace bottom taphole 3, are all 500-1000 Nm³ / h. 3 / h, to agitate the molten steel to quickly create foamy slag and melt the scrap steel.

[0019] (2) Lime and lightly calcined dolomite are added during the time periods when the scrap steel content in the furnace reaches 0-30%, 30-50%, and 50-80%, respectively. The total amount of lime added is 20-30 kg / t, and the total amount of lightly calcined dolomite added is 15-25 kg / t. After the scrap steel content in the furnace exceeds 50%, the flow rates of oxygen lances 7 and 8 located on both sides of the furnace door 2, and oxygen lances 9 and 10 located on both sides of the eccentric furnace bottom taphole 3 are all adjusted to 1000-1500 Nm. 3 / h; After the amount of scrap steel added into the furnace exceeds 80%, the flow rates of oxygen lances No. 3 (7) and No. 4 (8) located on both sides of the furnace door 2, and oxygen lances No. 5 (9) and No. 6 (10) located on both sides of the eccentric furnace bottom taphole 3 are all adjusted to 1500-2000 Nm. 3 / h.

[0020] (3) After all the scrap steel is added, the flow rates of oxygen lance 5 and oxygen lance 6 located on both sides of the connecting trolley 4 are adjusted to 1500-2000 Nm. 3 The process involves heating and melting the scrap steel at a rate of / h, and agitating the molten pool to achieve rapid dephosphorization. After all the scrap steel has been added, the temperature is measured and a steel sample is taken 4 minutes or more later, ideally 4–8 minutes. Based on the target composition and the [P] content in the steel sample, it is determined whether to add lime; if the [P] content is high, lime is added. Similarly, based on the target composition and the [C] content in the steel sample, it is determined whether to add carbon powder; if the [C] content is high, the flow rate of all oxygen lances is adjusted to 2000–3000 Nm³. 3 / h, to rapidly decarburize and raise the temperature; if the [C] content is low, add carbon powder and adjust the flow rate of all oxygen lances to 500-1500 Nm. 3 / h, to heat up and stir the molten steel to homogenize the composition; when the temperature and composition meet the requirements, the electrodes are de-energized, the carbon lance is set to standby mode, and the oxygen lance is set to purging mode, ready for tapping.

[0021] (4) This method is applicable to a variety of steel types, including plain carbon steel, low carbon steel, and high carbon steel.

[0022] Example 1: The blowing method of this Consteel electric arc furnace is described in detail below.

[0023] A 150t Consteel electric arc furnace is used, with a total steel capacity of 230-250t, producing 45# round steel. 153.5t of steel is tapped from the eccentric bottom tap hole, leaving 53% of the steel. After the electric arc furnace returns to the horizontal position, the electrodes are energized for heating, and scrap steel is added. The carbon powder injection rate is 120kg / min, and the flow rates of oxygen lances 1 (5) and 2 (6) are both 2500Nm³. 3 / h, the flow rates of oxygen lances 7 (number 3), 8 (number 4), 9 (number 5), and 10 (number 6) are all 500 Nm³ / h. 3 / h; When 5t of scrap steel is added to the furnace, 1008kg of lime and 1001kg of lightly calcined dolomite are added; when 60t of scrap steel is added, 1015kg of lime and 994kg of lightly calcined dolomite are added; when 95t of scrap steel is added, 1504kg of lime and 543kg of lightly calcined dolomite are added; a total of 3527kg of lime is added, which is 23.3kg / ton of steel, and a total of 2538kg of lightly calcined dolomite is added, which is 16.8kg / ton of steel. When 85t of scrap steel is added to the furnace, the flow rates of oxygen lances 7 (No. 3), 8 (No. 4), 9 (No. 5), and 10 (No. 6) are all adjusted to 1000Nm. 3 / h; When 138t of scrap steel is added to the furnace, the flow rates of oxygen lances 7 (No. 3), 8 (No. 4), 9 (No. 5), and 10 (No. 6) are all adjusted to 1500 Nm. 3 / h; 165t of scrap steel was added. After the scrap steel addition was completed, the flow rates of oxygen lance 5 (No. 1) and oxygen lance 6 (No. 2) were both adjusted to 1500 Nm. 3 / h. After all the scrap steel was added, the temperature was measured and a steel sample was taken 6 minutes later. The carbon content was 0.103%, the phosphorus content was 0.0071%, and the temperature was 1606℃, which met the requirements for tapping. The electrodes were de-energized, the carbon lance was set to standby mode, and the oxygen lance was set to purging mode. 151.3t of steel was tapped, the steel retention ratio was 52.1%, and the smelting cycle was 47 minutes.

[0024] Example 2: The blowing method of this Consteel electric arc furnace is described in detail below.

[0025] A 150t Consteel electric arc furnace is used, with a total steel capacity of 230-250t, producing 40Cr steel. 150.6t of steel is tapped from the eccentric bottom tap hole, leaving a 55.9% steel residue. After the electric arc furnace returns to the horizontal position, the electrodes are energized for heating, and scrap steel is added. The carbon powder injection rate is 80kg / min, and the flow rates of oxygen lances 1 (5) and 2 (6) are both 3000Nm³. 3 / h, the flow rates of oxygen lances 7 (number 3), 8 (number 4), 9 (number 5), and 10 (number 6) are all 1000 Nm³ / h. 3 / h; When 10t of scrap steel is added to the furnace, 1039kg of lime and 997kg of lightly calcined dolomite are added; when 55t of scrap steel is added, 1033kg of lime and 1006kg of lightly calcined dolomite are added; when 100t of scrap steel is added, 1057kg of lime and 1010kg of lightly calcined dolomite are added; a total of 3129kg of lime is added, which is 20.3kg / ton of steel, and a total of 3013kg of lightly calcined dolomite is added, which is 19.5kg / ton of steel. When 90t of scrap steel is added to the furnace, the flow rates of oxygen lances 7 (No. 3), 8 (No. 4), 9 (No. 5), and 10 (No. 6) are all adjusted to 1500Nm. 3 / h; When 140t of scrap steel is added to the furnace, the flow rates of oxygen lances 7 (No. 3), 8 (No. 4), 9 (No. 5), and 10 (No. 6) are all adjusted to 2000 Nm³. 3 / h; 163t of scrap steel was added. After the addition was completed, the flow rates of oxygen lance 5 (No. 1) and oxygen lance 6 (No. 2) were both adjusted to 2000 Nm. 3 / h. After all the scrap steel was added, the temperature was measured and a steel sample was taken 6 minutes later. The carbon content was 0.075%, the phosphorus content was 0.0101%, and the temperature was 1594℃, which met the requirements for tapping. The electrodes were de-energized, the carbon lance was set to standby mode, and the oxygen lance was set to purging mode. 154.2t of steel was tapped, the steel retention ratio was 51.1%, and the smelting cycle was 43min.

[0026] Example 3: The blowing method of this Consteel electric arc furnace is described in detail below.

[0027] A 150t Consteel electric arc furnace is used, with a total steel capacity of 230-250t, producing 45# round steel. 152t of steel is tapped from the eccentric bottom tap hole, leaving 50% of the steel. After the electric arc furnace returns to the horizontal position, the electrodes are energized for heating, and scrap steel is added. The carbon powder injection rate is 120kg / min, and the flow rates of oxygen lances 1 (5) and 2 (6) are both 2600Nm³. 3 / h, the flow rates of oxygen lances 7 (number 3), 8 (number 4), 9 (number 5), and 10 (number 6) are all 600 Nm³ / h. 3 / h; Lime and lightly calcined dolomite are added at scrap steel content of 5%, 32%, and 51% respectively, with a total lime content of 20 kg / t and a total lightly calcined dolomite content of 25 kg / t. When scrap steel content in the furnace reaches 50%, the flow rates of oxygen lances 7 (No. 3), 8 (No. 4), 9 (No. 5), and 10 (No. 6) are all adjusted to 1100 Nm³ / h. 3 / h; When 80% of the scrap steel is added into the furnace, the flow rates of oxygen lances 7 (No. 3), 8 (No. 4), 9 (No. 5), and 10 (No. 6) are all adjusted to 1600 Nm³. 3 / h; After the scrap steel is added, the flow rates of oxygen lance 5 (No. 1) and oxygen lance 6 (No. 2) are both adjusted to 1600 Nm. 3 / h. After all the scrap steel was added, the temperature was measured and a steel sample was taken 4 minutes later. The carbon content was 0.18%, the phosphorus content was 0.0088%, the temperature was 1610℃, and the [C] content was higher than the tapping requirement. The oxygen lance flow rate was adjusted to 2500 Nm. 3 / h, until the steel tapping requirements are met, the electrode is de-energized, the carbon lance is set to standby mode, and the oxygen lance is set to purging mode. The smelting cycle is 49min.

[0028] Example 4: The blowing method of this Consteel electric arc furnace is described in detail below.

[0029] A 150t Consteel electric arc furnace is used, with a total steel capacity of 230-250t, producing Q420B steel. 155.5t of steel is tapped from the eccentric bottom tap hole, leaving a 50.5% steel residue. After the electric arc furnace returns to the horizontal position, the electrodes are energized for heating, and scrap steel is added. The carbon powder injection rate is 60kg / min, and the flow rates of oxygen lances 1 (5) and 2 (6) are both 2800 Nm³. 3 / h, the flow rates of oxygen lances 7 (number 3), 8 (number 4), 9 (number 5), and 10 (number 6) are all 900 Nm³ / h. 3 / h; when the scrap steel content in the furnace is 28%, 49%, and 78%, lime and lightly calcined dolomite are added respectively, with a total lime content of 30 kg / t and a total lightly calcined dolomite content of 15 kg / t. When the scrap steel content in the furnace is 52%, the flow rates of oxygen lances 7 (No. 3), 8 (No. 4), 9 (No. 5), and 10 (No. 6) are all adjusted to 1500 Nm³. 3 / h; When 84% of the scrap steel is added to the furnace, the flow rates of oxygen lances 7 (No. 3), 8 (No. 4), 9 (No. 5), and 10 (No. 6) are all adjusted to 1900 Nm³. 3 / h; After the scrap steel is added, the flow rates of oxygen lance 5 (No. 1) and oxygen lance 6 (No. 2) are both adjusted to 1900 Nm. 3 / h. After all the scrap steel was added, the temperature was measured and a steel sample was taken 8 minutes later. The carbon content was 0.03%, the phosphorus content was 0.0084%, and the temperature was 1605℃. The [C] content was lower than the tapping requirement. Carbon powder was added and the oxygen lance flow rate was adjusted to 1000 Nm. 3 / h, until the steel tapping requirements are met, the electrode is de-energized, the carbon lance is set to standby mode, and the oxygen lance is set to purging mode. The smelting cycle is 48min.

Claims

1. A blowing method for a Consteel electric arc furnace, characterized in that, The electric arc furnace used is equipped with six oxygen lances: oxygen lance 1 (5) and oxygen lance 2 (6) asymmetrically arranged on both sides of the connecting trolley (4); oxygen lance 3 (7) and oxygen lance 4 (8) asymmetrically arranged on both sides of the furnace door (2); and oxygen lance 5 (9) and oxygen lance 6 (10) asymmetrically arranged on both sides of the eccentric furnace bottom taphole (3). The angles between oxygen lance 1 (5) and oxygen lance 2 (6) and the center line of the connecting trolley are 20-40° and 40-60° respectively. 0°, the angles between the No. 3 oxygen lance (7) and the No. 4 oxygen lance (8) and the center line of the furnace door are 20-40° and 40-60° respectively, and the angles between the No. 5 oxygen lance (9) and the No. 6 oxygen lance (10) and the center line of the eccentric furnace bottom taphole are 20-40° and 40-60° respectively; the No. 1 oxygen lance (5), No. 4 oxygen lance (8), No. 3 oxygen lance (7), No. 5 oxygen lance (9), No. 6 oxygen lance (10), and No. 2 oxygen lance (6) are arranged counterclockwise; the following steps are adopted: 1) After the electric arc furnace adopts eccentric bottom tapping, the steel retention ratio is ≥50%. After the electric arc furnace returns to the horizontal position, the electrodes are energized for heating, and scrap steel is added. At the same time, the oxygen lance is started to blow oxygen and the carbon lance is started to inject carbon powder. The flow rates of oxygen lance No. 1 (5) and oxygen lance No. 2 (6) are both 2500~3000 Nm. 3 / h, the flow rate of the remaining oxygen lances is 500-1000 Nm³ / h. 3 / h; 2) Lime and lightly calcined dolomite are added during the time periods when the scrap steel content in the furnace reaches 0-30%, 30-50%, and 50-80%, respectively. After the scrap steel content in the furnace exceeds 50%, the flow rates of oxygen lances No. 3 (7), No. 4 (8), No. 5 (9), and No. 6 (10) are all adjusted to 1000-1500 Nm. 3 / h; After the amount of scrap steel added into the furnace exceeds 80%, the flow rate of oxygen lances No. 3 (7), No. 4 (8), No. 5 (9) and No. 6 (10) is adjusted to 1500~2000 Nm. 3 / h; 3) After all the scrap steel has been added to the furnace, the flow rates of oxygen lance No. 1 (5) and oxygen lance No. 2 (6) are adjusted to 1500-2000 Nm³. 3 / h; After all the scrap steel has been added, the temperature should be measured and a steel sample taken. If the [C] content in the steel sample is higher than the tapping requirement, the oxygen lance flow rate should be adjusted to 2000-3000 Nm. 3 / h; if the [C] content in the steel sample is lower than the tapping requirement, add carbon powder and adjust the oxygen lance flow rate to 500-1500 Nm. 3 / h; When the temperature and composition meet the requirements, prepare to tap the steel.

2. The blowing method of a Consteel electric arc furnace according to claim 1, characterized in that: In step 1), the amount of carbon powder added is 60-120 kg / min; in step 2), the total amount of lime added is 20-30 kg / t, and the total amount of lightly calcined dolomite added is 15-25 kg / t.

3. The blowing method of a Consteel electric arc furnace according to claim 1, characterized in that: All six oxygen lances are set at an angle downwards, with an angle of 30 to 45° to the horizontal.

4. The blowing method of a Consteel electric arc furnace according to claim 3, characterized in that: The first oxygen lance (5), the third oxygen lance (7), and the fifth oxygen lance (9) extend into the furnace at a horizontal distance of 70-100cm, while the second oxygen lance (6), the fourth oxygen lance (8), and the sixth oxygen lance (10) extend into the furnace at a horizontal distance of 40-70cm.

Citation Information

Patent Citations

  • Eccentric bottom electric furnace oxygen lance arrangement structure