LCP extruded films and their manufacturing methods, LCP extruded films for stretching, LCP stretch films, heat-shrinkable LCP stretch films, insulating materials for circuit boards, and metal foil laminates.

By controlling the molecular orientation and internal strain of thermoplastic liquid crystal polymers through three-layer co-extrusion molding and stretching, the problem of large anisotropy of dimensional change rate in insulating materials for circuit boards is solved, and the preparation of highly reliable LCP extruded and stretched films is realized, which can meet the requirements of ultra-fine processing.

CN117400571BActive Publication Date: 2026-11-10DENKA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311289318.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-09
Filing Date
2021-12-07
Publication Date
2026-11-10
Estimated Expiration
2041-12-07

AI Technical Summary

Technical Problem

In the prior art, thermoplastic liquid crystal polymer films used as insulating materials for circuit boards have problems such as large anisotropy of dimensional change rate, difficulty in meeting the requirements of ultra-fine processing, and insufficient manufacturing process margin.

Method used

By controlling the molecular orientation and internal strain of thermoplastic liquid crystal polymers, LCP extruded films and stretched films with low dimensional change rates were prepared using a three-layer co-extrusion molding method and stretching treatment. Aromatic polyester resins and inorganic fillers were used to control the molecular orientation of the film surface and interior.

Benefits of technology

This technology reduces the anisotropy of the dimensional change rate of thermoplastic liquid crystal polymer films, improves the reliability of insulating materials for circuit boards used in ultra-micro processing, and simplifies the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117400571B_ABST
    Figure CN117400571B_ABST
Patent Text Reader

Abstract

This application relates to LCP extruded films and their manufacturing methods, LCP extruded films for stretching treatment, LCP stretch films, heat-shrinkable LCP stretch films, insulating materials for circuit boards, and metal-clad laminates. The LCP extruded film comprises a thermoplastic liquid crystal polymer and has a thickness of 15 μm to 300 μm. The coefficients of linear expansion in the MD and TD directions of the LCP extruded film, as measured by the TMA method according to JIS K7197, are in the range of -30 to 55 ppm / K within 23 to 200 °C, and satisfy the following conditions (A) and / or (B): (A) The orientation degree α1 (%) of the exposed film surface S1 and the orientation degree α2 (%) of the film surface S2 located at a depth of 5 μm from the film surface S1 satisfy the relationship -4.0 ≤ [(α2-α1) / α1] × 100 ≤ 0.0. (B) The hardness H1 at a depth of 1 μm, located 1 μm from the film surface in the thickness direction, and the hardness H2 at the thickness center point, measured by nanoindentation on a film cross section parallel to the MD direction, satisfy -10.0 ≤ 100 × (H2 - H1) / H1 ≤ 0.0.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of Chinese Invention Patent Application No. 202180082926.8 (PCT application number PCT / JP2021 / 044969), filed on December 7, 2021, entitled "LCP Extruded Film and Manufacturing Method Thereof, LCP Extruded Film for Stretching Process, LCP Stretch Film, Heat Shrinkable LCP Stretch Film, Insulating Material for Circuit Board and Metal Foil Laminate". Technical Field

[0002] This invention relates to LCP extruded films and their manufacturing methods, LCP extruded films for stretching treatment, LCP stretched films, heat-shrinkable LCP stretched films, insulating materials for circuit boards, and metal foil laminates, etc. Background Technology

[0003] Previously, a composite material impregnated with varnish was known as an insulating material for circuit boards. This was obtained by impregnating glass cloth with a varnish containing thermosetting resins such as epoxy resin, inorganic fillers, and solvents, followed by hot pressing. However, this method lacks manufacturing process margins and has poor productivity, considering factors such as resin flowability during varnish impregnation and curing properties during hot pressing. Furthermore, thermosetting resins are prone to moisture absorption, causing dimensional changes, resulting in poor dimensional accuracy (heating dimensional accuracy) of the resulting varnish-impregnated composite material.

[0004] On the other hand, liquid crystal polymers (LCPs) are polymers that exhibit liquid crystal properties in the molten or solution state. In particular, thermotropic liquid crystal polymers exhibiting liquid crystal properties in the molten state can be extruded and possess excellent properties such as high gas barrier properties, high film strength, high heat resistance, high insulation, low water absorption, and low dielectric properties in the high-frequency region. Therefore, the practical application of films using thermoplastic liquid crystal polymers in gas barrier film materials, electronic materials, and electrical insulating materials has been investigated.

[0005] However, it has been found that when attempting to implement single-layer extrusion molding, the high liquid crystal orientation of thermoplastic liquid crystal polymers makes it difficult to obtain thermoplastic liquid crystal polymer films with high industrial applicability, i.e., it is difficult to obtain thermoplastic liquid crystal polymer films with excellent thickness accuracy, appearance, and surface flatness.

[0006] Moreover, for example, Patent Document 1 discloses a method that uses a three-layer co-extrusion die instead of a single-layer extrusion die, extruding a fully aromatic polyester thermotropic liquid crystal polymer as the intermediate layer and a polyolefin resin or polycarbonate resin as the two outer layers simultaneously, forming a three-layer laminated film with a thermoplastic liquid crystal polymer layer as the intermediate layer and thermoplastic resin layers as the two outer layers, and peeling off the two outer thermoplastic resin layers to remove the intermediate layer as a film, thereby obtaining a thermoplastic liquid crystal polymer film with excellent thickness accuracy, good appearance, and good surface flatness.

[0007] Furthermore, for example, Patent Document 2 found that the strength of the thermoplastic liquid crystal polymer film described in Patent Document 1 was not practical in the TD direction (Transverse Direction) relative to the MD direction (Machine Direction). It disclosed that by using a three-layer co-extrusion die in the form of a feed block to replace a co-extrusion die in the form of a multi-manifold, the anisotropy of the strength in the TD direction and MD direction (Machine Direction) of the thermoplastic liquid crystal polymer film was mitigated.

[0008] Existing technical documents

[0009] Patent documents

[0010] Patent Document 1: Japanese Patent Application Publication No. 63-31729

[0011] Patent Document 2: Japanese Patent Application Publication No. 2-178016 Summary of the Invention

[0012] The problem that the invention aims to solve

[0013] Liquid crystal polymers have excellent high-frequency characteristics and low dielectric properties, making them increasingly attractive as insulating materials for circuit boards such as flexible printed circuit boards (FPCs), flexible printed circuit board laminates, and fiber-reinforced flexible laminates used in future fifth-generation mobile communication systems (5G), millimeter-wave radar, and other circuit boards.

[0014] The technologies described in Patent Documents 1 and 2 are believed to achieve thermoplastic liquid crystal polymer films with excellent thickness accuracy, appearance, and surface flatness. However, in reality, although the peeling of the skin layer and the peeling of fibrillated fibers caused by the high molecular orientation of the thermoplastic liquid crystal polymer on the film surface can be suppressed, the thermoplastic liquid crystal polymer films described in Patent Documents 1 and 2, as a whole, are still highly molecularly oriented thermoplastic liquid crystal polymers, and cannot withstand practical use as insulating materials for circuit boards.

[0015] Specifically, in applications as insulating materials for circuit boards, thermoplastic liquid crystal polymer films are sometimes used as metal-clad laminates by hot-pressing copper foil or other metal foils onto one or both sides. Furthermore, by patterning or etching the metal foil to form fine wiring, these metal-clad laminates can be used as raw materials for circuit boards such as electronic circuit boards and multilayer boards. Therefore, the thermoplastic liquid crystal polymer film supporting the metal foil requires high dimensional stability. However, in the thermoplastic liquid crystal polymer films described in Patent Documents 1 and 2, the difference in dimensional change rates between the TD and MD directions after etching remains large, failing to meet the application requirements for ultra-fine processing in recent years.

[0016] The present invention was made in view of the above-mentioned problems. One aspect of the present invention aims to provide a novel LCP extrusion film in which the molecular orientation and internal strain of thermoplastic liquid crystal polymers are sufficiently reduced and the anisotropy of the rate of dimensional change is significantly reduced compared with the past, as well as LCP stretch films, insulating materials for circuit boards, metal foil laminates, etc. using the same.

[0017] Another objective of this invention is to provide a method for manufacturing novel LCP extruded films that significantly reduces the high orientation of thermoplastic liquid crystal polymers, which is difficult to avoid in conventional extrusion molding.

[0018] Another objective of this invention is to provide a novel manufacturing method for obtaining LCP extruded films with good reproducibility and ease, in which the molecular orientation and internal strain of the thermoplastic liquid crystal polymer are mitigated not only on the film surface but also inside the film.

[0019] On the other hand, another objective of the present invention is to provide an LCP stretch film with excellent stretchability during stretching processing, thereby achieving anisotropy of dimensional change rate and small absolute value of dimensional change rate with heat shrinkage, and an LCP extruded film for stretching processing. Furthermore, another objective of the present invention is to provide an LCP stretch film with anisotropy of dimensional change rate and small absolute value of dimensional change rate with heat shrinkage, as well as insulating materials for circuit boards, metal foil laminates, etc., using the same.

[0020] Methods for solving problems

[0021] In order to solve the above-mentioned problems, the inventors of this application conducted in-depth research and as a result, produced a new LCP extruded film in which the molecular orientation and internal strain of the thermoplastic liquid crystal polymer are also mitigated, not only on the film surface but also inside the film. In this LCP extruded film, the difference between the orientation degree α1 of the exposed film surface S1 and the orientation degree α2 of the film surface S2 exposed by etching the film surface S1 in the thickness direction and located at a depth of 5 μm from the film surface S1 is small, and the coefficient of linear expansion is small. It was also found that the anisotropy of the dimensional change rate of this LCP extruded film is reduced compared with the past, thus completing one aspect of the present invention.

[0022] That is, one aspect of the present invention provides various specific embodiments as shown below.

[0023] (1) LCP extruded film, which is an LCP extruded film containing thermoplastic liquid crystal polymer and having a thickness of more than 15 μm and less than 300 μm.

[0024] The LCP extruded film satisfies the following conditions (A) and / or condition (B).

[0025] (A) The orientation degree α1 (%) of the exposed film surface S1 and the orientation degree α2 (%) of the film surface S2 located at a depth of 5 μm from the aforementioned film surface S1 after etching the aforementioned film surface S1 in the thickness direction satisfy the relationship -4.0≤[(α2-α1) / α1]×100≤0.0, and the linear expansion coefficients in the MD direction and TD direction within 23 to 200 °C, as determined by the TMA method according to JIS K7197, are in the range of -30 to 55 ppm / K.

[0026] (B) The hardness H1 at a depth of 1 μm at a distance of 1 μm from the film surface in the thickness direction, measured by nanoindentation on a film cross section parallel to the MD direction, and the hardness H2 at the thickness center point satisfy -10.0 ≤ 100 × (H2 - H1) / H1 ≤ 0.0, and the linear expansion coefficients in the MD and TD directions within the range of -30 to 55 ppm / K, as determined by the TMA method according to JIS K7197, are within the range of -30 to 55 ppm / K.

[0027] (2) The LCP extruded film as described in (1), wherein the aforementioned coefficient of linear expansion in the TD direction is 0 to 55 ppm / K.

[0028] (3) The LCP extruded film as described in (1) or (2) is the aforementioned intermediate layer obtained by removing the two outer layers from a laminated extruded film having an outer layer, an intermediate layer and an outer layer.

[0029] (4) The LCP extruded film as described in any one of (1) to (3), wherein the aforementioned film surface S1 does not have a skin layer that can peel off during a tightness test using the cross-cutting method according to JIS K5600-5-6.

[0030] (5) The LCP extruded film as described in any one of (1) to (4), wherein, in the aforementioned condition (A), the aforementioned orientation degree α2 of the aforementioned surface S2 is 37.7% or less.

[0031] (6) The LCP extruded film as described in any one of (1) to (5), wherein, in the aforementioned condition (A), the aforementioned orientation degree α1 of the aforementioned film surface S1 is 39.0% or less.

[0032] (7) The LCP extruded film as described in any one of (1) to (6), wherein, in the aforementioned condition (B), the aforementioned hardness H2 at the aforementioned thickness center point is 0.240 (GPa) or higher.

[0033] (8) The LCP extruded film as described in any one of (1) to (7), wherein, in the aforementioned condition (B), the aforementioned hardness H1 at the aforementioned depth of 1 μm is 0.250 (GPa) or higher.

[0034] (9) The LCP extruded membrane as described in any one of (1) to (8) further contains inorganic fillers.

[0035] (10) The LCP extruded film as described in any one of (1) to (9) is a T-die extruded film.

[0036] (11) An insulating material for a circuit board, comprising a laminate having at least one of (1) to (10) an LCP extruded film and a woven fabric disposed on one or both sides of the aforementioned LCP extruded film.

[0037] (12) A metal foil laminate, comprising any one of (1) to (10) an LCP extruded film and a metal foil disposed on one or both sides of the aforementioned LCP extruded film.

[0038] (13) A metal foil laminate comprising: a laminate having at least one of the LCP extruded film and woven fabric described in (1) to (10); and a metal foil disposed on one and / or both sides of the aforementioned laminate.

[0039] (14) An LCP stretching film having a stretching body of an LCP extruded film as described in any one of (1) to (10).

[0040] (15) The LCP stretch film as described in (14), wherein the aforementioned stretch body has a total stretch ratio (MD direction × TD direction) of 1.3 to 2.5 times that of the aforementioned LCP extruded film.

[0041] (16) An insulating material for a circuit board, comprising a laminate having at least the LCP stretch film described in (14) or (15) and a woven fabric disposed on at least one side of the aforementioned LCP stretch film.

[0042] (17) A metal foil laminate having the LCP stretch film described in (14) or (15) and metal foil disposed on one and / or both sides of the aforementioned LCP stretch film.

[0043] (18) A metal foil laminate having at least a laminate of the LCP stretch film and fabric described in (14) or (15) and a metal foil disposed on one or / on both sides of the aforementioned laminate.

[0044] In addition, the inventors of this application conducted in-depth research on various extrusion molding processes of single-layer and multi-layer films in order to solve the above-mentioned problems. As a result, they found that if two specific three-layer co-extrusion molding methods are used, the high orientation of thermoplastic liquid crystal polymers, which is difficult to avoid in conventional extrusion molding, can be significantly reduced, thereby completing one aspect of the present invention.

[0045] That is, one aspect of the present invention also provides various specific embodiments as shown below.

[0046] (19) A method for manufacturing an LCP extruded film, wherein the aforementioned manufacturing method comprises:

[0047] The process of preparing resin composition A for a first surface layer containing thermoplastic resin, resin composition B for an intermediate layer containing thermoplastic liquid crystal polymer, and resin composition C for a second surface layer containing thermoplastic resin.

[0048] The process of co-extruding the aforementioned resin composition A, the aforementioned resin composition B, and the aforementioned resin composition C from two three-layer extruders under conditions of shear stress below 40 kPa and draw ratio below 3.5, thereby forming two three-layer films having at least the aforementioned first surface layer, the aforementioned intermediate layer, and the aforementioned second surface layer in sequence;

[0049] And an LCP extruded film with a thickness of 15 μm or more and 300 μm or less is obtained by removing the first and second surface layers from the two aforementioned three-layer films.

[0050] (20) The method for manufacturing an LCP extruded film as described in (19), wherein the manufacturing method yields the aforementioned LCP extruded film, wherein the hardness H1 at a depth of 1 μm at a distance of 1 μm from the film surface in the thickness direction, measured by nanoindentation on a film cross section parallel to the MD direction, and the hardness H2 at the thickness center point satisfy -10.0 ≤ 100 × (H2 - H1) / H1 ≤ 0.0, and the linear expansion coefficients in the MD direction and TD direction within 23 to 200 °C, as determined by the TMA method according to JIS K7197, are in the range of -30 to 55 ppm / K.

[0051] (21) The method for manufacturing an LCP extruded film as described in (19) or (20), wherein the aforementioned thermoplastic liquid crystal polymer comprises a (fully) aromatic polyester resin.

[0052] (22) A method for manufacturing an LCP extruded film as described in any one of (19) to (21), wherein the aforementioned thermoplastic resin comprises one selected from the group consisting of polyolefin resins, acrylic resins, polyamide resins, acrylonitrile-butadiene-styrene copolymers, polystyrene, polyvinyl chloride, polybutylene terephthalate, polyethylene terephthalate, polycarbonate, polyetheretherketone, and polyphenylene sulfide.

[0053] (23) A method for manufacturing an LCP extruded film as described in any one of (19) to (22), wherein the aforementioned resin composition B further contains an inorganic filler.

[0054] (24) A method for manufacturing an LCP extruded film as described in any one of (19) to (23), wherein the aforementioned resin composition A, the aforementioned resin composition B and the aforementioned resin composition C are co-extruded from a T-die.

[0055] (25) The method for manufacturing an LCP extruded film as described in any one of (19) to (24), wherein the aforementioned manufacturing method yields an LCP extruded film having a linear expansion coefficient of 55 ppm / K or less in the TD direction.

[0056] (26) A method for manufacturing an LCP extruded film as described in any one of (19) to (25), wherein the obtained LCP extruded film is subjected to heat and pressure treatment at a temperature of 200 to 360°C.

[0057] (27) The method of manufacturing an LCP extruded film as described in any one of (19) to (26), wherein the aforementioned manufacturing method yields an LCP extruded film on the surface of which does not have a skin layer that can peel off during a tightness test performed using the cross-cutting method in accordance with JISK5600-5-6.

[0058] Furthermore, the inventors of this application conducted in-depth research to solve the above-mentioned problems and discovered a novel manufacturing method that can easily and reproducibly produce LCP extrusion films in which the molecular orientation and internal strain of the thermoplastic liquid crystal polymer are mitigated not only on the film surface but also inside the film, thus completing one aspect of the present invention.

[0059] That is, one aspect of the present invention also provides various specific aspects as shown below.

[0060] (28) A method for manufacturing an LCP extruded film, wherein the aforementioned manufacturing method comprises:

[0061] The process of preparing resin composition A for a first surface layer containing thermoplastic resin, resin composition B for an intermediate layer containing thermoplastic liquid crystal polymer, and resin composition C for a second surface layer containing thermoplastic resin.

[0062] The process of co-extruding the aforementioned resin composition A, the aforementioned resin composition B, and the aforementioned resin composition C from two three-layer extruders under conditions of shear stress below 40 kPa and draw ratio below 3.5, thereby forming two three-layer films having at least the aforementioned first surface layer, the aforementioned intermediate layer, and the aforementioned second surface layer in sequence;

[0063] And an LCP extruded film with a thickness of 15 μm to 300 μm obtained by removing the first and second surface layers from the two aforementioned three-layer films, wherein the orientation degree α1 (%) of the exposed film surface S1 and the orientation degree α1 (%) of the film surface S2 located at a depth of 5 μm from the film surface S1 after etching the film surface S1 in the thickness direction satisfy the relationship -4.0 ≤ {(α2-α1) / α1}×100 ≤ 0.0, and the linear expansion coefficients in the MD and TD directions within 23 to 200 °C as measured by the TMA method according to JIS K7197 are in the range of -30 to 55 ppm / K.

[0064] (29) The method for manufacturing an LCP extruded film as described in (28), wherein the aforementioned thermoplastic liquid crystal polymer comprises a (fully) aromatic polyester resin.

[0065] (30) The method for manufacturing an LCP extruded film as described in (28) or (29), wherein the aforementioned thermoplastic resin comprises one selected from the group consisting of polyolefin resins, acrylic resins, polyamide resins, acrylonitrile-butadiene-styrene copolymers, polystyrene, polyvinyl chloride, polybutylene terephthalate, polyethylene terephthalate, polycarbonate, polyetheretherketone and polyphenylene sulfide.

[0066] (31) A method for manufacturing an LCP extruded film as described in any one of (28) to (30), wherein the aforementioned resin composition B further contains an inorganic filler.

[0067] (32) A method for manufacturing an LCP extruded film as described in any one of (28) to (31), wherein the aforementioned resin composition A, the aforementioned resin composition B and the aforementioned resin composition C are co-extruded from a T-die.

[0068] (33) The method for manufacturing an LCP extruded film as described in any one of (28) to (32), wherein the aforementioned manufacturing method yields an LCP extruded film having a linear expansion coefficient of 55 ppm / K or less in the TD direction.

[0069] (34) A method for manufacturing an LCP extruded film as described in any one of (28) to (33), wherein the obtained LCP extruded film is subjected to heat and pressure treatment at a temperature of 200 to 360°C.

[0070] (35) The method of manufacturing an LCP extruded film as described in any one of (28) to (34), wherein the aforementioned manufacturing method yields an LCP extruded film on the aforementioned film surface S1 that does not have a skin layer that can peel off during a tightness test using the cross-cutting method in accordance with JISK5600-5-6.

[0071] In addition, the inventors of this application conducted in-depth research to solve the above-mentioned problems and found that LCP extruded films with specified stretching characteristics have excellent stretchability during stretching treatment. They also discovered that heat-shrinkable LCP stretch films with anisotropy of dimensional change rate and small absolute value of dimensional change rate can be achieved by stretching them, thus completing another aspect of the present invention.

[0072] That is, another aspect of the present invention provides various specific embodiments as shown below.

[0073] (35) A stretch-treated LCP extruded film, which is a stretch-treated LCP extruded film containing a thermoplastic liquid crystal polymer, wherein, in the stress-strain curve determined by a constant temperature bath tensile test (according to JIS K7161-1:2014, 200℃, tensile speed 200mm / min), the yield strength X (MPa) and fracture strength Y (MPa) of the aforementioned stretch-treated LCP extruded film in the TD direction satisfy the following formula (I).

[0074] 0.75≤ fracture strength Y / yield strength X≤1.50···(I).

[0075] (36) The LCP extruded film for stretching treatment as described in (35), wherein the linear expansion coefficient in the TD direction of the aforementioned LCP extruded film for stretching treatment is 5 to 55 ppm / K.

[0076] (37) The LCP extruded film for stretching treatment as described in (35) or (36), wherein the aforementioned LCP extruded film for stretching treatment is a T-die extruded film.

[0077] (38) The LCP extruded film for stretching treatment as described in any one of (35) to (37), wherein the LCP extruded film for stretching treatment is the aforementioned intermediate layer obtained by removing the aforementioned two outer layers from a laminated extruded film having an outer layer, an intermediate layer and an outer layer.

[0078] (39) The LCP extruded film for stretching treatment as described in any one of (35) to (38), wherein the aforementioned LCP extruded film for stretching treatment does not have a skin layer on the film surface that would cause tape peeling during a tightness test performed using the cross-cutting method in accordance with JIS K5600-5-6.

[0079] (40) The LCP extruded film for stretching treatment as described in any one of (35) to (39), wherein the aforementioned LCP extruded film for stretching treatment has a thickness of 15 μm or more and 300 μm or less.

[0080] (41) The LCP extruded membrane for stretching treatment as described in any one of (35) to (40), wherein the aforementioned LCP extruded membrane for stretching treatment further contains inorganic fillers.

[0081] (42) A heat-shrinkable LCP stretch film comprising a stretch body of an LCP extruded film for stretching treatment as described in any one of (35) to (41), wherein the linear expansion coefficient of the stretch body in the TD direction is in the range of -20ppm / K or more and less than 0ppm / K, and the linear expansion coefficient of the stretch body in the MD direction is in the range of -20ppm / K or more and less than 0ppm / K.

[0082] (43) The heat-shrinkable LCP stretch film as described in (42), wherein the stretch body has a stretch ratio of 1.3 to 2.5 times relative to the LCP extruded film for stretching treatment in the TD direction.

[0083] (44) An insulating material for a circuit board, comprising a laminate having at least the heat-shrinkable LCP stretch film described in (42) or (43) and a woven fabric disposed on at least one side of the aforementioned heat-shrinkable LCP stretch film.

[0084] (45) A metal foil laminate having a heat-shrinkable LCP stretch film as described in (42) or (43) and metal foil disposed on one or both sides of the aforementioned heat-shrinkable LCP stretch film.

[0085] (46) A metal foil laminate comprising at least a laminate containing a heat-shrinkable LCP stretch film and a woven fabric as described in (42) or (43), and a metal foil disposed on one and / or both sides of the aforementioned laminate.

[0086] Invention Effects

[0087] According to one aspect of the present invention, novel LCP extruded films, LCP stretched films, insulating materials for circuit boards, and metal-coated laminates with reduced anisotropy in dimensional change rate compared to conventional products can be realized. Furthermore, according to another aspect of the present invention, novel LCP extruded films, LCP stretched films, insulating materials for circuit boards, and metal-coated laminates with inherently small dimensional change rates in both the MD and TD directions can be realized. Therefore, according to various aspects of the present invention, highly reliable products adapted to the ultra-micro processing techniques of recent years can be realized.

[0088] In addition, according to one aspect of the present invention, a novel method for manufacturing a novel LCP extruded film that significantly reduces the high orientation of thermoplastic liquid crystal polymers that is difficult to avoid in conventional extrusion molding can be provided.

[0089] Furthermore, according to one aspect of the present invention, a novel manufacturing method is provided that can readily produce LCP extruded films with good reproducibility, where the molecular orientation and internal strain of the thermoplastic liquid crystal polymer are mitigated not only on the film surface but also inside the film.

[0090] On the other hand, according to another aspect of the present invention, it is possible to realize LCP stretch films with excellent stretchability during stretching processing, thereby achieving anisotropy of dimensional change rate and small absolute value of dimensional change rate, as well as heat-shrinkable LCP extruded films for stretching processing. Furthermore, according to another aspect of the present invention, it is possible to realize novel heat-shrinkable LCP stretch films with anisotropy of dimensional change rate and small absolute value of dimensional change rate, as well as insulating materials for circuit boards using these materials, metal-clad laminates, etc. Therefore, according to various aspects of the present invention, it is possible to realize highly reliable products that are adapted to the ultra-micro processing of recent years. Attached Figure Description

[0091] [ Figure 1 This is a schematic cross-sectional view showing an LCP extruded film as an example of one method.

[0092] [ Figure 2 [A schematic perspective view showing an LCP extruded film as another example of a method.]

[0093] [ Figure 3 [A conceptual diagram illustrating the calculation principle of orientation degree based on the area ratio of orientation peaks.]

[0094] [ Figure 4[A diagram illustrating the calculation method for hardness determination based on nanoindentation.]

[0095] [ Figure 5 [A diagram illustrating a method of co-extrusion of an LCP extruded film.]

[0096] [ Figure 6 [A diagram illustrating a method of co-extrusion of an LCP extruded film.]

[0097] [ Figure 7 [A diagram illustrating a method of co-extrusion of an LCP extruded film.]

[0098] [ Figure 8 This is a schematic cross-sectional view of an insulating material used in a circuit board as an example of one method.

[0099] [ Figure 9 This is a schematic cross-sectional view of an insulating material for a circuit board, which is another example of such a method.

[0100] [ Figure 10 This is a schematic cross-sectional view of a metal foil laminate as an example of one method.

[0101] [ Figure 11 This is a schematic cross-sectional view of a metal foil laminate as another example of a method.

[0102] [ Figure 12 This is a schematic cross-sectional view of a metal foil laminate as an example of one method.

[0103] [ Figure 13 This is a schematic cross-sectional view of a metal foil laminate as another example of a method.

[0104] [ Figure 14 This is a diagram illustrating an example of the stress-strain curve in the TD direction of an LCP extruded film subjected to another type of stretching treatment.

[0105] [ Figure 15 This is a diagram illustrating an example of the stress-strain curve in the TD direction of an LCP extruded film subjected to another type of stretching treatment.

[0106] [ Figure 16 This is a diagram illustrating an example of the stress-strain curve in the TD direction of a prior art LCP extruded film for stretching treatment.

[0107] [ Figure 17 [A diagram illustrating another method of stretching treatment using a co-extrusion process of an LCP extruded film.]

[0108] [ Figure 18 [A diagram illustrating another method of stretching treatment using a co-extrusion process of an LCP extruded film.]

[0109] [ Figure 19 [A diagram illustrating another method of stretching treatment using a co-extrusion process of an LCP extruded film.]

[0110] [ Figure 20 This is a schematic cross-sectional view showing an alternative type of insulating material for a circuit board.

[0111] [ Figure 21 This is a schematic cross-sectional view illustrating another type of metal foil laminate.

[0112] [ Figure 22 This is a schematic cross-sectional view illustrating another type of metal foil laminate. Detailed Implementation

[0113] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. It should be noted that, unless otherwise specified, positional relationships such as up, down, left, and right are based on the positional relationships shown in the accompanying drawings. Furthermore, the scale of the accompanying drawings is not limited to the scale shown. The following embodiments are examples used to illustrate the present invention, and the present invention is not limited to these. That is, the present invention can be implemented in any way without departing from its spirit. It should be noted that, in this specification, expressions of numerical ranges such as "1 to 100" include both the lower limit "1" and the upper limit "100". The same applies to expressions of other numerical ranges.

[0114] (LCP extruded film)

[0115] Figure 1 This is a schematic cross-sectional view showing the main parts of an LCP extruded film 100 according to one embodiment of the present invention. Figure 2 This is a schematic cross-sectional view showing the main portion of an LCP extruded film 100 according to another embodiment of this invention. These LCP extruded films 100 of each embodiment are formed by extruding a resin composition containing a thermoplastic liquid crystal polymer into a film with a thickness of 15 μm or more and 300 μm or less, satisfying the following conditions (A) and / or condition (B).

[0116] (A) The orientation degree α1 (%) of the exposed film surface S1 and the orientation degree α2 (%) of the film surface S2 located at a depth of 5 μm from the aforementioned film surface S1 after etching the aforementioned film surface S1 in the thickness direction satisfy the relationship -4.0≤[(α2-α1) / α1]×100≤0.0, and the linear expansion coefficients in the MD direction and TD direction within 23 to 200 °C, as determined by the TMA method according to JIS K7197, are in the range of -30 to 55 ppm / K.

[0117] (B) The hardness H1 at a depth of 1 μm at a distance of 1 μm from the film surface in the thickness direction, measured by nanoindentation on a film cross section parallel to the MD direction, and the hardness H2 at the thickness center point satisfy -10.0 ≤ 100 × (H2 - H1) / H1 ≤ 0.0, and the linear expansion coefficients in the MD and TD directions within the range of -30 to 55 ppm / K, as determined by the TMA method according to JIS K7197, are within the range of -30 to 55 ppm / K.

[0118] As mentioned above, existing LCP extruded films are films in which the thermoplastic liquid crystal polymer is highly molecularly oriented on the film surface (film surface S1) due to peeling of the skin layer, peeling of fibrillated fibers, etc. This is presumably because the thermoplastic liquid crystal polymer is subjected to shear stress from the side of the device during extrusion, resulting in high orientation of the thermoplastic liquid crystal polymer on the surface of the extruded molded body. Furthermore, although it has been confirmed that the extreme molecular orientation of the thermoplastic liquid crystal polymer on the film surface has been mitigated through improvements such as those in Patent Documents 1 and 2, it has also been discovered, according to the inventors of this application, that simply controlling the molecular orientation of the thermoplastic liquid crystal polymer on the film surface is insufficient to achieve the required performance of a film capable of withstanding the insulating material requirements of a circuit board. That is, in order to achieve an LCP extruded film with reduced anisotropy in dimensional change rate, it is necessary not only to control the molecular orientation of the thermoplastic liquid crystal polymer on the film surface S1, but also to control the molecular orientation of the thermoplastic liquid crystal polymer occurring inside the film (film surface S2), and to reduce internal strain, etc.

[0119] Furthermore, unlike the prior art, the LCP extruded films 100 of this embodiment exhibit reduced molecular orientation and internal strain of the thermoplastic liquid crystal polymer not only on the film surface (film surface S1) but also inside the film (film surface S2), thereby significantly reducing the anisotropy of the dimensional change rate compared to the past. For example, Figure 1 The LCP extruded film 100 of one embodiment shown is characterized at least in that the orientation degree α1 (%) of the exposed film surface S1 and the orientation degree α2 (%) of the film surface S2, exposed by etching the film surface S1 in the thickness direction and located at a depth of 5 μm from the film surface S1, satisfy the relationship -4.0 ≤ [(α2-α1) / α1] × 100 ≤ 0.0, and the linear expansion coefficients in the MD and TD directions, measured by the TMA method according to JIS K7197, are in the range of -30 to 55 ppm / K within 23 to 200 °C. Furthermore, Figure 2The LCP extruded film 100 of another embodiment shown is characterized at least in that the hardness H1 at a depth of 1 μm, located 1 μm from the film surface in the thickness direction, and the hardness H2 at the thickness center point, measured by nanoindentation on a film cross-section parallel to the MD direction, satisfy -10.0 ≤ 100 × (H2 - H1) / H1 ≤ 0.0, and the coefficients of linear expansion in the MD and TD directions, measured by the TMA method according to JIS K7197, are in the range of -30 to 55 ppm / K within 23 to 200 °C. Further details are provided below.

[0120] As the LCP extruded film 100, an extruded film such as a T-die extrusion film is preferred. Furthermore, as the LCP extruded film 100, the intermediate layer (core layer) of a three-layer co-extruded film having a stacked structure of at least a thermoplastic resin layer, a thermoplastic liquid crystal polymer layer, and a thermoplastic resin layer arranged sequentially is also preferred, namely, the thermoplastic liquid crystal polymer layer. In this case, by removing the two outer thermoplastic resin layers of the three-layer co-extruded film, it can be used as a single-layer thermoplastic liquid crystal polymer film (LCP extruded film 100). Compared to woven fabrics and nonwoven fabrics formed from thermoplastic liquid crystal polymer fibers, thermoplastic liquid crystal polymer extruded films can produce homogeneous films at low cost.

[0121] The thermoplastic liquid crystal polymer contained in the LCP extruded film 100 can be any liquid crystal polymer known in the art, and there is no particular limitation on the type. The liquid crystal polymer is a polymer that forms an optically anisotropic molten phase; thermotropic liquid crystal compounds are representative examples. It should be noted that the properties of the anisotropic molten phase can be confirmed by known methods such as polarization examination using crossed polarizers. More specifically, the confirmation of the anisotropic molten phase can be performed by observing the sample placed on a Leitz hot stage at 40x magnification under a nitrogen atmosphere using a Leitz polarizing microscope.

[0122] Specific examples of thermoplastic liquid crystal polymers include polymers obtained by polycondensation of monomers such as aromatic or aliphatic dihydroxy compounds, aromatic or aliphatic dicarboxylic acids, aromatic hydroxycarboxylic acids, aromatic diamines, aromatic hydroxyamines, and aromatic aminocarboxylic acids, but are not particularly limited thereto. The thermoplastic liquid crystal polymer is preferably a copolymer. Specifically, examples include aromatic polyamide resins formed by polycondensation of monomers such as aromatic hydroxycarboxylic acids, aromatic diamines, and aromatic hydroxyamines; (fully)aromatic polyester resins formed by polycondensation of monomers such as aromatic diols, aromatic carboxylic acids, and aromatic hydroxycarboxylic acids; etc., but are not particularly limited thereto. They can be used alone, or in any combination and ratio of two or more.

[0123] Thermoplastic liquid crystal polymers are generally classified into Type I, Type II, Type III, etc., from the viewpoint of heat distortion temperature (TDUL). Regarding the LCP extrusion film 100 of this embodiment, any type of thermoplastic liquid crystal polymer can be suitably used, provided that it is appropriately selected according to the application. For applications requiring lead-free solder at, for example, around 230–260°C, Type I thermoplastic liquid crystal polymers with high heat resistance of around 250–350°C and Type II thermoplastic liquid crystal polymers with relatively high heat resistance of around 240–250°C can be suitably used.

[0124] Of the above, (fully)aromatic polyester resins exhibiting thermotropic liquid crystal-like properties and having a melting point of 250°C or higher, preferably 280°C to 380°C, are preferred. Examples of such (fully)aromatic polyester resins include those synthesized from monomers such as aromatic diols, aromatic carboxylic acids, and hydroxycarboxylic acids, which exhibit liquid crystal properties upon melting. Representative examples include condensation polymers of polyethylene terephthalate and p-hydroxybenzoic acid, condensation polymers of phenol and phthalic acid with p-hydroxybenzoic acid, and condensation polymers of 2,6-hydroxynaphthoic acid with p-hydroxybenzoic acid, but these are not particularly limited to these. It should be noted that one (fully)aromatic polyester resin can be used alone, or two or more can be used in any combination and ratio. Depending on the required performance, fully aromatic polyester resins with relatively high melting points or high heat distortion temperatures and high heat resistance can be used, or aromatic polyester resins with relatively low melting points or low heat distortion temperatures and excellent molding and processability can be used.

[0125] As a preferred embodiment, an example is a (fully)aromatic polyester resin that uses 6-hydroxy-2-naphthoic acid and its derivatives (hereinafter sometimes referred to as "monomer component A") as its basic structure and has at least one monomer component selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthoic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, polyethylene terephthalate and their derivatives (hereinafter sometimes referred to as "monomer component B"). Such a (fully)aromatic polyester resin exhibits an anisotropic molten phase in which the linear chains of its molecules are regularly arranged, typically displaying thermotropic liquid crystal-like properties and possessing excellent basic properties in terms of mechanical properties, electrical properties, high-frequency properties, heat resistance, and hygroscopicity.

[0126] Furthermore, the (fully)aromatic polyester resin of the preferred embodiment described above can have any composition as long as it has monomer component A and monomer component B as essential units. For example, it can have two or more monomer components A, or it can have three or more monomer components A. In addition, the (fully)aromatic polyester resin of the preferred embodiment described above can also contain other monomer components besides monomer components A and B (hereinafter sometimes simply referred to as "monomer component C"). That is, the (fully)aromatic polyester resin of the preferred embodiment described above can be a binary or higher condensation polymer formed only by monomer components A and B, or it can be a ternary or higher condensation polymer formed by monomer components A, B, and C. Other monomer components can be listed besides monomer components A and B, specifically aromatic or aliphatic dihydroxy compounds and their derivatives; aromatic or aliphatic dicarboxylic acids and their derivatives; aromatic hydroxycarboxylic acids and their derivatives; aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids and their derivatives; etc., but are not particularly limited to these. Other monomeric components may be used alone, or in any combination and ratio of two or more.

[0127] It should be noted that, in this specification, the term "derivative" refers to a component obtained by introducing a halogen atom (e.g., fluorine atom, chlorine atom, bromine atom, iodine atom), an alkyl group with 1 to 5 carbon atoms (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, etc.), an aryl group such as phenyl, a hydroxyl group, an alkoxy group with 1 to 5 carbon atoms (e.g., methoxy, ethoxy, etc.), a carbonyl group, or a -O-, -S-, -CH2- group (hereinafter sometimes referred to as "monomer component with substituents"). Here, "derivative" can also refer to ester-forming monomers such as acylates, ester derivatives, or acyl halides of monomer components A and B that may have the aforementioned modifying groups.

[0128] As a particularly preferred embodiment, examples include: binary condensation polymers of p-hydroxybenzoic acid and its derivatives with 6-hydroxy-2-naphthoic acid and its derivatives; ternary or higher condensation polymers of p-hydroxybenzoic acid and its derivatives with 6-hydroxy-2-naphthoic acid and its derivatives and monomeric component C; and polymers composed of p-hydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, and selected from terephthalic acid, isophthalic acid, 6-naphthoic acid, 4,4'-biphenyl, bisphenol A, hydroquinone, and 4,4-dihydroxybiphenyl. These are ternary or higher condensation polymers formed from one or more of the group consisting of phenols, polyethylene terephthalate, and their derivatives; and quaternary or higher condensation polymers formed from one or more of the group consisting of p-hydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, terephthalic acid, isophthalic acid, 6-naphthoic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, polyethylene terephthalate, and their derivatives, and one or more monomeric components C. They can be obtained as substances with lower melting points than, for example, homopolymers of p-hydroxybenzoic acid; therefore, thermoplastic liquid crystal polymers using them exhibit excellent processability in hot-pressing adhesives.

[0129] From the viewpoints of lowering the melting point of the (fully)aromatic polyester resin, improving the processability of the LCP extruded film 100 during hot pressing onto the substrate, or obtaining high peel strength when the LCP extruded film 100 is hot-pressed onto a metal foil, the content of monomer component A relative to the (fully)aromatic polyester resin, calculated by molar ratio, is preferably 10 mol% to 90 mol% or less, more preferably 30 mol% to 85 mol% or less, and even more preferably 50 mol% to 80 mol% or less. Similarly, the content of monomer component B relative to the (fully)aromatic polyester resin, calculated by molar ratio, is preferably 10 mol% to 90 mol% or less, more preferably 15 mol% to 70 mol% or less, and even more preferably 20 mol% to 50 mol% or less. In addition, the content of monomer component C, which can be included in the (fully)aromatic polyester resin, is preferably 10 mol% or less, more preferably 8 mol% or less, even more preferably 5 mol% or less, and particularly preferably 3 mol% or less.

[0130] It should be noted that the synthesis of (fully)aromatic polyester resins can be achieved using any known method, without particular limitation. Known polycondensation methods that utilize the aforementioned monomer components to form ester bonds, such as melt polymerization, melt acid hydrolysis, and slurry polymerization, can be used. When using these polymerization methods, conventional methods can be followed, including acylation or acetylation steps.

[0131] The LCP extruded film 100 may also contain inorganic fillers. By including inorganic fillers, it is possible to achieve an LCP extruded film 100 with a reduced coefficient of linear expansion. Specifically, it is easy to obtain an LCP extruded film 100 with reduced anisotropy of the coefficient of linear expansion in the MD direction, TD direction, and ZD direction (Z-axis Direction; film thickness direction). Such an LCP extruded film 100 is particularly useful in applications such as rigid substrates requiring multilayer lamination.

[0132] Inorganic packing materials can be any inorganic packing materials known in the art, and there is no particular limitation on their types. Examples include kaolin, calcined kaolin, calcined clay, uncalcined clay, silica (e.g., natural silica, fused silica, amorphous silica, hollow silica, wet silica, synthetic silica, AEROSIL (fumed silica)), aluminum compounds (e.g., boehmite, aluminum hydroxide, aluminum oxide, hydrotalcite, aluminum borate, aluminum nitride), magnesium compounds (e.g., magnesium aluminosilicate, magnesium carbonate, magnesium oxide, magnesium hydroxide), calcium compounds (e.g., calcium carbonate, calcium hydroxide, calcium sulfate, calcium sulfite, calcium borate), molybdenum compounds (e.g., molybdenum oxide, zinc molybdate), talc (e.g., natural talc, calcined talc), mica, titanium dioxide, zinc oxide, zirconium oxide, barium sulfate, zinc borate, barium metaborate, sodium borate, boron nitride, condensed boron nitride, silicon nitride, carbon nitride, strontium titanate, barium titanate, zinc stannate, etc., but are not specifically limited to these. They can be used individually or in combination of two or more. Of the above, silicon dioxide is preferred from the viewpoint of dielectric properties, etc.

[0133] Alternatively, the inorganic filler used herein may be an inorganic filler that has undergone surface treatments known in the art. Surface treatment can improve moisture resistance, bond strength, dispersibility, etc. Examples of surface treatment agents include silane coupling agents, titanate coupling agents, sulfonates, carboxylic esters, and phosphate esters, but are not particularly limited thereto.

[0134] The median particle size (d50) of the inorganic filler can be appropriately set according to the required performance and is not particularly limited. Considering factors such as mixing properties, operability, and reduction of the coefficient of linear expansion during preparation, the d50 of the inorganic filler is preferably 0.01 μm to 50 μm, more preferably 0.03 μm to 50 μm, and even more preferably 0.1 μm to 50 μm. It should be noted that, in this specification, the median particle size (d50) of the inorganic filler refers to the value measured using a laser diffraction / scattering particle size distribution measuring device (Horiba Manufacturing Co., Ltd. LA-500) with a volume basis, employing the laser diffraction and scattering method.

[0135] The content of inorganic fillers can be appropriately set according to the required performance, taking into account the balance with other essential and optional components, and is not particularly limited. From the viewpoints of mixing properties, operability, and the effect of reducing the coefficient of linear expansion during preparation, the content of inorganic fillers is preferably 1% to 45% by mass, more preferably 3% to 40% by mass, and even more preferably 5% to 35% by mass, based on the total solid content relative to the total amount of LCP extruded film 100.

[0136] The LCP extrusion film 100 may also contain resin components other than the aforementioned thermoplastic liquid crystal polymer (hereinafter sometimes simply referred to as "other resin components"), such as thermosetting resins and thermoplastic resins, within a range that does not excessively impair the effects of the present invention. Furthermore, the LCP extrusion film 100 may also contain additives known in the art, such as release modifiers (e.g., higher fatty acids with 10-25 carbon atoms, higher fatty acid esters, higher fatty acid amides, higher fatty acid metal salts, polysiloxanes, fluoropolymers, etc.); colorants (e.g., dyes, pigments); organic fillers; antioxidants; heat stabilizers; light stabilizers; ultraviolet absorbers; flame retardants; antistatic agents; surfactants; rust inhibitors; defoamers; fluorescent agents, etc. These additives may be used individually or in combination of two or more. These additives may be included in the molten resin composition prepared during the molding of the LCP extrusion film 100. The content of these resin components and additives is not particularly limited, but from the viewpoint of molding processability, thermal stability, etc., it is preferable that each is 0.01 to 10% by mass relative to the total amount of LCP extruded film 100, more preferably 0.1 to 7% by mass, and even more preferably 0.5 to 5% by mass.

[0137] The thickness of the LCP extruded film 100 can be appropriately set according to the required performance and is not particularly limited. Considering the operability and productivity during extrusion molding, it is preferably 15μm to 300μm, more preferably 18μm to 250μm, and even more preferably 20μm to 200μm.

[0138] Here, the LCP extruded film 100 of this embodiment only needs to satisfy the above conditions (A) and / or (B), and there is no particular limitation. That is, the LCP extruded film 100 of this embodiment may only satisfy the above conditions (A), may only satisfy the above conditions (B), or may satisfy both of the above conditions (A) and (B). Among the above, it is preferable to satisfy both of the above conditions (A) and (B).

[0139] For example, from the viewpoint of mitigating the molecular orientation and internal strain of the thermoplastic liquid crystal polymer not only on the film surface (film surface S1) but also inside the film (film surface S2) and reducing the anisotropy of the target dimensional change rate, the LCP extruded film 100 that satisfies the above condition (A) is adjusted in such a way that the orientation degree α1 of the film surface S1 and the orientation degree α2 of the film surface S2 satisfy the relationship shown below.

[0140] The preferred value is -4.0≤[(α2-α1) / α1]×100≤0.0.

[0141] More preferably, -3.0≤[(α2-α1) / α1]×100≤0.0.

[0142] A further preferred value is -2.0≤[(α2-α1) / α1]×100≤0.0.

[0143] Here, as Figure 1 As shown, membrane surface S1 is the outermost surface of the LCP extruded membrane 100 of this embodiment, and is the exposed surface facing outward. The orientation degree (orientation degree α1) including membrane surface S1 is preferably 39.0% or less, more preferably 38.5% or less, and even more preferably 38.0% or less. On the other hand, membrane surface S2 is the surface newly exposed by etching the membrane surface S1 of the LCP extruded membrane 100 of this embodiment in the thickness direction. Figure 1 In the diagram, a dashed line represents an imaginary surface located 5 μm from the film surface S1. The orientation degree (orientation degree α2) of the film surface S2 is preferably 37.7% or less, more preferably 37.5% or less, and even more preferably 37.3% or less. Furthermore, considering dissolution errors during etching, the depth of the film surface S2 does not need to be strictly 5 μm from the film surface S1; a depth of 5.0 μm or more from the film surface S1 is sufficient. Additionally, the etching conditions used to fabricate the film surface S2 are not particularly limited; from the viewpoint of ensuring the objectivity of the measurement data, the conditions described in the examples described later are used.

[0144] It should be noted that, in this specification, the orientation degrees α1 and α2 (%) of the LCP extruded film 100, including film surfaces S1 and S2, mean: values ​​calculated by the following formula based on the area ratio of the orientation peak in the obtained diffraction intensity distribution curve obtained by X-ray diffraction measurement using a transmission method with an X-ray diffraction device. Typically, in the case of a test object with a small orientation degree (%), diffraction peaks with low intensity and wide widths are observed in X-ray diffraction measurements. Therefore, the calculation method based on the half-width at half-maximum (HWHM) of the orientation peak cannot ensure high measurement accuracy. Therefore, in this specification, the orientation degree α1 of the film surface S1 and the orientation degree α2 (%) of the film surface S2 are calculated separately using a calculation method based on the area ratio of the orientation peak, not the HWHM of the orientation peak. Specifically, as... Figure 3 As shown in Equation 1, as a method for calculating the area ratio based on orientation peaks, the intensity of the peak (orientation component) is measured by 2θ / θ scanning, and the intensity in the azimuth direction from 0° to 360° is measured by β scanning to obtain the intensity distribution in the azimuth direction (baseline intensity (isotropic component)). The proportion of the area occupied by the orientation component after removing the area of ​​the isotropic component as the baseline in the total area (area of ​​orientation component + area of ​​isotropic component) is calculated as the orientation degree (%).

[0145] [Mathematical Expression 1]

[0146]

[0147] On the other hand, from the viewpoint of mitigating the molecular orientation and internal strain of the thermoplastic liquid crystal polymer not only on the film surface but also inside the film, and reducing the anisotropy of the target dimensional change rate, the LCP extruded film 100 that satisfies the above condition (B) is adjusted in such a way that the hardness H1 at a depth of 1 μm at a distance of 1 μm from the film surface in the thickness direction and the hardness H2 at the thickness center point, measured by nanoindentation on a film cross section parallel to the MD direction, satisfy the relationship shown below.

[0148] The preferred value is -10.0≤100×(H2-H1) / H1≤0.0.

[0149] More preferably, -7.5≤100×(H2-H1) / H1≤0.0.

[0150] A further preferred value is -5.0≤100×(H2-H1) / H1≤0.0.

[0151] The relationship expressed by the above formula, namely the relationship between the hardness H1 at a depth of 1 μm and the hardness H2 at the center of the thickness, indicates the orientation of the thermoplastic liquid crystal polymer in the film. The lower the absolute value, the more isotropic the orientation is towards the MD and TD directions.

[0152] Here, as Figure 2As shown, the hardness H1 at a point 1 μm deep in the thickness direction, located 1 μm from the film surface in the film cross-section parallel to the MD direction (a position 1 μm from one side of the film surface in the thickness direction when viewed from above), is an indicator of the molecular orientation and internal strain of the thermoplastic liquid crystal polymer near the film surface of the LCP extruded film 100. There is a tendency that the lower the orientation of the thermoplastic liquid crystal polymer, the greater the hardness H1 at the 1 μm depth point; conversely, there is a tendency that the higher the orientation of the thermoplastic liquid crystal polymer, the smaller the hardness H1 at the 1 μm depth point. Furthermore, the hardness H1 at the 1 μm depth point is preferably 0.250 GPa or more, more preferably 0.255 GPa or more. On the other hand, the hardness H2 at the thickness center point in the film cross-section parallel to the MD direction (a position equidistant from the film surface on one side and the film surface on the other side when viewed from above), is an indicator of the molecular orientation and internal strain of the thermoplastic liquid crystal polymer inside the LCP extruded film 100. The lower the orientation of the thermoplastic liquid crystal polymer, the greater the hardness H2 at the thickness center point; conversely, the higher the orientation of the thermoplastic liquid crystal polymer, the smaller the hardness H2 at the thickness center point. The hardness H2 at the thickness center point is preferably 0.240 GPa or higher, more preferably 0.245 GPa or higher. It should be noted that the method for fabricating the cross-section of the LCP extruded film 100 parallel to the MD direction is not particularly limited. From the viewpoint of ensuring the objectivity of the measured data, the LCP extruded film 100 is subjected to ion beam processing under freezing conditions to produce a smooth cross-section parallel to the MD direction.

[0153] It should be noted that the hardness measurement based on nanoindentation in this specification is performed under the following conditions: using a diamond Berkovich indenter (Berkovich indenter), with an indentation depth hmax = 0.05 μm, the hardness H1 at a point 1 μm from the film surface and the hardness H2 at the center of the thickness are measured on a cross-section of the film parallel to the MD direction of the LCP extruded film 100. Additionally, as... Figure 4 As shown, the hardness H1 and hardness H2 are calculated based on the maximum load Pmax and the contact projection area A (the area of ​​contact between the indenter and the membrane cross section) using the following formula.

[0154] Hardness (GPa) = Pmax / A

[0155] On the other hand, the LCP extruded films 100 of each embodiment not only sufficiently reduce the molecular orientation of the thermoplastic liquid crystal polymer as expressed by the aforementioned orientation degree, but also sufficiently reduce the molecular orientation of the thermoplastic liquid crystal polymer as expressed by the coefficients of linear expansion in the MD and TD directions. As mentioned above, the LCP extruded films described in prior art patent documents 1 and 2, by being protected by the two outer thermoplastic resin layers during three-layer co-extrusion, mitigate the molecular orientation of the thermoplastic liquid crystal polymer to a certain extent, thereby mitigating the anisotropy of the strength in the MD and TD directions of the resulting thermoplastic liquid crystal polymer film. That being said, in reality, the coefficient of linear expansion in the MD direction of the LCP extruded films described in patent documents 1 and 2 can stably reach about -20 ppm / K, while the coefficient of linear expansion in the TD direction exceeds 55 ppm, sometimes reaching about 100 ppm / K. From this, it is easy to understand that, as a whole, the LCP extruded films described in prior art patent documents 1 and 2 still retain a large amount of the molecular orientation of the thermoplastic liquid crystal polymer, or a large amount of internal strain, etc. Therefore, the molecular orientation and internal strain of the thermoplastic liquid crystal polymer of the LCP extruded film 100 as a whole need to be controlled by the combination of the orientation degree and coefficient of linear expansion of the film surface and / or the combination of hardness and coefficient of linear expansion based on nanoindentation.

[0156] Specifically, the coefficients of linear expansion (CTE, α2, 23–200°C) in the MD and TD directions of the LCP extruded film 100 of this embodiment are in the range of -30 to 55 ppm / K. LCP extruded films 100 with coefficients of linear expansion within this range are in a state where internal strain is sufficiently reduced. Compared to films that are not in this range, they exhibit less anisotropy in dimensional change rate, and furthermore, LCP extruded films with sufficiently small absolute values ​​of dimensional change rate can be obtained. From the viewpoint of improving adhesion to metal foils, the coefficient of linear expansion (CTE, α2, 23–200°C) in the MD direction of the LCP extruded film 100 of this embodiment is preferably in the range of -30 to 10 ppm / K, more preferably in the range of -25 to 5 ppm / K, and even more preferably in the range of -20 to 0 ppm / K. Furthermore, from the viewpoint of improving adhesion to the metal foil, the coefficient of linear expansion (CTE, α2, 23–200°C) in the TD direction of the LCP extruded film 100 of this embodiment is preferably in the range of 0–55 ppm / K, more preferably in the range of 0–50 ppm / K, and even more preferably in the range of 0–45 ppm / K. It should be noted that, in this specification, the coefficient of linear expansion (CTE, α2, 23–200°C) refers to the value measured using the TMA method according to JIS K7197 within the temperature range of 23–200°C. Other detailed measurement conditions are as described in the examples described later.

[0157] It should be noted that in this specification, the linear expansion coefficient is determined using the TMA method according to JIS K 7197. The average linear expansion coefficient refers to the average value of the linear expansion coefficients measured by this method from 23 to 200°C. The linear expansion coefficient measured here refers to the value obtained by heating the LCP extruded film 100 at a heating rate of 5°C / min (1st heating), cooling it to the ambient temperature (23°C), and then heating it a second time at a heating rate of 5°C / min (2nd heating) to observe the value after eliminating the thermal history. Other detailed measurement conditions are as described in the examples below.

[0158] On the other hand, the dielectric properties of the LCP extruded film 100 of this embodiment can be appropriately set according to the desired performance, and are not particularly limited. From the viewpoint of obtaining higher dielectric properties, the relative permittivity ε... r The dielectric constant ε (36GHz) is preferably 3.0 or higher and 3.7 or lower, more preferably 3.0 to 3.5. Similarly, the dielectric loss tangent tanδ (36GHz) is preferably 0.0010 or higher and 0.0050 or lower, more preferably 0.0010 or higher and 0.0045 or lower. It should be noted that in this specification, the relative permittivity ε... r The values ​​(36GHz) and dielectric loss tangent tanδ(36GHz) refer to the values ​​at 36GHz measured using the cavity resonator perturbation method according to JIS K6471. Other detailed measurement conditions are as described in the examples below.

[0159] (Manufacturing method of LCP extruded film)

[0160] The LCP extruded film 100 of each embodiment can be obtained by extruding a resin composition containing the above-mentioned thermoplastic liquid crystal polymer and optional components such as inorganic fillers and other resin components to a specified thickness. Various known methods can be used for extrusion, and there is no particular limitation on the type. Any combination of methods can be applied: for example, T-die method, blow molding method; for example, multi-manifold co-extrusion method, feed block co-extrusion method; for example, two-layer co-extrusion method, three-layer co-extrusion method, and other multi-layer co-extrusion methods.

[0161] From the viewpoint of ease of controlling the molecular orientation of the thermoplastic liquid crystal polymer on the film surface (film surface S1) and inside the film (film surface S2), a preferred method is to extrude the resin composition from a T-die and form it into a film using a T-die extrusion molding method (hereinafter sometimes simply referred to as "T-die extrusion"), and then perform cooling treatment, pressing treatment, pressure heating treatment, etc., as needed to obtain the specified LCP extruded film 100. Specifically, the following co-extrusion method is preferred: a resin composition A containing a first surface layer of thermoplastic resin, a resin composition B containing a thermoplastic liquid crystal polymer for an intermediate layer, and a resin composition C containing a second surface layer of thermoplastic resin are prepared in advance, and they are co-extruded from a co-extrusion die of an extruder to extrude a co-extruded melt consisting of three layers, and the LCP extruded film 100 is formed in the form of a thermoplastic liquid crystal polymer layer in the intermediate layer. With such co-extrusion molding, the molecular orientation of the thermoplastic liquid crystal polymer in the intermediate layer is moderated by being protected by the two outer thermoplastic resin layers. Hereinafter, a preferred embodiment of the method for manufacturing the LCP extruded film 100 of this embodiment will be described in detail.

[0162] Figures 5-7 This diagram illustrates a preferred embodiment of the method for manufacturing the LCP extruded film 100 according to this embodiment. Here, the resin composition B described above, containing the thermoplastic liquid crystal polymer and optional components such as inorganic fillers and other resin components, is melt-extruded from the T-die of an extruder in a film form. At this time, by co-extruding the resin compositions A and C containing the thermoplastic resin onto both sides of the film-shaped melt extrudate, a co-extruded melt (three-layer laminate) of a predetermined thickness is produced, comprising a first outer layer (release layer) containing thermoplastic resin, an intermediate layer (LCP layer) containing thermoplastic liquid crystal polymer, and a second outer layer (release layer) containing thermoplastic resin. This co-extruded melt is picked up by a pick-up roller and fed to a cooling roller and a pressing roller. Then, the first and second outer layers are peeled off from the intermediate layer, and the thermoplastic resin layers of the two outer layers and the thermoplastic liquid crystal polymer layer of the intermediate layer (LCP extruded film 100) are respectively wound onto a winding roller.

[0163] The preparation of the resin composition B containing the thermoplastic liquid crystal polymer described above can be carried out using conventional methods without particular limitations. Known methods such as mixing, melt mixing, granulation, extrusion molding, pressurization, or injection molding can be used to manufacture and process the above components. It should be noted that during melt mixing, commonly used single-screw or twin-screw extruders, various kneaders, and other mixing devices can be used. When supplying the components to these melt mixing devices, the liquid crystal polymer, other resin components, inorganic fillers, additives, etc., can also be pre-mixed using a mixing device such as a roller mixer or Henschel mixer. During melt mixing, the barrel temperature of the mixing device can be set appropriately without particular limitations; generally, a range of 360°C above the melting point of the liquid crystal polymer is preferred, and more preferably, a range of 10°C above the melting point of the liquid crystal polymer and 360°C below.

[0164] The preparation of resin compositions A and C containing thermoplastic resins can be carried out using conventional methods and is not particularly limited. Examples of thermoplastic resins include, for instance, polyolefin resins such as polyethylene, polypropylene, polymethylpentene, and ethylene-α-olefin copolymer; acrylic resins such as PMMA; polyamide resins; acrylonitrile-butadiene-styrene copolymer (ABS resin); polystyrene (PS); polyvinyl chloride; polybutylene terephthalate (PBT); polyethylene terephthalate (PET); polycarbonate (PC); polyetheretherketone (PEEK); and polyphenylene sulfide (PPS), but these are not particularly limited. When forming a co-extruded melt, both polar resins such as polycarbonate and non-polar resins such as polymethylpentene can effectively function as a release layer. Other optional components, such as resin components and inorganic fillers, that may be included in the LCP extrusion film 100 described above can be incorporated into these thermoplastic resins. It should be noted that resin composition A and resin composition C may have the same resin composition or different resin compositions; they may contain the same thermoplastic resin or different thermoplastic resins. Furthermore, resin compositions containing thermoplastic resins can be manufactured and processed using known methods such as mixing, melt mixing, granulation, extrusion molding, pressurization, or injection molding. It should be noted that during melt mixing, commonly used single-screw or twin-screw extruders, various kneaders, and other mixing devices can be used. When supplying the components to these melt mixing devices, the liquid crystal polymer, other resin components, inorganic fillers, additives, etc., can be pre-mixed using mixing devices such as rollers or Henschel mixers. During melt mixing, the barrel temperature of the mixing device can be appropriately set as long as it is below the temperature at which the thermoplastic resin does not undergo pyrolysis and deterioration; there is no particular limitation. Generally, it is preferable to be above the melting point of the thermoplastic resin, and more preferably above the melting point of the thermoplastic resin +10°C.

[0165] The settings for co-extrusion can be appropriately set according to the type and composition of the resin composition used, and the desired performance of the extruded film as the target, and are not particularly limited. For example, the set temperature of the extruder barrel can be appropriately set according to the type and composition of the resin composition used, and the desired performance of the extruded film as the target, and is not particularly limited, preferably 230 to 360°C, more preferably 280 to 350°C.

[0166] In addition, the width (mm) of the T-die can be appropriately set according to the type and composition of the resin composition used, the desired performance of the extruded film as the target, etc., and is not particularly limited. It is usually preferred to be 200 to 2000 mm, and more preferably 400 to 1500 mm.

[0167] Furthermore, the die lip opening (mm) of the T-die, for example, can also be appropriately set according to the type and composition of the resin composition used, the desired performance of the extruded film as the target, etc., without particular limitation. It is generally preferred to be 0.1 to 3.0 (mm), and more preferably 0.2 to 2.0 (mm).

[0168] Furthermore, for example, the shear rate (sec) of the lip wall of the T-mode -1 Similarly, the value can be appropriately set according to the type and composition of the resin composition used, the desired performance of the extruded film as the target, etc., and there is no particular limitation. Generally, 100 to 1500 (sec) is preferred. -1 ), more preferably 150 to 1000 (sec) -1 ).

[0169] In addition, the total amount of resin composition extruded from the T-mold (mm) 3 Similarly, the value ( / sec) can be appropriately set according to the type and composition of the resin composition used, the desired performance of the extruded film as the target, etc., and is not particularly limited, but is generally preferred to be 500 to 15000 (mm). 3 / sec), more preferably 1500~10000 (mm) 3 / sec).

[0170] On the other hand, the melt viscosity (Pa·sec) of the thermoplastic liquid crystal polymer can also be appropriately set according to the type and composition of the resin composition used, the desired performance of the target extruded film, etc., and is not particularly limited, but is generally preferred to be 10 to 300 (Pa·sec), and more preferably 20 to 250 (Pa·sec). It should be noted that the melt viscosity (Pa·sec) of the thermoplastic liquid crystal polymer refers to the value measured according to JIS K7199 using a Capilograph 1D (manufactured by Toyo Seiki Co., Ltd.) under the conditions of a barrel length of 10.00 mm, a barrel diameter of 1.00 mm, and a barrel body diameter of 9.55 mm, under the conditions of manufacturing the LCP extruded film 100 (die temperature and shear rate of the lip wall).

[0171] In addition, the pick-up speed (mm / sec) of the co-extruded film can also be set appropriately according to the type and composition of the resin composition used and the desired performance of the target extruded film. There is no particular limitation, but it is generally preferred to be 15 to 1000 (mm / sec), and more preferably 20 to 500 (mm / sec).

[0172] Here, from the perspective of reducing the molecular orientation of the thermoplastic liquid crystal polymer along the MD direction during co-extrusion, a low shear stress (kPa) during co-extrusion is ideal. High shear stress during co-extrusion tends to result in high orientation of the thermoplastic liquid crystal polymer along the MD direction and also tends to leave residual internal strain. Conversely, low shear stress during co-extrusion tends to easily reduce the molecular orientation of the thermoplastic liquid crystal polymer both on the film surface (film surface S1) and inside the film (film surface S2), and also tends to prevent residual internal strain. It should be noted that the shear stress (kPa) during co-extrusion is the shear rate (sec) at the lip wall. -1 The shear rate is expressed as the product of the total amount of resin composition extruded during co-extrusion and the melt viscosity (Pa·sec) of the thermoplastic liquid crystal polymer. The shear rate is calculated based on the total amount of resin composition extruded, the die width, and the die lip opening during co-extrusion. Therefore, the shear stress during co-extrusion can be controlled by adjusting the above values. Specifically, the shear stress during co-extrusion is preferably 40 kPa or less, more preferably 38 kPa or less, and even more preferably 36 kPa or less. It should be noted that the lower limit is not particularly limited; considering productivity, it is preferably 5 kPa or more, and more preferably 10 kPa or more.

[0173] Furthermore, from the viewpoint of reducing the molecular orientation of the thermoplastic liquid crystal polymer along the MD direction during co-extrusion, a low draw ratio during co-extrusion is ideal. A high draw ratio during co-extrusion tends to result in high orientation of the thermoplastic liquid crystal polymer along the MD direction and a tendency for internal strain to remain. Conversely, a low draw ratio tends to easily reduce the molecular orientation of the thermoplastic liquid crystal polymer at both the film surface (film surface S1) and the film interior (film surface S2), and a tendency for internal strain to remain. It should be noted that the draw ratio is a value expressed as the pick-up speed (mm / sec) / the flow rate of the thermoplastic liquid crystal polymer (mm / sec), and the flow rate of the thermoplastic liquid crystal polymer is calculated based on the total extrusion volume of the resin composition during co-extrusion, the die width, and the die lip opening. Therefore, the draw ratio during co-extrusion can be controlled by adjusting these values. Specifically, the draw ratio during co-extrusion is preferably 3.5 or less, more preferably 3.3 or less, and even more preferably 3.1 or less. It should be noted that there is no particular limitation on its lower limit value. If productivity and other factors are taken into account, it is preferable to be 1.0 or higher, and more preferably 1.2 or higher.

[0174] The thickness of the resulting LCP extruded film 100 can be appropriately set according to the required performance, and there is no particular limitation. Considering the operability and productivity during extrusion molding, it is preferably 15 μm to 300 μm, more preferably 18 μm to 250 μm, and even more preferably 20 μm to 200 μm.

[0175] The melting point (melting temperature) of the obtained LCP extruded film 100 is not particularly limited. However, from the viewpoint of heat resistance and processability, a melting point (melting temperature) of 200–400°C is preferred. Especially from the viewpoint of improving hot-pressing properties with metal foil, 250–360°C is preferred, more preferably 260–355°C, further preferably 270–350°C, and particularly preferably 275–345°C. It should be noted that, in this specification, the melting point of the LCP extruded film 100 refers to the melting peak temperature obtained by differential scanning calorimetry (DSC) using a DSC8500 (PerkinElmer) in a temperature range of 30–400°C, after heating the extruded film at a heating rate of 20°C / min (first heating), cooling it at a cooling rate of 50°C / min (first cooling), and then heating it again at a heating rate of 20°C / min (second heating). In addition, regarding other matters, the measurement conditions are as described in the examples described later.

[0176] It should be noted that the LCP extruded film 100 formed by extrusion can be used directly, but it can also be further pressurized and heated as needed to further reduce the molecular orientation (anisotropy) of the thermoplastic liquid crystal polymer or further release the internal strain. This can also result in an LCP extruded film 100 with further reduced anisotropy of dimensional change rate and a smaller absolute value of dimensional change rate.

[0177] The heating and pressurizing treatment can be performed using methods known in the art, such as contact heat treatment or non-contact heat treatment, and there is no particular limitation on the type. For example, known equipment such as non-contact heaters, ovens, blowing devices, hot rollers, cooling rollers, hot presses, and double-belt hot presses can be used for heat setting. At this time, if necessary, a release film or a porous film known in the art can be disposed on the surface of the LCP extruded film 100 and then heat-treated. In addition, when performing this heat treatment, from the viewpoint of controlling orientation, it is preferable to use the following hot pressing method: a release film and a porous film are disposed on the surface and back of the LCP extruded film 100, and hot-pressed together while being held between the annular belts of a double-belt press, and then the release film and the porous film are removed. The hot pressing method can be performed by referring to, for example, Japanese Patent Application Laid-Open No. 2010-221694. As for the processing temperature during hot pressing of the LCP extruded film 100 using the above-described resin composition between the annular belt pairs of a dual-belt press, in order to control the crystallization state of the LCP extruded film 100, it is preferable to perform the process at a temperature higher than the melting point of the liquid crystal polymer and lower than 70°C above the melting point, more preferably at a temperature higher than 5°C above the melting point and lower than 60°C above the melting point, and even more preferably at a temperature higher than 10°C above the melting point and lower than 50°C above the melting point. The hot pressing conditions can be appropriately set according to the desired performance and are not particularly limited. It is preferable to perform the process at a surface pressure of 0.5 to 10 MPa and a heating temperature of 250 to 430°C, more preferably at a surface pressure of 0.6 to 8 MPa and a heating temperature of 260 to 400°C, and even more preferably at a surface pressure of 0.7 to 6 MPa and a heating temperature of 270 to 370°C. On the other hand, when using non-contact heaters or ovens, it is preferable to carry out the process at 200–320°C for 1–20 hours.

[0178] (Insulating material for circuit boards)

[0179] Figure 8 and Figure 9This is a schematic cross-sectional view showing the main parts of the insulating material 200 for circuit boards according to this embodiment. The insulating material 200 for circuit boards according to this embodiment includes a laminate having at least an LCP extruded film 100 that satisfies the above conditions (A) and / or (B) and a woven fabric WF disposed on one or both sides of the LCP extruded film 100.

[0180] Specifically, the insulating material 200 for the circuit board comprises a laminate having a three-layer structure in which an LCP extruded film 100, a woven fabric WF, and the LCP extruded film 100 are arranged at least sequentially. In this laminate, one LCP extruded film 100 is disposed on the surface side of the woven fabric WF, and another LCP extruded film 100 is disposed on the back side of the woven fabric WF. These three layers are heat-pressed together to form a three-layer laminate. It should be noted that a three-layer laminate is illustrated here, but the present invention can be implemented in the form of a two-layer laminate with one LCP extruded film 100 omitted, or in the form of a laminate with four or more layers obtained by further stacking LCP extruded films 100 and woven fabric WF, which is self-evident.

[0181] In this specification, the term "woven fabric WF disposed on one and / or both sides of LCP extrusion film 100" means not only that the LCP extrusion film 100 is directly placed on the surface of the woven fabric WF as in this embodiment, but also that any layer (e.g., base layer, adhesive layer, etc.) not shown is sandwiched between the LCP extrusion film 100 and the woven fabric WF, or that the LCP extrusion film 100 and the woven fabric WF are separately disposed.

[0182] Woven fabric (WF) is a fabric obtained by weaving fibers. There is no particular limitation on the type of fiber used in woven fabric (WF); any of inorganic fibers, organic fibers, or organic-inorganic hybrid fibers can be used. In particular, woven fabric (WF) made of inorganic fibers is preferred. By heat-pressing the inorganic fiber woven fabric (WF) to the LCP extrusion film 100, the anisotropy of the dimensional change rates in the MD and TD directions can be kept small, thereby reducing the dimensional change rates themselves in the MD and TD directions in a suitable manner. Commercially available woven fabrics (WF) can be used; alternatively, they can be manufactured using methods known in the art.

[0183] Examples of inorganic fibers include, for example, glass fibers such as E-glass, D-glass, L-glass, M-glass, S-glass, T-glass, Q-glass, UN-glass, NE-glass, and spherical glass, inorganic fibers other than glass such as quartz, and ceramic fibers such as silica, but these are not particularly limited to these. Regarding woven fabrics (WF) of inorganic fibers, fabrics that have undergone fiber-opening treatment and mesh-clogging treatment are suitable from the viewpoint of dimensional stability. Among the above, glass cloth is preferred from the viewpoints of mechanical strength, dimensional stability, and water absorption. From the viewpoint of improving heat-bonding properties with the LCP extruded film 100, glass cloth that has undergone fiber-opening treatment and mesh-clogging treatment is preferred. Additionally, glass cloth obtained through surface treatments based on silane coupling agents, such as epoxy-silane treatment or amino-silane treatment, can also be suitably used. It should be noted that one type of fiber can be used alone or in appropriate combinations of two or more types of fibers in the woven fabric (WF).

[0184] The thickness of the woven fabric (WF) can be appropriately set according to the required performance and is not particularly limited. From the viewpoints of lamination, processability, and mechanical strength, it is preferably 10 to 300 μm, more preferably 10 to 200 μm, and even more preferably 15 to 180 μm.

[0185] The total thickness of the insulating material 200 for the circuit board can be appropriately set according to the required performance and is not particularly limited. From the viewpoints of lamination, processability, and mechanical strength, it is preferably 30 to 500 μm, more preferably 50 to 400 μm, even more preferably 70 to 300 μm, and particularly preferably 90 to 250 μm.

[0186] The circuit board insulating material 200 of this embodiment, by adopting the above-described configuration, has the following significant effects: the anisotropy of the dimensional change rate in the MD and TD directions is small, thereby reducing the dimensional change rate itself in the MD and TD directions in a suitable manner; furthermore, it has excellent dielectric properties in the high-frequency region, is easy to manufacture, and has excellent productivity.

[0187] The aforementioned insulating material 200 for circuit boards can be manufactured using known methods, and the manufacturing method is not particularly limited. For example, an LCP extruded film 100 and a woven fabric WF can be laminated and heated and pressurized, and the LCP extruded film 100 and the woven fabric WF can be hot-pressed together to obtain the insulating material 200 for circuit boards. Alternatively, the following method is preferred: LCP extruded film 100, woven fabric WF, and LCP extruded film 100 are sequentially laminated to form a laminate, and the laminate is heated and pressurized while being held using a press, a double-belt press, etc., thereby hot-pressing the insulating material 200 for circuit boards. It should be noted that the processing temperature during hot pressing can be appropriately set according to the required performance and is not particularly limited; preferably 200–400°C, more preferably 250–360°C, and even more preferably 270–350°C. It should be noted that the processing temperature during hot pressing is a value measured from the surface temperature of the LCP extruded film 100 of the aforementioned laminate. In addition, the pressurization conditions at this time can be appropriately set according to the desired performance, without particular limitation, for example, the surface pressure is 0.5 to 10 MPa and the time is 1 to 240 minutes, more preferably the surface pressure is 0.8 to 8 MPa and the time is 1 to 120 minutes.

[0188] (Metal foil laminate)

[0189] Figure 10 and Figure 11 This is a schematic cross-sectional view showing the main parts of the metal-coated foil laminate 300 of this embodiment. The metal-coated foil laminate 300 of this embodiment includes an LCP extruded film 100 that satisfies the above conditions (A) and / or (B) and a metal foil MF disposed on one side and / or both sides of the LCP extruded film 100.

[0190] Specifically, the metal foil laminate 300 is a two-sided metal foil laminate having a laminated structure (three-layer structure) in which metal foil MF, LCP extruded film 100, and metal foil MF are arranged at least sequentially. These three layers are heat-pressed together to form a three-layer laminate. It should be noted that this embodiment shows a two-sided metal foil laminate, but the invention can also be implemented with metal foil MF only on one surface of the LCP extruded film 100. That is, a three-layer laminate is illustrated here, but the invention can be implemented as a two-layer laminate omitting one metal foil MF, or as a laminate with four or more layers obtained by further laminating LCP extruded film 100 and woven fabric WF, which is self-evident.

[0191] Figure 12 and Figure 13This is a schematic cross-sectional view showing the main parts of the metal-coated foil laminate 400 of this embodiment. The metal-coated foil laminate 400 of this embodiment includes at least an LCP extruded film 100 that satisfies the above conditions (A) and / or (B), a laminate containing the above-mentioned woven fabric WF disposed on one and / or both sides of the LCP extruded film 100, and a metal foil MF disposed on one and / or both sides of the laminate.

[0192] Specifically, the metal foil laminate 400 is a double-sided metal foil laminate having a laminated structure (five-layer structure) in which metal foil MF, LCP extruded film 100, woven fabric WF, LCP extruded film 100, and metal foil MF are arranged at least sequentially. These five layers are heat-pressed together to form a five-layer laminate. It should be noted that this embodiment shows a double-sided metal foil laminate, but the present invention can also be implemented with metal foil MF on only one surface. That is, a five-layer laminate is illustrated here, but the present invention can be implemented as a four-layer laminate with one metal foil MF omitted, or as a laminated structure with six or more layers obtained by further laminating LCP extruded film 100, circuit board insulating material 200, and woven fabric WF, which is self-evident.

[0193] The material of the metal foil MF is not particularly limited, and examples include gold, silver, copper, copper alloys, nickel, nickel alloys, aluminum, aluminum alloys, iron, and iron alloys. Among these, copper foil, aluminum foil, stainless steel foil, and copper-aluminum alloy foil are preferred, and copper foil is more preferred. As the copper foil, any copper foil manufactured by rolling or electrolysis can be used, but electrolytic copper foil or rolled copper foil with a large surface roughness is preferred.

[0194] The thickness of the metal foil MF can be appropriately set according to the desired performance and is not particularly limited. It is typically preferred to be 1.5–1000 μm, more preferably 2–500 μm, further preferably 5–150 μm, and particularly preferably 7–100 μm. It should be noted that, as long as the effectiveness of the invention is not impaired, the metal foil MF can also undergo surface treatments such as acid cleaning or other chemical surface treatments. It should also be noted that the type and thickness of the metal foil MF can be the same or different.

[0195] The method for depositing metal foil MF on the surface of LCP extruded film 100 and circuit board insulating material 200 can be performed using conventional methods and is not particularly limited. It can also be any method among those that involve laminating metal foil MF onto LCP extruded film 100 and circuit board insulating material 200 and bonding or pressing the two layers together, physical methods such as sputtering and vapor deposition (dry methods), chemical methods such as non-electroplating and electroplating after non-electroplating (wet methods), and methods such as coating with metal paste. Alternatively, a multi-stage press, a multi-stage vacuum press, a continuous forming machine, or an autoclave forming machine can be used to hot-press the laminate formed by laminating LCP extruded film 100, circuit board insulating material 200, and one or more metal foils MF, thereby obtaining metal foil-coated laminates 300 and 400.

[0196] The aforementioned metal foil laminates 300 and 400 can be manufactured using known methods, and the manufacturing method is not particularly limited. For example, one method could be as follows: an LCP extruded film 100, a circuit board insulating material 200, and a metal foil MF are laminated to form a laminate on which the metal foil MF is placed, and the laminate is then hot-pressed while being held between the annular belts of a dual-belt press. As described above, the LCP extruded film 100 used in this embodiment has low anisotropy in the MD and TD directions, and consequently, in a suitable manner, the dimensional change rates in the MD and TD directions are themselves small, thus achieving high peel strength with the metal foil MF.

[0197] The temperature during hot pressing of the metal foil MF can be appropriately set according to the required performance and is not particularly limited. Preferably, it is a temperature 50°C or more lower than the melting point of the liquid crystal polymer and 50°C or less higher than the melting point; more preferably, it is a temperature 40°C or more lower than the melting point of the liquid crystal polymer and 40°C or less higher than the melting point; even more preferably, it is a temperature 30°C or more lower than the melting point of the liquid crystal polymer and 30°C or less higher than the melting point; particularly preferably, it is a temperature 20°C or more lower than the melting point of the liquid crystal polymer and 20°C or less higher than the melting point. It should be noted that the temperature during hot pressing of the metal foil MF is a value measured in the form of the surface temperature of the aforementioned LCP extruded film 100. In addition, the pressing conditions at this time can be appropriately set according to the desired performance and are not particularly limited. For example, when using a dual-belt press, it is preferable to perform the pressing under the conditions of a surface pressure of 0.5 to 10 MPa and a heating temperature of 200 to 360°C.

[0198] The metal foil laminates 300 and 400 of this embodiment, as long as they are heat-pressed bodies with a double-layer structure of LCP extruded film 100 and metal foil MF, can also have other laminated structures or further laminated structures. For example, they can be made into: a two-layer structure of metal foil MF / LCP extruded film 100; a three-layer structure such as metal foil MF / LCP extruded film 100 / metal foil MF, LCP extruded film 100 / metal foil MF / LCP extruded film 100; a four-layer structure such as metal foil MF / LCP extruded film 100 / woven fabric WF / LCP extruded film 100; a five-layer structure such as metal foil MF / LCP extruded film 100 / metal foil MF / LCP extruded film 100 / metal foil MF, metal foil MF / LCP extruded film 100 / woven fabric WF / LCP extruded film 100 / metal foil MF; and so on, multi-layer structures. In addition, multiple (e.g., 2 to 50) metal foil laminates 300 and 400 can be laminated and heat-pressed together.

[0199] In the metal-coated laminates 300 and 400 of this embodiment, the peel strength between the LCP extruded film 100 and the metal foil MF is not particularly limited. However, from the viewpoint of achieving higher peel strength, it is preferable to have a peel strength of 0.8 (N / mm) or higher, more preferably 1.0 (N / mm) or higher, and even more preferably 1.2 (N / mm) or higher. As described above, the metal-coated laminates 300 and 400 of this embodiment can achieve high peel strength, thus, for example, peeling between the LCP extruded film 100 and the metal foil MF can be suppressed during the heating process of substrate manufacturing. Furthermore, when obtaining peel strength equivalent to that of the prior art, manufacturing conditions with excellent process margin and productivity can be applied. Therefore, it is possible to suppress the deterioration of the basic properties of the liquid crystal polymer while maintaining the same level of peel strength as before.

[0200] Furthermore, for the metal foil laminates 300 and 400 of this embodiment, at least a portion of the metal foil MF can be patterned or etched, thereby making it suitable as a raw material for circuit boards such as electronic circuit boards and multilayer boards. In addition, the metal foil laminates 300 and 400 of this embodiment have excellent dielectric properties in the high-frequency region, small anisotropy in the dimensional change rate in the MD and TD directions, and thus, in a suitable manner, the dimensional change rate in the MD and TD directions is small, resulting in excellent dimensional stability, ease of manufacturing, and high productivity. Therefore, they are particularly useful raw materials as insulating materials for flexible printed wiring boards (FPCs) in fifth-generation mobile communication systems (5G), millimeter-wave radar, etc.

[0201] (LCP stretch film)

[0202] It should be noted that the above embodiments use an LCP extruded film 100 formed by extruding a resin composition containing a thermoplastic liquid crystal polymer in a film form. However, if necessary, the LCP extruded film 100 can also be further subjected to uniaxial and / or biaxial stretching treatment to be used as an LCP stretched film (a stretched body of the LCP extruded film 100). Furthermore, the LCP stretched film can also be used to construct the above-mentioned circuit board insulating material 200, metal foil laminate 300, 400, etc.

[0203] The stretching conditions can be set appropriately based on the type and composition of the resin composition used and the desired performance of the LCP stretched film, and are not particularly limited. For uniaxial stretching, it is preferable to stretch the LCP extruded film 100 along the TD direction (transverse direction; short side direction) at 90–180°C by 1.1–2.5 times, followed by heat treatment (heat setting) at 100–240°C for 1–600 seconds. For biaxial stretching, it is preferable to stretch the LCP extruded film 100 along the MD direction (machine direction; long side direction) at 70–180°C by 1.1–2.5 times to form a uniaxial stretched film, then further stretch it along the TD direction (transverse direction; short side direction) at 90–180°C by 1.1–2.5 times, followed by heat treatment (heat setting) at 100–240°C for 1–600 seconds. Alternatively, biaxial stretching can be performed simultaneously instead of gradually. The stretching ratio is not particularly limited, but from the viewpoints of improving film transportability and demolding properties, suppressing thickness unevenness, and preventing wrinkles, the total stretching ratio in the MD direction × TD direction (where the stretching ratio in the MD direction is set as m and the stretching ratio in the TD direction is set as n, and m × n represents the stretching ratio) is preferably 1.1 times or more, more preferably 1.2 times or more, further preferably 1.3 times or more, and particularly preferably 1.5 times or more. It should be noted that there is no particular upper limit, but the target is 3.0 times or less, preferably 2.7 times or less, further preferably less than 2.5 times, and particularly preferably less than 2.3 times. Furthermore, during heat setting, methods known in the art can be implemented, such as contact heat treatment, non-contact heat treatment, etc., and the type is not particularly limited. For example, known equipment such as non-contact heaters, ovens, blowing devices, hot rollers, cooling rollers, hot presses, and double-belt hot presses can be used for heat setting. At this time, if necessary, a release film or a porous film known in the art can be disposed on the surface of the LCP stretch film and then subjected to hot pressing.

[0204] The coefficients of linear expansion (CTE, α2, 23~200℃) in the MD and TD directions of the LCP extruded film 100 (the stretched body of the LCP extruded film 100) can be appropriately set according to the desired performance, without particular limitation. From the viewpoint of reducing the anisotropy of the dimensional change rate and the absolute value of the dimensional change rate, and improving the adhesion with the metal foil, it is preferred that each is in the range of -20~15ppm / K, more preferably in the range of -15~10ppm / K, further preferably in the range of -10~5ppm / K, and particularly preferably in the range of -10~0ppm / K.

[0205] (LCP extruded film for stretching treatment)

[0206] The following describes in detail a stretched LCP extruded film (LCP extruded film before stretching treatment, sometimes simply referred to as "LCP extruded film for stretching treatment") that can be suitably used as a precursor film for LCP stretching films. The stretched LCP extruded film described herein is another aspect of the present invention, which is an LCP extruded film (stretched LCP extruded film) containing a thermoplastic liquid crystal polymer and capable of being uniformly stretched during stretching treatment.

[0207] As mentioned above, existing LCP extruded films are films in which the thermoplastic liquid crystal polymer is highly molecularly oriented on the film surface due to peeling of the skin layer, peeling of fibrillated fibers, etc. This is presumably due to the shear stress from the side of the extrusion device during extrusion, resulting in high orientation of the thermoplastic liquid crystal polymer on the surface of the extruded molded body. Furthermore, even with such high orientation of the thermoplastic liquid crystal polymer in existing LCP extruded films, it is expected that anisotropy of dimensional change rate and small absolute value of dimensional change rate can be achieved by performing stretching treatment. However, according to the inventors of this application, it has been found that existing LCP extruded films have almost no stretchability during stretching treatment, making it practically difficult to obtain industrially useful LCP stretching films. Specifically, existing LCP extruded films, for example, exhibit uneven stretching even when stretched by a stretching ratio of 1.1 times along the TD direction, or film breakage occurs when the stretching ratio along the TD direction is increased to, for example, 1.2 times, indicating a lack of stretchability. On the other hand, although it has been confirmed that the extreme molecular orientation in the surface of the thermoplastic liquid crystal polymer film is mitigated by improvements such as those in Patent Documents 1 and 2, at the same time, according to the inventors of this application, it has been found that simply controlling the molecular orientation of the thermoplastic liquid crystal polymer in the film surface is not enough to achieve a film that can withstand the required performance of an insulating material for a circuit board.

[0208] From the above perspective, the LCP extruded film (stretched LCP extruded film) for stretching treatment in this embodiment was studied. Specifically, the LCP extruded film (stretched LCP extruded film) for stretching treatment in this embodiment possesses good stretchability at least along the TD direction by having specified stretching characteristics, thus enabling uniform stretching that is difficult to achieve in the prior art. Furthermore, by stretching the stretched LCP extruded film, the molecular orientation and internal strain of the thermoplastic liquid crystal polymer occurring on the film surface and / or inside the film are reduced, thereby enabling the achievement of anisotropic dimensional change rates and a small absolute value of heat shrinkage in the LCP stretching film.

[0209] The thermoplastic liquid crystal polymer contained in the LCP extruded film for stretching can be any liquid crystal polymer known in the art, and there is no particular limitation on the type. Liquid crystal polymers are polymers that form an optically anisotropic molten phase; thermotropic liquid crystal compounds are representative examples. It should be noted that the properties of the anisotropic molten phase can be confirmed by known methods such as polarization examination using crossed polarizers. More specifically, the confirmation of the anisotropic molten phase can be performed by observing the sample placed on a Leitz hot stage at 40x magnification under a nitrogen atmosphere using a Leitz polarizing microscope.

[0210] Specific examples of thermoplastic liquid crystal polymers include polymers obtained by polycondensation of monomers such as aromatic or aliphatic dihydroxy compounds, aromatic or aliphatic dicarboxylic acids, aromatic hydroxycarboxylic acids, aromatic diamines, aromatic hydroxyamines, and aromatic aminocarboxylic acids, but are not particularly limited thereto. The thermoplastic liquid crystal polymer is preferably a copolymer. Specifically, examples include aromatic polyamide resins formed by polycondensation of monomers such as aromatic hydroxycarboxylic acids, aromatic diamines, and aromatic hydroxyamines; (fully)aromatic polyester resins formed by polycondensation of monomers such as aromatic diols, aromatic carboxylic acids, and aromatic hydroxycarboxylic acids; etc., but are not particularly limited thereto. They can be used individually or in any combination and ratio of two or more.

[0211] Thermoplastic liquid crystal polymers are generally classified into Type I, Type II, Type III, etc., from the viewpoint of heat distortion temperature (TDUL). For the LCP extruded film for stretching processing in this embodiment, any type of thermoplastic liquid crystal polymer can be used appropriately, as long as it is selected according to the application. In electronic circuit board applications requiring application in lead-free solder at, for example, around 230–260°C, Type I thermoplastic liquid crystal polymers with high heat resistance of around 250–350°C and Type II thermoplastic liquid crystal polymers with relatively high heat resistance of around 240–250°C can be used appropriately.

[0212] Of the above, a fully aromatic polyester resin exhibiting thermotropic liquid crystal-like properties and having a melting point of 250°C or higher, preferably 280°C to 380°C, is preferred. Such fully aromatic polyester resins are known, for example, those synthesized from monomers such as aromatic diols, aromatic carboxylic acids, and hydroxycarboxylic acids that exhibit liquid crystal properties upon melting. Representative examples include condensation polymers of polyethylene terephthalate and p-hydroxybenzoic acid, condensation polymers of phenol and phthalic acid with p-hydroxybenzoic acid, and condensation polymers of 2,6-hydroxynaphthoic acid with p-hydroxybenzoic acid, but these are not particularly limited to these. It should be noted that a single fully aromatic polyester resin can be used alone, or two or more can be used in any combination and ratio. Depending on the required performance, a fully aromatic polyester resin with a relatively high melting point or high heat distortion temperature and high heat resistance can be used, or an aromatic polyester resin with a relatively low melting point or low heat distortion temperature and excellent molding processability can be used.

[0213] As a preferred embodiment, an example is a (fully)aromatic polyester resin that uses 6-hydroxy-2-naphthoic acid and its derivatives (hereinafter sometimes referred to as "monomer component A") as its basic structure and has at least one monomer component selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthoic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, polyethylene terephthalate and their derivatives (hereinafter sometimes referred to as "monomer component B"). Such a (fully)aromatic polyester resin exhibits an anisotropic molten phase in which the linear chains of its molecules are regularly arranged, typically displaying thermotropic liquid crystal-like properties and possessing excellent basic properties in terms of mechanical properties, electrical properties, high-frequency properties, heat resistance, and hygroscopicity.

[0214] Furthermore, the (fully)aromatic polyester resin of the preferred embodiment described above can have any composition as long as it has monomer component A and monomer component B as essential units. For example, it can have two or more monomer components A, or it can have three or more monomer components A. In addition, the (fully)aromatic polyester resin of the preferred embodiment described above can also contain other monomer components besides monomer components A and B (hereinafter sometimes simply referred to as "monomer component C"). That is, the (fully)aromatic polyester resin of the preferred embodiment described above can be a condensation polymer of two or more monomer components formed only by monomer components A and B, or it can be a condensation polymer of three or more monomer components formed by monomer components A, B, and C. Other monomer components can be listed besides monomer components A and B, specifically aromatic or aliphatic dihydroxy compounds and their derivatives; aromatic or aliphatic dicarboxylic acids and their derivatives; aromatic hydroxycarboxylic acids and their derivatives; aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids and their derivatives; etc., but are not particularly limited to these. Other monomeric components may be used alone, or in any combination and ratio of two or more.

[0215] It should be noted that, in this specification, the term "derivative" refers to a component obtained by introducing a halogen atom (e.g., fluorine atom, chlorine atom, bromine atom, iodine atom), an alkyl group with 1 to 5 carbon atoms (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, etc.), an aryl group such as phenyl, a hydroxyl group, an alkoxy group with 1 to 5 carbon atoms (e.g., methoxy, ethoxy, etc.), a carbonyl group, or a -O-, -S-, -CH2- group, etc. (hereinafter, it is sometimes referred to as "monomer component with substituents"). Here, "derivative" can also refer to ester-forming monomers such as acylates, ester derivatives, or acyl halides of monomer components A and B that may have the aforementioned modifying groups.

[0216] As a particularly preferred embodiment, examples include: binary condensation polymers of p-hydroxybenzoic acid and its derivatives with 6-hydroxy-2-naphthoic acid and its derivatives; ternary or higher condensation polymers of p-hydroxybenzoic acid and its derivatives with 6-hydroxy-2-naphthoic acid and its derivatives and monomeric component C; and polymers composed of p-hydroxybenzoic acid and its derivatives with 6-hydroxy-2-naphthoic acid and its derivatives and selected from terephthalic acid, isophthalic acid, 6-naphthoic acid, 4,4'-biphenyl, bisphenol A, hydroquinone, and 4,4-dihydroxybiphenyl. These are ternary or higher condensation polymers formed from one or more of the group consisting of phenols, polyethylene terephthalate, and their derivatives; and quaternary or higher condensation polymers formed from one or more of the group consisting of p-hydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, terephthalic acid, isophthalic acid, 6-naphthoic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, polyethylene terephthalate, and their derivatives, and one or more monomeric components C. They can be obtained as substances with lower melting points than, for example, homopolymers of p-hydroxybenzoic acid; therefore, thermoplastic liquid crystal polymers using them exhibit excellent processability in hot-pressing adhesives.

[0217] From the viewpoints of lowering the melting point of (fully)aromatic polyester resin, improving the processability of LCP extruded film or its stretched body when hot-pressed onto an adherend, or obtaining high peel strength when hot-pressing LCP extruded film or its stretched body onto a metal foil, the content of monomer component A relative to (fully)aromatic polyester resin, calculated by molar ratio, is preferably 10 mol% to 90 mol% or less, more preferably 30 mol% to 85 mol% or less, and even more preferably 50 mol% to 80 mol% or less. Similarly, the content of monomer component B relative to (fully)aromatic polyester resin, calculated by molar ratio, is preferably 10 mol% to 90 mol% or less, more preferably 15 mol% to 70 mol% or less, and even more preferably 20 mol% to 50 mol% or less. In addition, the content of monomer component C, which may also be included in (fully)aromatic polyester resin, is preferably 10 mol% or less, more preferably 8 mol% or less, even more preferably 5 mol% or less, and particularly preferably 3 mol% or less.

[0218] It should be noted that the synthesis of (fully)aromatic polyester resins can be achieved using any known method, without particular limitation. Known polycondensation methods that utilize the aforementioned monomer components to form ester bonds, such as melt polymerization, melt acid hydrolysis, and slurry polymerization, can be used. When using these polymerization methods, conventional methods can be followed, including acylation or acetylation steps.

[0219] LCP extruded films for stretching can also contain inorganic fillers. By including inorganic fillers, it is possible to achieve LCP extruded films for stretching with a reduced coefficient of linear expansion. Specifically, it is easy to obtain LCP extruded films for stretching with reduced anisotropy of the coefficient of linear expansion in the MD direction, TD direction, and ZD direction (Z-axis direction; film thickness direction). Such LCP extruded films for stretching are particularly useful in applications such as rigid substrates requiring multilayer stacking.

[0220] Inorganic packing materials can be any inorganic packing materials known in the art, and there is no particular limitation on their types. Examples include kaolin, calcined kaolin, calcined clay, uncalcined clay, silica (e.g., natural silica, fused silica, amorphous silica, hollow silica, wet silica, synthetic silica, AEROSIL (fumed silica)), aluminum compounds (e.g., boehmite, aluminum hydroxide, aluminum oxide, hydrotalcite, aluminum borate, aluminum nitride), magnesium compounds (e.g., magnesium aluminosilicate, magnesium carbonate, magnesium oxide, magnesium hydroxide), calcium compounds (e.g., calcium carbonate, calcium hydroxide, calcium sulfate, calcium sulfite, calcium borate), molybdenum compounds (e.g., molybdenum oxide, zinc molybdate), talc (e.g., natural talc, calcined talc), mica, titanium dioxide, zinc oxide, zirconium oxide, barium sulfate, zinc borate, barium metaborate, sodium borate, boron nitride, condensed boron nitride, silicon nitride, carbon nitride, strontium titanate, barium titanate, zinc stannate, etc., but are not specifically limited to these. They can be used individually or in combination of two or more. Of the above, silicon dioxide is preferred from the viewpoint of dielectric properties, etc.

[0221] Alternatively, the inorganic filler used herein may be an inorganic filler that has undergone surface treatments known in the art. Surface treatment can improve moisture resistance, bond strength, dispersibility, etc. Examples of surface treatment agents include silane coupling agents, titanate coupling agents, sulfonates, carboxylic esters, and phosphate esters, but are not particularly limited thereto.

[0222] The median particle size (d50) of the inorganic filler can be appropriately set according to the required performance and is not particularly limited. Considering factors such as mixing properties, operability, and reduction of the coefficient of linear expansion during preparation, the d50 of the inorganic filler is preferably 0.01 μm to 50 μm, more preferably 0.03 μm to 50 μm, and even more preferably 0.1 μm to 50 μm. It should be noted that, in this specification, the median particle size (d50) of the inorganic filler refers to the value measured using a laser diffraction / scattering particle size distribution measuring device (Horiba Manufacturing Co., Ltd. LA-500) with a volume basis, employing the laser diffraction and scattering method.

[0223] The content of inorganic fillers can be appropriately set according to the required performance, taking into account the balance with other essential and optional components, and is not particularly limited. From the viewpoints of mixing properties, operability, and the effect of reducing the coefficient of linear expansion during preparation, the content of inorganic fillers is preferably 1% to 45% by mass, more preferably 3% to 40% by mass, and even more preferably 5% to 35% by mass, based on the total solid content of the LCP extruded film for relative stretching treatment.

[0224] The LCP extruded film for stretching can also contain resin components other than the aforementioned thermoplastic liquid crystal polymer (hereinafter sometimes simply referred to as "other resin components"), such as thermosetting resins and thermoplastic resins, within a range that does not excessively impair the effects of the present invention. Furthermore, the LCP extruded film for stretching can also contain additives known in the art, such as release modifiers (e.g., higher fatty acids with 10-25 carbon atoms, higher fatty acid esters, higher fatty acid amides, higher fatty acid metal salts, polysiloxanes, fluoropolymers, etc.); colorants (e.g., dyes, pigments); organic fillers; antioxidants; heat stabilizers; light stabilizers; ultraviolet absorbers; flame retardants; antistatic agents; surfactants; rust inhibitors; defoamers; fluorescent agents, etc. These additives can be used individually or in combination of two or more. These additives can be included in the molten resin composition prepared during the molding of the LCP extruded film for stretching. The content of these resin components and additives is not particularly limited, but from the viewpoint of molding processability, thermal stability, etc., it is preferable that each is 0.01 to 10% by mass relative to the total amount of LCP extruded film for stretching treatment, more preferably 0.1 to 7% by mass, and even more preferably 0.5 to 5% by mass.

[0225] The LCP extruded film for stretching treatment according to this embodiment has specified tensile properties, and therefore, unlike the prior art, it has good tensile adaptability at least along the TD direction, and can be stretched uniformly during stretching treatment. Specifically, in the stress-strain curves of the LCP extruded film for stretching treatment according to this embodiment, measured by a constant temperature bath tensile test (according to JIS K7161-1:2014, 200°C, tensile speed 200 mm / min), the yield strength X (MPa) and breaking strength Y (MPa) of the aforementioned LCP extruded film for stretching treatment in the TD direction satisfy the following formula (I).

[0226] 0.75 ≤ fracture strength Y / yield strength X ≤ 1.50 ···(I)

[0227] Here, the tensile test conducted according to JIS K7161-1:2014 involves stretching the test specimen along its main axis at a constant speed (a constant speed perpendicular to the cross-section of the specimen) until the specimen breaks. The force and elongation of the specimen are then measured. The yield strength X (MPa) refers to the highest point in the yield region of the stress-strain curve obtained in the tensile test. A higher value indicates a greater force required to deform the material. Conversely, the fracture strength Y (MPa) refers to the stress just before the specimen breaks in the tensile test. A higher value indicates a greater force required to break the material. Furthermore, the fracture strength Y / yield strength X is the ratio of the fracture strength Y to the yield strength X in the stress-strain curve obtained from the tensile test. Figure 14 and Figure 15 This is a diagram illustrating an example of the stress-strain curve in the TD direction of the LCP extruded film for stretching processing according to the present invention, satisfying 0.75 ≤ Y / X ≤ 1.50. Additionally, Figure 16 This is a diagram illustrating an example of the stress-strain curves in the TD direction of a prior art LCP extruded film undergoing tensile processing, equivalent to Y / X < 0.75. From these... Figures 14-16 As can be understood from the comparison, the LCP extruded film for stretching treatment of the present invention has a larger strength ratio of breaking strength Y / yield strength X compared with the prior art, and therefore has uniform tensile properties under a certain load. Furthermore, the displacement (horizontal axis) of the breaking strength Y from the yield strength X is related to the stretching ratio; a large displacement indicates that a high stretching ratio can be applied. That is, it can be understood that the LCP extruded film for stretching treatment of this embodiment, which satisfies the above formula (I), differs from the prior art in that it can achieve more uniform stretching and can also be applied at a higher stretching ratio.

[0228] The value of the fracture strength Y / yield strength X in the TD direction is not particularly limited, but is preferably 0.80 to 1.50, more preferably 0.85 to 1.50, even more preferably 0.90 to 1.35, and particularly preferably 0.90 to 1.20. There is a tendency that the larger this value, the higher the uniform tensile strength along the TD direction. It should be noted that, in this specification, from the viewpoint of ensuring measurement accuracy, the value of fracture strength Y / yield strength X is set as the average value of five tensile tests performed under the conditions described in the examples described later.

[0229] It should be noted that the value of the fracture strength Y / yield strength X in the MD direction is not particularly limited. When uniform tensile strength along the MD direction is required, the value of the fracture strength Y / yield strength X in the MD direction is preferably 0.75 to 1.50, more preferably 0.80 to 1.50, even more preferably 0.85 to 1.50, and particularly preferably 0.90 to 1.50. There is a tendency that the larger this value, the higher the uniform tensile strength along the MD direction.

[0230] As an LCP extruded film for stretching, a melt-extruded film such as a T-die extrusion film is preferred. Furthermore, as an LCP extruded film for stretching, a thermoplastic liquid crystal polymer layer, specifically the middle layer (core layer), of a three-layer co-extruded film having a stacked structure of at least one thermoplastic resin layer, one thermoplastic liquid crystal polymer layer, and one thermoplastic resin layer arranged sequentially, is also preferred. In this case, by removing the two outer thermoplastic resin layers of the three-layer co-extruded film, it can be used as a single-layer thermoplastic liquid crystal polymer film (LCP extruded film for stretching). Compared to woven fabrics and nonwoven fabrics formed from thermoplastic liquid crystal polymer fibers, thermoplastic liquid crystal polymer extruded films can produce homogeneous films at low cost.

[0231] The thickness of the LCP extruded film for stretching can be appropriately set according to the required performance and is not particularly limited. Considering the operability and productivity during extrusion molding, it is preferably 15 μm to 300 μm, more preferably 18 μm to 250 μm, and even more preferably 20 μm to 200 μm.

[0232] On the other hand, in this embodiment, the molecular orientation of the thermoplastic liquid crystal polymer, expressed in terms of the coefficients of linear expansion in the MD and TD directions, is sufficiently reduced in the LCP extruded film used for stretching treatment. As mentioned above, the LCP extruded films described in prior art patent documents 1 and 2, by being protected by two outer thermoplastic resin layers during three-layer co-extrusion, mitigate the molecular orientation of the thermoplastic liquid crystal polymer to a certain extent, thereby mitigating the anisotropy of the strength in the MD and TD directions of the resulting thermoplastic liquid crystal polymer film. That being said, in reality, the coefficient of linear expansion in the MD direction of the LCP extruded films described in patent documents 1 and 2 can be stably obtained to around -20 ppm / K, while the coefficient of linear expansion in the TD direction exceeds 55 ppm, sometimes reaching around 100 ppm / K. From this, it is easy to understand that, as a whole, the LCP extruded films described in prior art patent documents 1 and 2 still retain a significant amount of the molecular orientation of the thermoplastic liquid crystal polymer, or a significant amount of internal strain, etc.

[0233] The LCP extruded film for stretching treatment in this embodiment preferably has a coefficient of linear expansion (CTE, α2, 23 to 200°C) in both the MD and TD directions within the range of -30 to 55 ppm / K. LCP extruded films for stretching treatment with a coefficient of linear expansion within this range exhibit reduced internal strain, resulting in less anisotropy in dimensional change rate compared to films that do not. Furthermore, LCP extruded films for stretching treatment can be obtained with sufficiently small absolute values ​​of dimensional change rate. From the viewpoint of improving adhesion to metal foils, the coefficient of linear expansion (CTE, α2, 23 to 200°C) in the MD direction of the LCP extruded film for stretching treatment is preferably in the range of -30 to 10 ppm / K, more preferably in the range of -25 to 5 ppm / K, and even more preferably in the range of -20 to 0 ppm / K. Furthermore, from the viewpoint of improving adhesion to metal foil, the coefficient of linear expansion (CTE, α2, 23–200°C) in the TD direction of the LCP extruded film for stretching is preferably in the range of 0–55 ppm / K, more preferably in the range of 5–55 ppm / K, and even more preferably in the range of 5–50 ppm / K. It should be noted that, in this specification, the coefficient of linear expansion (CTE, α2, 23–200°C) refers to the value measured using the TMA method according to JIS K7197 within the temperature range of 23–200°C. Other detailed measurement conditions are as described in the examples described later.

[0234] On the other hand, the dielectric properties of the LCP extruded film for stretching in this embodiment can be appropriately set according to the desired performance, and are not particularly limited. From the viewpoint of obtaining higher dielectric properties, the relative permittivity ε... r The dielectric constant ε (36GHz) is preferably 3.0 or higher and 3.7 or lower, more preferably 3.0 to 3.5. Similarly, the dielectric loss tangent tanδ (36GHz) is preferably 0.0010 or higher and 0.0050 or lower, more preferably 0.0010 or higher and 0.0045 or lower. It should be noted that in this specification, the relative permittivity ε... r The values ​​(36GHz) and dielectric loss tangent tanδ(36GHz) refer to the values ​​at 36GHz measured using the cavity resonator perturbation method according to JIS K6471. Other detailed measurement conditions are as described in the examples below.

[0235] (Method for manufacturing LCP extruded film for stretching)

[0236] The LCP extruded film for stretching treatment in this embodiment can be obtained by extruding a resin composition containing the above-mentioned thermoplastic liquid crystal polymer and optional components such as inorganic fillers and other resin components to a specified thickness. Various known methods can be used for extrusion, and there is no particular limitation on the type. Any combination of methods can be applied: for example, T-die extrusion, blow extrusion; for example, multi-manifold co-extrusion, feed block co-extrusion; for example, two-layer co-extrusion, three-layer co-extrusion, and other multi-layer co-extrusion methods.

[0237] From the viewpoint of ease of controlling the molecular orientation of the thermoplastic liquid crystal polymer on the film surface (film surface S1) and inside the film (film surface S2), a preferred method is to extrude the resin composition into a film using a T-die extrusion molding method (hereinafter sometimes simply referred to as "T-die extrusion"), and then perform cooling treatment, pressing treatment, pressure heating treatment, etc., as needed to obtain a specified LCP extruded film for stretching treatment. Specifically, the following co-extrusion method is preferred: a resin composition A containing a first surface layer of thermoplastic resin, a resin composition B containing a thermoplastic liquid crystal polymer for an intermediate layer, and a resin composition C containing a second surface layer of thermoplastic resin are prepared in advance, and they are co-extruded from a co-extrusion die of an extruder to extrude a co-extruded melt consisting of three layers, forming an LCP extruded film for stretching treatment in the form of an intermediate thermoplastic liquid crystal polymer layer. With such co-extrusion molding, the molecular orientation of the thermoplastic liquid crystal polymer in the intermediate thermoplastic liquid crystal polymer layer is mitigated by being protected by the two outer thermoplastic resin layers. Hereinafter, a preferred embodiment of the method for manufacturing the LCP extruded film for stretching treatment according to this embodiment will be described in detail.

[0238] Figures 17-19 This diagram illustrates a preferred embodiment of the method for manufacturing the LCP extruded film for stretching according to this embodiment. Here, the resin composition B described above, comprising the thermoplastic liquid crystal polymer and optional components such as inorganic fillers and other resin components, is melt-extruded from the T-die of an extruder in a film form. At this time, by co-extruding the resin compositions A and C containing the thermoplastic resin onto both sides of the film-shaped melt extrudate, a co-extruded melt (three-layer laminate) of a predetermined thickness is produced, comprising a first outer layer (release layer) of thermoplastic resin, an intermediate layer (LCP layer) containing the thermoplastic liquid crystal polymer, and a second outer layer (release layer) containing the thermoplastic resin. This co-extruded melt is picked up by a pick-up roller and fed to a cooling roller and a pressing roller. Then, the first and second outer layers are peeled off from the intermediate layer, and the thermoplastic resin layers of the two outer layers and the thermoplastic liquid crystal polymer layer of the intermediate layer (LCP extruded film for stretching) are respectively wound onto a winding roller.

[0239] The preparation of the resin composition B containing the thermoplastic liquid crystal polymer described above can be carried out using conventional methods without particular limitations. The components described above can be manufactured and processed using known methods such as mixing, melt mixing, granulation, extrusion molding, pressurization, or injection molding. It should be noted that during melt mixing, commonly used single-screw or twin-screw extruders, various kneaders, and other mixing devices can be used. When supplying the components to these melt mixing devices, the liquid crystal polymer, other resin components, inorganic fillers, additives, etc., can be pre-mixed using a mixing device such as a roller mixer or Henschel mixer. During melt mixing, the barrel temperature of the mixing device can be set appropriately without particular limitations; generally, a range of 360°C above the melting point of the liquid crystal polymer is preferred, and more preferably, a range of 10°C above the melting point of the liquid crystal polymer and 360°C below.

[0240] The preparation of resin compositions A and C containing thermoplastic resins can be carried out using conventional methods and is not particularly limited. Examples of thermoplastic resins include, but are not limited to, polyolefin resins such as polyethylene, polypropylene, polymethylpentene, and ethylene-α-olefin copolymers; acrylic resins such as PMMA; polyamide resins; acrylonitrile-butadiene-styrene copolymer (ABS resin); polystyrene (PS); polyvinyl chloride; polybutylene terephthalate (PBT); polyethylene terephthalate (PET); polycarbonate (PC); polyetheretherketone (PEEK); and polyphenylene sulfide (PPS). When formed into a co-extruded melt, both polar resins such as polycarbonate and non-polar resins such as polymethylpentene can effectively function as a release layer. Other optional components, such as resin components and inorganic fillers, that can be included in the aforementioned stretching-processed LCP extrusion film can be incorporated into these thermoplastic resins. It should be noted that resin composition A and resin composition C may have the same resin composition or different resin compositions; they may contain the same thermoplastic resin or different thermoplastic resins. Furthermore, resin compositions containing thermoplastic resins can be manufactured and processed using known methods such as mixing, melt mixing, granulation, extrusion molding, pressurization, or injection molding. It should be noted that during melt mixing, commonly used single-screw or twin-screw extruders, various kneaders, and other mixing devices can be used. When supplying the components to these melt mixing devices, the liquid crystal polymer, other resin components, inorganic fillers, additives, etc., can be pre-mixed using mixing devices such as rollers or Henschel mixers. During melt mixing, the barrel temperature of the mixing device can be appropriately set as long as it is below the temperature at which the thermoplastic resin does not undergo pyrolysis and deterioration; there is no particular limitation. Generally, it is preferable to be above the melting point of the thermoplastic resin, and more preferably above the melting point of the thermoplastic resin +10°C.

[0241] The settings for co-extrusion can be appropriately set according to the type and composition of the resin composition used, and the desired performance of the extruded film as the target, and are not particularly limited. For example, the set temperature of the extruder barrel can be appropriately set according to the type and composition of the resin composition used, and the desired performance of the extruded film as the target, and is not particularly limited, preferably 230 to 360°C, more preferably 280 to 350°C.

[0242] In addition, the width (mm) of the T-die can be appropriately set according to the type and composition of the resin composition used, the desired performance of the extruded film as the target, etc., and is not particularly limited. It is usually preferred to be 200 to 2000 mm, and more preferably 400 to 1500 mm.

[0243] Furthermore, the die lip opening (mm) of the T-die, for example, can also be appropriately set according to the type and composition of the resin composition used, the desired performance of the extruded film as the target, etc., without particular limitation. It is generally preferred to be 0.1 to 3.0 (mm), and more preferably 0.2 to 2.0 (mm).

[0244] Furthermore, for example, the shear rate (sec) of the lip wall of the T-mode -1 Similarly, the value can be appropriately set according to the type and composition of the resin composition used, the desired performance of the extruded film as the target, etc., and there is no particular limitation. Generally, 100 to 1500 (sec) is preferred. -1 ), more preferably 150 to 1000 (sec) -1 ).

[0245] In addition, the total amount of resin composition extruded from the T-mold (mm) 3 Similarly, the value ( / sec) can be appropriately set according to the type and composition of the resin composition used, the desired performance of the extruded film as the target, etc., and is not particularly limited, but is generally preferred to be 500 to 15000 (mm). 3 / sec), more preferably 1500~10000 (mm) 3 / sec).

[0246] On the other hand, the melt viscosity (Pa·sec) of the thermoplastic liquid crystal polymer can also be appropriately set according to the type and composition of the resin composition used, the desired performance of the target extruded film, etc., and is not particularly limited, but is generally preferred to be 10 to 300 (Pa·sec), and more preferably 20 to 250 (Pa·sec). It should be noted that the melt viscosity (Pa·sec) of the thermoplastic liquid crystal polymer refers to the value measured according to JIS K7199 using Capilograph 1D (manufactured by Toyo Seiki Co., Ltd.), under the conditions of a barrel length of 10.00 mm, a barrel diameter of 1.00 mm, and a barrel diameter of 9.55 mm, under the conditions of manufacturing an LCP extruded film for stretching treatment (die temperature and shear rate of the lip wall).

[0247] In addition, the pick-up speed (mm / sec) of the co-extruded film can also be set appropriately according to the type and composition of the resin composition used and the desired performance of the target extruded film. There is no particular limitation, but it is generally preferred to be 15 to 1000 (mm / sec), and more preferably 20 to 500 (mm / sec).

[0248] Here, from the perspective of reducing the molecular orientation of the thermoplastic liquid crystal polymer along the molecular direction (MD) during co-extrusion, a low shear stress (kPa) during co-extrusion is ideal. High shear stress during co-extrusion tends to result in high orientation of the thermoplastic liquid crystal polymer along the MD direction and residual internal strain. Conversely, low shear stress tends to reduce the molecular orientation of the thermoplastic liquid crystal polymer both on the film surface and inside the film, and reduces the likelihood of residual internal strain. It should be noted that the shear stress (kPa) during co-extrusion refers to the shear rate (sec) at the lip wall. -1 The shear rate is expressed as the product of the total amount of resin composition extruded during co-extrusion and the melt viscosity (Pa·sec) of the thermoplastic liquid crystal polymer. The shear rate is calculated based on the total amount of resin composition extruded, the die width, and the die lip opening during co-extrusion. Therefore, the shear stress during co-extrusion can be controlled by adjusting the above values. Specifically, the shear stress during co-extrusion is preferably 40 kPa or less, more preferably 38 kPa or less, and even more preferably 36 kPa or less. It should be noted that the lower limit is not particularly limited; considering productivity, it is preferably 5 kPa or more, and more preferably 10 kPa or more.

[0249] Furthermore, from the viewpoint of reducing the molecular orientation of the thermoplastic liquid crystal polymer along the molecular direction (MD) during co-extrusion, a low draw ratio during co-extrusion is ideal. A high draw ratio during co-extrusion tends to result in high orientation of the thermoplastic liquid crystal polymer along the MD direction and a tendency for internal strain to remain. Conversely, a low draw ratio during co-extrusion tends to reduce the molecular orientation of the thermoplastic liquid crystal polymer both on the film surface and inside the film, and a tendency for internal strain to remain. It should be noted that the draw ratio is a value expressed as pick-up speed (mm / sec) / thermoplastic liquid crystal polymer flow rate (mm / sec), where the flow rate is calculated based on the total output of the resin composition during co-extrusion, the die width, and the die lip opening. Therefore, the draw ratio during co-extrusion can be controlled by adjusting these values. Specifically, the draw ratio during co-extrusion is preferably 3.5 or less, more preferably 3.3 or less, and even more preferably 3.1 or less. It should be noted that there is no particular limitation on its lower limit value. If productivity and other factors are taken into account, it is preferable to be 1.0 or higher, and more preferably 1.2 or higher.

[0250] The thickness of the resulting LCP extruded film for stretching can be appropriately set according to the required performance and is not particularly limited. Considering the operability and productivity during extrusion molding, it is preferably 15 μm to 300 μm, more preferably 18 μm to 250 μm, and even more preferably 20 μm to 200 μm.

[0251] The melting point (melting temperature) of the resulting LCP extruded film for stretching is not particularly limited. However, from the viewpoint of heat resistance and processability, a melting point (melting temperature) of 200–400°C is preferred. Especially from the viewpoint of improving heat-pressing properties with metal foil, 250–360°C is preferred, more preferably 260–355°C, further preferably 270–350°C, and particularly preferably 275–345°C. It should be noted that, in this specification, the melting point of the LCP extruded film for stretching refers to the melting peak temperature obtained by differential scanning calorimetry (DSC) during the following process: heating the extruded film at a heating rate of 20°C / min (first heating) followed by cooling at a cooling rate of 50°C / min (first cooling) using a DSC8500 (PerkinElmer) in the temperature range of 30–400°C, and then heating it a second time at a heating rate of 20°C / min (second heating). In addition, regarding other matters, the measurement conditions are as described in the examples described later.

[0252] It should be noted that the LCP extruded film for stretching after extrusion molding can be used directly, or it can be further subjected to a pressure and heating process as needed to further reduce the molecularity (anisotropy) of the thermoplastic liquid crystal polymer or further release the internal strain. This can also result in a stretching LCP extruded film with further reduced anisotropy of dimensional change rate and a smaller absolute value of dimensional change rate.

[0253] The heating and pressurizing treatment can be performed using methods known in the art, such as contact heat treatment or non-contact heat treatment, and the type is not particularly limited. For example, known equipment such as non-contact heaters, ovens, blowing devices, hot rollers, cooling rollers, hot presses, and double-belt hot presses can be used for heat setting. At this time, if necessary, a release film or a porous film known in the art can be disposed on the surface of the LCP extruded film for stretching and heat-treated. In addition, when performing this heat treatment, from the viewpoint of controlling orientation, the following hot pressing method is preferred: a release film and a porous film are disposed on the surface and back of the LCP extruded film for stretching, hot-pressed together while being held between the annular belts of a double-belt press, and then the release film and the porous film are removed. The hot pressing method can be referred to, for example, Japanese Patent Application Laid-Open No. 2010-221694. As for the processing temperature during hot pressing of the LCP extruded film for stretching treatment using the above-described resin composition between the annular belt pairs of a dual-belt press, in order to control the crystallization state of the LCP extruded film for stretching treatment, it is preferable to perform the process at a temperature higher than the melting point of the liquid crystal polymer and lower than 70°C above the melting point, more preferably at a temperature higher than 5°C above the melting point and lower than 60°C above the melting point, and even more preferably at a temperature higher than 10°C above the melting point and lower than 50°C above the melting point. The hot pressing conditions at this time can be appropriately set according to the desired performance and are not particularly limited. It is preferable to perform the process under the conditions of a surface pressure of 0.5 to 10 MPa and a heating temperature of 250 to 430°C, more preferably under the conditions of a surface pressure of 0.6 to 8 MPa and a heating temperature of 260 to 400°C, and even more preferably under the conditions of a surface pressure of 0.7 to 6 MPa and a heating temperature of 270 to 370°C. On the other hand, when using non-contact heaters or ovens, it is preferable to carry out the process at 200–320°C for 1–20 hours.

[0254] (LCP stretch film)

[0255] The aforementioned LCP extruded film for stretching can be subjected to uniaxial and / or biaxial stretching processes and used in the form of an LCP stretch film 100 (a stretched body of an LCP extruded film for stretching). In this case, the LCP stretch film 100 can be either heat-shrinkable or heat-expandable in the TD direction, preferably heat-shrinkable in the TD direction. Furthermore, the LCP stretch film 100 can be either heat-shrinkable or heat-expandable in the MD direction, preferably heat-shrinkable in the MD direction. It should be noted that, in this specification, the term "heat-shrinkable LCP stretch film" refers to an LCP stretch film that is heat-shrinkable in both the TD and MD directions. The term "heat-shrinkable" is confirmed by the negative value of the linear expansion coefficient (ppm / K) described later.

[0256] The stretching conditions can be appropriately set according to the type and composition of the resin composition used, and the desired performance of the LCP stretched film 100 as the target, and are not particularly limited. In the case of uniaxial stretching, for example, it is preferable to stretch the LCP extruded film subjected to the above-described stretching treatment along the TD direction (transverse direction; short side direction) at 90–180°C by 1.3–2.5 times, followed by heat treatment (heat setting) at 100–240°C for 1–600 seconds. The stretching ratio along the TD direction is preferably 1.4–2.4 times, more preferably 1.5–2.3 times, and even more preferably 1.6–2.3 times. In the case of biaxial stretching, for example, the above-described stretching process can be performed by stretching the LCP extruded film at 70–180°C along the MD direction (Machine Direction, long side direction) by 1.3–2.5 times to form a uniaxially stretched film, followed by further stretching along the TD direction (Transverse Direction, short side direction) at 90–180°C by 1.1–2.5 times, and then heat-treating (heat setting) at 100–240°C for 1–600 seconds. Alternatively, biaxial stretching can be performed simultaneously instead of stepwise stretching. The stretching ratio is not particularly limited, but from the viewpoints of improving film transportability and demolding properties, suppressing thickness unevenness, and preventing wrinkles, the total stretching ratio in the MD direction × TD direction (where the stretching ratio in the MD direction is set as m and the stretching ratio in the TD direction is set as n, and m × n represents the stretching ratio) is preferably 1.3 times or more, more preferably 1.4 times or more, further preferably 1.5 times or more, and particularly preferably 1.6 times or more. It should be noted that there is no particular upper limit, but the target is less than 6.0 times, preferably less than 5.0 times, more preferably less than 4.0 times, and even more preferably less than 3.0 times. Furthermore, during heat setting, methods known in the art can be implemented, such as contact heat treatment, non-contact heat treatment, etc., and the type is not particularly limited. For example, known equipment such as non-contact heaters, ovens, blowing devices, hot rollers, cooling rollers, hot presses, and double-belt hot presses can be used for heat setting. At this time, if necessary, a release film or a porous film known in the art can be disposed on the surface of the LCP stretch film 100 and then subjected to hot pressing treatment.

[0257] The coefficients of linear expansion (CTE, α2, 23~200℃) in the MD and TD directions of the LCP stretch film 100 (stretched body of LCP extruded film for stretching treatment) can be appropriately set according to the desired performance, without particular limitation. From the viewpoint of reducing the anisotropy of the dimensional change rate and the absolute value of the dimensional change rate, and improving the adhesion with the metal foil, it is preferred that each is in the range of -20~0ppm / K, more preferably in the range of -15~0ppm / K, further preferably in the range of -13~0ppm / K, and particularly preferably in the range of -10~0ppm / K.

[0258] (Insulating material for circuit boards)

[0259] Figure 20 This is a schematic cross-sectional view showing the main parts of the circuit board insulating material 200 of this embodiment. The circuit board insulating material 200 of this embodiment comprises a laminate having at least one and / or two woven fabrics WF provided on one and / or both sides of the LCP stretch film 100 (stretch body of LCP extruded film for stretching treatment) described above.

[0260] Specifically, the insulating material 200 for the circuit board comprises a laminate having an LCP stretch film 100, a woven fabric WF, and an LCP stretch film 100 arranged at least sequentially (a three-layer structure). In this laminate, one LCP stretch film 100 is disposed on the surface side of the woven fabric WF, and another LCP stretch film 100 is disposed on the back side of the woven fabric WF. These three layers are heat-pressed together to form a three-layer laminate. It should be noted that a three-layer laminate is illustrated here, but the present invention can be implemented in the form of a two-layer laminate with one LCP stretch film 100 omitted, or in the form of a laminate with four or more layers obtained by further stacking LCP stretch films 100 and woven fabric WF, which is self-evident.

[0261] In this specification, the term "woven fabric WF disposed on one or both sides of LCP stretch film 100" means not only that the LCP stretch film 100 is directly placed on the surface of the woven fabric WF as in this embodiment, but also that any layer (e.g., base layer, adhesive layer, etc.) not shown is sandwiched between the LCP stretch film 100 and the woven fabric WF, or that the LCP stretch film 100 and the woven fabric WF are separately disposed.

[0262] Woven fabric (WF) is a fabric obtained by weaving fibers. There is no particular limitation on the type of fiber used in woven fabric (WF); any of inorganic fibers, organic fibers, or organic-inorganic hybrid fibers can be used. In particular, woven fabric (WF) made of inorganic fibers is preferred. By heat-pressing the inorganic fiber woven fabric (WF) to the LCP stretch film 100, the anisotropy of the dimensional change rate in the MD and TD directions can be kept small, thereby reducing the dimensional change rate itself in the MD and TD directions in a suitable manner. Commercially available woven fabric (WF) can be used; alternatively, it can be manufactured using methods known in the art.

[0263] Examples of inorganic fibers include, but are not specifically limited to, glass fibers such as E-glass, D-glass, L-glass, M-glass, S-glass, T-glass, Q-glass, UN-glass, NE-glass, and spherical glass, inorganic fibers other than glass such as quartz, and ceramic fibers such as silica. Regarding woven fabrics (WF) of inorganic fibers, fabrics that have undergone fiber-opening treatment and mesh-closing treatment are suitable from the viewpoint of dimensional stability. Of the above, glass cloth is preferred from the viewpoints of mechanical strength, dimensional stability, and water absorption. From the viewpoint of improving heat-pressing adhesion with the LCP stretch film 100, glass cloth that has undergone fiber-opening treatment and mesh-closing treatment is preferred. Additionally, glass cloth obtained through surface treatments based on silane coupling agents, such as epoxy silane treatment or amino silane treatment, can also be suitably used. It should be noted that one type of fiber can be used alone or in appropriate combinations of two or more types of fibers in the woven fabric (WF).

[0264] The thickness of the woven fabric (WF) can be appropriately set according to the required performance and is not particularly limited. From the viewpoints of lamination, processability, and mechanical strength, a thickness of 10–300 μm is preferred, more preferably 10–200 μm, and even more preferably 15–180 μm.

[0265] The total thickness of the insulating material 200 for the circuit board can be appropriately set according to the required performance and is not particularly limited. From the viewpoints of lamination, processability, and mechanical strength, it is preferably 30 to 500 μm, more preferably 50 to 400 μm, even more preferably 70 to 300 μm, and particularly preferably 90 to 250 μm.

[0266] The circuit board insulating material 200 of this embodiment, by adopting the above-described configuration, has the following significant effects: the anisotropy of the dimensional change rate in the MD and TD directions is small, thereby reducing the dimensional change rate in the MD and TD directions in a suitable manner; furthermore, it has excellent dielectric properties in the high-frequency region, is easy to manufacture, and has excellent productivity.

[0267] The aforementioned insulating material 200 for circuit boards can be manufactured using known methods, and the manufacturing method is not particularly limited. For example, an LCP stretch film 100 and a woven fabric WF can be laminated and heated and pressurized, and the LCP stretch film 100 and the woven fabric WF can be hot-pressed together to obtain the insulating material 200 for circuit boards. Alternatively, the following method is preferred: LCP stretch film 100, woven fabric WF, and LCP stretch film 100 are sequentially laminated to form a laminate, and the laminate is heated and pressurized while being held using a press, a double-belt press, etc., thereby hot-pressing the insulating material 200 for circuit boards. It should be noted that the processing temperature during hot pressing can be appropriately set according to the required performance and is not particularly limited; preferably 200–400°C, more preferably 250–360°C, and even more preferably 270–350°C. It should be noted that the processing temperature during hot pressing is a value measured from the surface temperature of the LCP stretch film 100 of the aforementioned laminate. In addition, the pressurization conditions at this time can be appropriately set according to the desired performance, without particular limitation. For example, the surface pressure is 0.5 to 10 MPa and the time is 1 to 240 minutes, and more preferably the surface pressure is 0.8 to 8 MPa and the time is 1 to 120 minutes.

[0268] (Metal foil laminate)

[0269] Figure 21 This is a schematic cross-sectional view showing the main parts of the metal-coated foil laminate 300 of this embodiment. The metal-coated foil laminate 300 of this embodiment includes the LCP stretch film 100 described above and a metal foil MF disposed on one side and / or both sides of the LCP stretch film 100.

[0270] Specifically, the metal foil laminate 300 is a double-sided metal foil laminate having a laminated structure (three-layer structure) in which metal foil MF, LCP stretch film 100, and metal foil MF are arranged at least sequentially. These three layers are heat-pressed together to form a three-layer laminate. It should be noted that this embodiment shows a double-sided metal foil laminate, but the invention can also be implemented with metal foil MF only on one surface of the LCP stretch film 100. That is, a three-layer laminate is illustrated here, but the invention can be implemented as a double-layer laminate omitting one metal foil MF, or as a laminate with four or more layers obtained by further laminating LCP stretch film 100 and woven fabric WF, which is self-evident.

[0271] Figure 22This is a schematic cross-sectional view showing the main parts of the metal-coated foil laminate 400 of this embodiment. The metal-coated foil laminate 400 of this embodiment includes at least the above-described LCP stretch film 100 and the above-described woven fabric WF disposed on one and / or both sides of the LCP stretch film 100, and metal foil MF disposed on one and / or both sides of the laminate.

[0272] Specifically, the metal foil laminate 400 is a double-sided metal foil laminate having a laminated structure (five-layer structure) in which metal foil MF, LCP stretch film 100, woven fabric WF, LCP stretch film 100, and metal foil MF are arranged at least sequentially. These five layers are heat-pressed together to form a five-layer laminate. It should be noted that this embodiment shows a double-sided metal foil laminate, but the present invention can also be implemented with metal foil MF on only one surface. That is, a five-layer laminate is illustrated here, but the present invention can be implemented as a four-layer laminate with one metal foil MF omitted, or as a laminated structure with six or more layers obtained by further laminating LCP stretch film 100, circuit board insulating material 200, and woven fabric WF, which is self-evident.

[0273] The material of the metal foil MF is not particularly limited, and examples include gold, silver, copper, copper alloys, nickel, nickel alloys, aluminum, aluminum alloys, iron, and iron alloys. Among these, copper foil, aluminum foil, stainless steel foil, and copper-aluminum alloy foil are preferred, and copper foil is more preferred. As the copper foil, any copper foil manufactured by rolling or electrolysis can be used, but electrolytic copper foil or rolled copper foil with a large surface roughness is preferred.

[0274] The thickness of the metal foil MF can be appropriately set according to the desired performance and is not particularly limited. It is typically preferred to be 1.5–1000 μm, more preferably 2–500 μm, further preferably 5–150 μm, and particularly preferably 7–100 μm. It should be noted that, as long as the effectiveness of the invention is not impaired, the metal foil MF can also undergo surface treatments such as acid cleaning or other chemical surface treatments. It should also be noted that the type and thickness of the metal foil MF can be the same or different.

[0275] The method for depositing metal foil MF on the surface of LCP stretch film 100 and circuit board insulating material 200 can be performed using conventional methods and is not particularly limited. Any method can be used, such as laminating metal foil MF on LCP stretch film 100 and circuit board insulating material 200 and bonding or pressing the two layers together, physical methods such as sputtering and vapor deposition (dry methods), chemical methods such as non-electroplating and electroplating after non-electroplating (wet methods), or coating with a metal paste. Alternatively, a multi-stage press, multi-stage vacuum press, continuous forming machine, or autoclave forming machine can be used to hot-press the laminate formed by laminating LCP stretch film 100, circuit board insulating material 200, and one or more metal foils MF, thereby obtaining metal foil-coated laminates 300 and 400.

[0276] The aforementioned metal foil laminates 300 and 400 can be manufactured using known methods, and the manufacturing method is not particularly limited. For example, one method could be as follows: an LCP stretch film 100, a circuit board insulating material 200, and a metal foil MF are laminated to form a laminate on which the metal foil MF is placed; this laminate is then hot-pressed while being held between the annular belts of a dual-belt press. As described above, the LCP stretch film 100 used in this embodiment exhibits low anisotropy in the MD and TD directions, and consequently, in a suitable manner, the dimensional change rates in the MD and TD directions are themselves small, thus achieving high peel strength with the metal foil MF.

[0277] The temperature during hot pressing of the metal foil MF can be appropriately set according to the required performance and is not particularly limited. Preferably, it is a temperature 50°C or more lower than the melting point of the liquid crystal polymer and 50°C or less higher than the melting point; more preferably, it is a temperature 40°C or more lower than the melting point of the liquid crystal polymer and 40°C or less higher than the melting point; even more preferably, it is a temperature 30°C or more lower than the melting point of the liquid crystal polymer and 30°C or less higher than the melting point; and particularly preferably, it is a temperature 20°C or more lower than the melting point of the liquid crystal polymer and 20°C or less higher than the melting point. It should be noted that the temperature during hot pressing of the metal foil MF is a value measured in the form of the surface temperature of the aforementioned LCP stretch film 100. In addition, the pressing conditions can be appropriately set according to the desired performance and are not particularly limited. For example, when using a dual-belt press, it is preferable to perform the pressing under the conditions of a surface pressure of 0.5 to 10 MPa and a heating temperature of 200 to 360°C.

[0278] The metal foil laminates 300 and 400 of this embodiment, as long as they are heat-pressed bodies with a double-layer structure of LCP stretch film 100 and metal foil MF, can also have other laminated structures or further laminated structures. For example, they can be made into: a two-layer structure of metal foil MF / LCP stretch film 100; a three-layer structure such as metal foil MF / LCP stretch film 100 / metal foil MF, LCP stretch film 100 / metal foil MF / LCP stretch film 100; a four-layer structure such as metal foil MF / LCP stretch film 100 / woven fabric WF / LCP stretch film 100; a five-layer structure such as metal foil MF / LCP stretch film 100 / metal foil MF / LCP stretch film 100 / metal foil MF, metal foil MF / LCP stretch film 100 / woven fabric WF / LCP stretch film 100 / metal foil MF; and so on, multi-layer structures. In addition, multiple (e.g., 2 to 50) metal foil laminates 300 and 400 can be laminated and heat-pressed together.

[0279] In the metal foil laminates 300 and 400 of this embodiment, the peel strength between the LCP stretch film 100 and the metal foil MF is not particularly limited. However, from the viewpoint of achieving higher peel strength, it is preferably 0.8 (N / mm) or more, more preferably 1.0 (N / mm) or more, and even more preferably 1.2 (N / mm) or more. As described above, the metal foil laminates 300 and 400 of this embodiment can achieve high peel strength, thus, for example, peeling between the LCP stretch film 100 and the metal foil MF can be suppressed during the heating process of substrate manufacturing. Furthermore, when obtaining peel strength equivalent to that of the prior art, manufacturing conditions with excellent process margin and productivity can be applied. Therefore, the degradation of the basic properties of the liquid crystal polymer can be suppressed while maintaining the same level of peel strength as before.

[0280] Furthermore, for the metal foil laminates 300 and 400 of this embodiment, at least a portion of the metal foil MF can be patterned or etched, thereby making it suitable as a raw material for circuit boards such as electronic circuit boards and multilayer boards. In addition, the metal foil laminates 300 and 400 of this embodiment have excellent dielectric properties in the high-frequency region, small anisotropy in the dimensional change rate in the MD and TD directions, and thus, in a suitable manner, the dimensional change rate in the MD and TD directions is small, resulting in excellent dimensional stability, ease of manufacturing, and high productivity. Therefore, they are particularly useful raw materials as insulating materials for flexible printed circuit boards (FPCs) in fifth-generation mobile communication systems (5G), millimeter-wave radar, etc.

[0281] Example

[0282] The following examples and comparative examples illustrate the features of the present invention in more detail, but the present invention is not limited thereto. That is, the materials, amounts, proportions, processing contents, processing steps, etc., shown in the following examples can be appropriately modified as long as they do not depart from the spirit of the present invention. In addition, the various manufacturing conditions and evaluation results values ​​in the following examples have the meaning of preferred upper or lower limits in the embodiments of the present invention, and the preferred numerical range can also be a range defined by the aforementioned upper or lower limits, the values ​​of the following examples, or the values ​​of the examples themselves.

[0283] [Melt viscosity]

[0284] The melt viscosity [Pa·sec] of each LCP extruded film was measured under the following conditions.

[0285] Measurement equipment: Capilograph 1D (manufactured by Toyo Seiki Co., Ltd.)

[0286] Applicable device: Barrel length 10.00mm, barrel diameter 1.00mm, barrel body diameter 9.55mm

[0287] Measurement conditions: Temperature [°C] and shear rate [sec] during extrusion molding of each LCP extruded film. -1 ]

[0288] [Orientation Degree]

[0289] X-ray diffraction measurements of each LCP extruded film, including film surface S1 or film surface S2, were performed using the Smartlab X-ray diffraction apparatus (manufactured by Rigaku Corporation) via transmission method, and the orientation degree was determined. Here, a Cu-sealed tube was used as the X-ray source, and X-ray diffraction measurements were performed using a parallel beam optical system and transmission method (2θ / θ scan, β scan). First, the 2θ / θ scan confirmed a peak at 2θ = 19.5°. Next, the intensity of the diffraction peak at 2θ = 19.5° was measured from 0° to 360° in the azimuth direction using the β scan, thereby obtaining the intensity distribution in the azimuth direction. The orientation degree was calculated using the above formula based on the baseline intensity (isotropic component) and peak intensity (orientation component) of the obtained β profile, according to the area ratio of the orientation peak.

[0290] It should be noted that the membrane surface S2 of each LCP extruded membrane was adjusted in the following manner: each LCP extruded membrane was immersed in a 70% aqueous solution of monoethylamine (made by Daicel) at 23°C and 50% RH for 168 hours, and both surfaces of each LCP extruded membrane were etched with 5μm. Then, it was washed with running water for 5 minutes, further cleaned with distilled water, dried at 80°C for 1 hour, and cooled at 23°C and 50% RH for 24 hours.

[0291] [Hardness Measurement Based on Nanoindentation]

[0292] The hardness H1 at a depth of 1 μm and the hardness H2 at the center of the thickness of each LCP extruded film were measured using the nanoindentation method according to ISO 14577.

[0293] Measurement equipment: Hysitron TI 950 Tribo Indenter (manufactured by Bruker)

[0294] Indenter used: Diamond Berkovich type indenter

[0295] Measurement conditions: Indentation depth hmax 0.05 μm

[0296] Test method: Load-unload test

[0297] It should be noted that, for the measurement surface of each LCP extruded membrane, a smooth membrane cross section parallel to the MD direction of each LCP extruded membrane is set. This smooth membrane cross section is made by cutting each LCP extruded membrane under freezing conditions using ion beam processing.

[0298] [Coefficient of linear expansion]

[0299] The coefficient of linear expansion of each LCP extruded film and LCP stretched film was determined using the TMA method according to JIS K7197.

[0300] Measurement equipment: TMA 4000SE (manufactured by NETZSCH)

[0301] Measurement method: tensile mode

[0302] Measurement conditions: Sample size 25mm × 4mm × thickness 50μm

[0303] 20mm chuck spacing

[0304] Temperature range 23–200℃ (2nd run) Heating rate 5℃ / min

[0305] Atmospheric nitrogen (flow rate 50 ml / min)

[0306] Test load 5gf

[0307] * To observe the values ​​after eliminating the thermal history, the values ​​from 2ndRUN were used.

[0308] [Tape peel test]

[0309] For each LCP extruded membrane, a tightness test was performed on the membrane surface S1 using the cross-section method according to JIS K5600-5-6 to confirm the presence or absence of a skin layer. At this time, a Cellotape (registered trademark) manufactured by NICHIBAN (24mm wide × 50mm long) was used. Cases where no mesh was peeled off after the tape was removed were recorded as "no skin layer", and cases where the mesh was peeled off were recorded as "skin layer present".

[0310] ○ No dermis

[0311] × has a dermis

[0312] [Dimensional change rate and anisotropy of metal foil after etching]

[0313] Electrolytic copper foil (Mitsui Metals Corporation TQ-M7VSP) with a thickness of 12 μm was laminated on both sides of each LCP extruded film. The laminations were hot-pressed for 1 minute at 320°C and a surface pressure of 1 MPa to create double-sided metal-coated laminates consisting of copper foil / LCP extruded film / copper foil. Following JPCA-UB01 (2017), and according to its "16.4.4-18 Dimensional Change Rate" and "16.4.4-2-2 Sample Preparation Based on Copper Foil Removal" standards, samples were prepared from the obtained double-sided metal-coated laminates. The dimensional change rate of each sample after copper foil etching was measured using a measuring microscope (Mitutoyo Corporation MF-A4020C), and the anisotropy of the dimensional change rate was evaluated. Here, β1 represents the dimensional change rate in the MD direction, and β2 represents the dimensional change rate in the TD direction.

[0314] ◎The anisotropy of the rate of dimensional change is very small (|β2-β1|≤0.3%).

[0315] The anisotropy of the rate of dimensional change is small (0.3% < |β2-β1| < 0.4%).

[0316] × The anisotropy of the rate of dimensional change is large (0.4% ≤ |β2-β1|).

[0317] (Examples 1A-3A)

[0318] Specifically, a type II thermoplastic liquid crystal polymer (a copolymer of 74 mol% p-hydroxybenzoic acid and 26 mol% 6-hydroxy-2-naphthoic acid monomers) was used at a temperature of 300°C and a shear rate of 500 sec. -1with a melt viscosity of 80 Pa·sec) was used as the intermediate layer, polycarbonate PC (Panlite L-1225L manufactured by Teijin Limited) was used as the surface layers on both sides of the intermediate layer, under the molding conditions shown in Table 1, each resin was co-extruded at 300°C by a T-die casting method using a two-type three-layer extruder equipped with a T-die having a die width of 600 mm and a die lip opening of 0.2 to 1.0 mm, to mold a two-type three-layer film with an intermediate layer of 50 μm. The polycarbonate films of the two surface layers were respectively peeled off from the molded two-type three-layer film using a winding line, to obtain LCP extruded films of Examples 1A to 3A each having a melting point of 280°C and a thickness of 50 μm.

[0319] In addition, in a state where a glass cloth (IPC No. #1037) was sandwiched between the obtained pair of thermoplastic liquid crystal polymer films of Examples 1A to 3A, thermocompression bonding treatment was performed at 300°C for 5 minutes using a hot press, to obtain an insulating material for circuit boards of Examples 1A to 3A each having a melting point of 280°C and a total thickness of 100 μm.

[0320] (Comparative Example 1A)

[0321] A type II thermoplastic liquid crystal polymer (a copolymer having a monomer composition of 74 mol% p-hydroxybenzoic acid and 26 mol% 6-hydroxy-2-naphthoic acid, at a temperature of 300°C and a shear rate of 500 sec -1 with a melt viscosity of 80 Pa·sec) was extruded under the molding conditions shown in Table 1 at 300°C by a T-die casting method using a single-layer extruder equipped with a T-die having a die width of 600 mm and a die lip opening of 0.3 mm, to obtain an LCP extruded film of Comparative Example 1A having a melting point of 280°C and a thickness of 50 μm.

[0322] (Comparative Examples 2A to 4A)

[0323] Except that the molding conditions were changed to those described in Table 1, LCP extruded films of Comparative Examples 2A to 4A each having a melting point of 280°C and a thickness of 50 μm were respectively obtained in the same manner as in Example 1A.

[0324] [Table 1]

[0325]

[0326] (Examples 4A to 6A)

[0327] As the intermediate layer, a type I thermoplastic liquid crystal polymer (a copolymer having a monomer composition of 79 mol% p-hydroxybenzoic acid, 20 mol% 6-hydroxy-2-naphthoic acid, and 1 mol% terephthalic acid, at a temperature of 330°C and a shear rate of 500 sec -1The type II thermoplastic liquid crystal polymer was replaced with a melt viscosity of 70 Pa·sec. Each resin was co-extruded at 330°C. Otherwise, the LCP extruded films of Examples 4A to 6A with a melting point of 315°C and a thickness of 50 μm were obtained by the same method as in Example 1A.

[0328] In addition, with a glass cloth (IPC No. #1037) sandwiched between a pair of thermoplastic liquid crystal polymer films of Examples 4A to 6A, a hot pressing process was performed at 330°C for 5 minutes to obtain the circuit board insulating materials of Examples 4A to 6A with a melting point of 315°C and a total thickness of 100 μm.

[0329] (Comparative Example 5A)

[0330] A type I thermoplastic liquid crystal polymer (a copolymer of monomers consisting of 79 mol% p-hydroxybenzoic acid, 20 mol% 6-hydroxy-2-naphthoic acid, and 1 mol% terephthalic acid) was used at a temperature of 330°C and a shear rate of 500 sec. -1 The melt viscosity of the liquid crystal polymer (70 Pa·sec) was used instead of the type II thermoplastic liquid crystal polymer. The liquid crystal polymer was extruded at 330°C. Otherwise, the LCP extruded film of Comparative Example 5A with a melting point of 315°C and a thickness of 50 μm was obtained by the same method as Comparative Example 1A.

[0331] (Comparative Examples 6A-8A)

[0332] Except for changing the molding conditions to those described in Table 2, LCP extruded films of Comparative Examples 6A to 8A with a melting point of 315°C and a thickness of 50 μm were obtained by the same method as in Example 4A.

[0333] [Table 2]

[0334]

[0335] (Examples 7A-9A)

[0336] The surface layers on both sides were replaced with polymethylpentene PMP (TPXMX004 manufactured by Mitsui Chemicals Co., Ltd.). Otherwise, the LCP extruded films of Examples 7A to 9A with a melting point of 280°C and a thickness of 50 μm were obtained by the same method as in Example 1A.

[0337] In addition, with a glass cloth (IPC No. #1037) sandwiched between a pair of thermoplastic liquid crystal polymer films of Examples 7A to 9A, a hot pressing process was performed at 300°C for 5 minutes to obtain the circuit board insulating materials of Examples 7A to 9A with a melting point of 280°C and a total thickness of 100μm.

[0338] (Comparative Examples 9A-11A)

[0339] Except for changing the molding conditions as described in Table 3, LCP extruded films of Comparative Examples 9A to 11A with a melting point of 280°C and a thickness of 50 μm were obtained by the same method as in Example 7A.

[0340] [Table 3]

[0341]

[0342] The measurement results are shown in Tables 4-6.

[0343] [Table 4]

[0344]

[0345] [Table 5]

[0346]

[0347] [Table 6]

[0348]

[0349] In addition, the relationship between film-forming conditions, orientation degree, and coefficient of linear expansion in the manufacturing method of LCP extruded film is summarized in Tables 7-9.

[0350] [Table 7]

[0351]

[0352] [Table 8]

[0353]

[0354] [Table 9]

[0355]

[0356] The LCP extruded films of Examples 1A, 4A, and 7A were stretched 1.5 times (total stretch ratio: 1.5 times) along the TD direction at 130°C using a uniaxial stretching machine, and then heat-set at 130°C for 2 minutes to obtain LCP stretched films respectively.

[0357] The measurement results are shown in Table 10.

[0358] [Table 10]

[0359]

[0360] The LCP extruded films of Examples 1A, 4A, and 7A were stretched 2.0 times (total stretching ratio: 2.0 times) along the TD direction at 130°C using a uniaxial stretching machine, and then heat-set at 130°C for 2 minutes to obtain LCP stretched films.

[0361] The measurement results are shown in Table 11.

[0362] [Table 11]

[0363]

[0364] (Examples 1B-3B)

[0365] Specifically, a type II thermoplastic liquid crystal polymer (a copolymer of 74 mol% p-hydroxybenzoic acid and 26 mol% 6-hydroxy-2-naphthoic acid monomers) was used at a temperature of 300°C and a shear rate of 500 sec. -1 Using a resin with a melt viscosity of 80 Pa·sec as the intermediate layer, and polycarbonate PC (Panlite L-1225L manufactured by Teijin Corporation) as the surface layers on both sides of the intermediate layer, under the molding conditions shown in Table 12, each resin was co-extruded at 300°C using a T-die casting method from two three-layer extruders equipped with a T-die width of 600 mm and a die lip opening of 0.2 to 1.0 mm, forming two three-layer films with an intermediate layer of 50 μm. The two surface polycarbonate films were then peeled off from the formed three-layer films using a winding line to obtain LCP extruded films of Examples 1B to 3B, each with a melting point of 280°C and a thickness of 50 μm.

[0366] In addition, with a glass cloth (IPC No. #1037) sandwiched between a pair of thermoplastic liquid crystal polymer films of Examples 1B to 3B, a hot pressing process was performed at 300°C for 5 minutes to obtain the circuit board insulating materials of Examples 1B to 3B with a melting point of 280°C and a total thickness of 100μm.

[0367] (Comparative Example 1B)

[0368] The method used was a type II thermoplastic liquid crystal polymer (a copolymer of 74 mol% p-hydroxybenzoic acid and 26 mol% 6-hydroxy-2-naphthoic acid), at a temperature of 300°C and a shear rate of 500 sec. -1 The melt viscosity was 80 Pa·sec. Under the molding conditions shown in Table 12, the liquid crystal polymer was extruded at 300°C from a single-layer extruder with a T-die having a die width of 600 mm and a die lip opening of 0.3 mm using a T-die casting method to obtain the LCP extruded film of Comparative Example 1B with a melting point of 280°C and a thickness of 50 μm.

[0369] (Comparative Examples 2B-4B)

[0370] Except for changing the molding conditions to those described in Table 12, LCP extruded films of Comparative Examples 2B to 4B with a melting point of 280°C and a thickness of 50 μm were obtained by the same method as in Example 1B.

[0371] [Table 12]

[0372]

[0373] (Examples 4B-6B)

[0374] The intermediate layer uses a type I thermoplastic liquid crystal polymer (a copolymer of 79 mol% p-hydroxybenzoic acid, 20 mol% 6-hydroxy-2-naphthoic acid, and 1 mol% terephthalic acid, at a temperature of 330°C and a shear rate of 500 sec). -1 The type II thermoplastic liquid crystal polymer was replaced with a melt viscosity of 70 Pa·sec. Each resin was co-extruded at 330°C. Otherwise, the LCP extruded films of Examples 4B to 6B with a melting point of 315°C and a thickness of 50 μm were obtained by the same method as in Example 1B.

[0375] In addition, with a glass cloth (IPC No. #1037) sandwiched between a pair of thermoplastic liquid crystal polymer films of Examples 4B to 6B, a hot pressing process was performed at 330°C for 5 minutes to obtain the circuit board insulating materials of Examples 4B to 6B with a melting point of 315°C and a total thickness of 100μm.

[0376] (Comparative Example 5B)

[0377] A type I thermoplastic liquid crystal polymer (a copolymer of monomers consisting of 79 mol% p-hydroxybenzoic acid, 20 mol% 6-hydroxy-2-naphthoic acid, and 1 mol% terephthalic acid) was used at a temperature of 330°C and a shear rate of 500 sec. -1 The melt viscosity of the liquid crystal polymer (70 Pa·sec) was used instead of the type II thermoplastic liquid crystal polymer. The liquid crystal polymer was extruded at 330°C. Otherwise, the LCP extruded film of Comparative Example 5B with a melting point of 315°C and a thickness of 50 μm was obtained by the same method as Comparative Example 1B.

[0378] (Comparative Examples 6B-8B)

[0379] Except for changing the molding conditions to those described in Table 13, LCP extruded films of Comparative Examples 6B to 8B with a melting point of 315°C and a thickness of 50 μm were obtained by the same method as in Example 4B.

[0380] [Table 13]

[0381]

[0382] (Examples 7B-9B)

[0383] The surface layers on both sides were replaced with polymethylpentene PMP (TPXMX004 manufactured by Mitsui Chemicals Co., Ltd.). Otherwise, the LCP extruded films of Examples 7B to 9B with a melting point of 280°C and a thickness of 50 μm were obtained by the same method as in Example 1B.

[0384] In addition, with a glass cloth (IPC No. #1037) sandwiched between a pair of thermoplastic liquid crystal polymer films of Examples 7B to 9B, a hot pressing process was performed at 300°C for 5 minutes to obtain the circuit board insulating materials of Examples 7B to 9B with a melting point of 280°C and a total thickness of 100μm.

[0385] (Comparative Examples 9B-11B)

[0386] Except for changing the molding conditions to those described in Table 14, LCP extruded films of Comparative Examples 9B to 11B with a melting point of 280°C and a thickness of 50 μm were obtained by the same method as in Example 7B.

[0387] [Table 14]

[0388]

[0389] The measurement results are shown in Tables 15-17.

[0390] [Table 15]

[0391]

[0392] [Table 16]

[0393]

[0394] [Table 17]

[0395]

[0396] In addition, the relationship between film-forming conditions, hardness, and coefficient of linear expansion in the manufacturing method of LCP extruded film is summarized in Tables 18-20.

[0397] [Table 18]

[0398]

[0399] [Table 19]

[0400]

[0401] [Table 20]

[0402]

[0403] The measurement results are shown in Table 21.

[0404] [Table 21]

[0405]

[0406] The LCP extruded films of Examples 1B, 4B, and 7B were stretched 1.5 times (total stretch ratio: 1.5 times) along the TD direction at 130°C using a uniaxial stretching machine, and then heat-set at 130°C for 2 minutes to obtain LCP stretched films.

[0407] The measurement results are shown in Table 22.

[0408] [Table 22]

[0409]

[0410] The LCP extruded films of Examples 1B, 4B, and 7B were stretched 2.0 times (total stretch ratio: 2.0 times) along the TD direction at 130°C using a uniaxial stretching machine, and then heat-set at 130°C for 2 minutes to obtain LCP stretched films.

[0411] The measurement results are shown in Table 23.

[0412] [Table 23]

[0413]

[0414] [Melt viscosity]

[0415] The melt viscosity [Pa·sec] of LCP extruded films for each stretching treatment was measured under the following conditions.

[0416] Measurement equipment: Capilograph 1D (manufactured by Toyo Seiki Co., Ltd.)

[0417] Applicable device: Barrel length 10.00mm, barrel diameter 1.00mm, barrel body diameter 9.55mm

[0418] Measurement conditions: Temperature [°C] and shear rate [sec] during extrusion molding of LCP extruded film for stretching treatment. -1 ]

[0419] [Yield strength X and fracture strength Y]

[0420] Tensile tests were conducted on LCP extruded films for various tensile treatments under the following conditions to determine the yield strength X and the breaking strength Y.

[0421] According to JIS K7161-1:2014

[0422] Tensile testing machine: Strograph VE1D (manufactured by Toyo Seiki Co., Ltd.)

[0423] Sample size: dumbbell shape

[0424] Conditioning before the experiment: 23℃, 50%RH, 24 hours

[0425] Measurement temperature: 200℃

[0426] Stretching speed: 200mm / min

[0427] Distance between markings: 50mm

[0428] Measurement results: the average of 5 measurements

[0429] [Coefficient of linear expansion]

[0430] The coefficients of linear expansion of each stretching-treated LCP extruded film and each LCP stretching film were determined using the TMA method according to JIS K7197.

[0431] Measurement equipment: TMA 4000SE (manufactured by NETZSCH)

[0432] Measurement method: tensile mode

[0433] Measurement conditions: Sample size 25mm × 4mm × thickness 50μm

[0434] 20mm chuck spacing

[0435] Temperature range: 23–200℃ (2nd RUN)

[0436] Heating rate 5℃ / min

[0437] Atmospheric nitrogen (flow rate 50 ml / min)

[0438] Test load 5gf

[0439] * To observe the values ​​after eliminating the thermal history, the values ​​from 2ndRUN were used.

[0440] [Tape peel test]

[0441] For each stretching treatment of LCP extruded film, an adhesion test was performed on the film surface using the cross-section method according to JISK 5600-5-6 to confirm the presence or absence of a skin layer. At this time, a Cellotape (registered trademark) manufactured by NICHIBAN (24mm wide × 50mm long) was used. Cases where no mesh was peeled off after the tape was removed were recorded as "no skin layer", and cases where the mesh was peeled off were recorded as "skin layer present".

[0442] ○ No dermis

[0443] × has a dermis

[0444] (Examples 1C-3C)

[0445] Specifically, a type I thermoplastic liquid crystal polymer (a copolymer of monomers consisting of 79 mol% p-hydroxybenzoic acid, 20 mol% 6-hydroxy-2-naphthoic acid, and 1 mol% terephthalic acid) was used at a temperature of 330°C and a shear rate of 500 sec. -1 Using a resin with a melt viscosity of 70 Pa·sec as the intermediate layer, and polycarbonate PC (Panlite L-1225L manufactured by Teijin Corporation) as the surface layers on both sides of the intermediate layer, under a shear stress of 40 kPa and a draw ratio of 2.0, the resins were co-extruded at 330°C using a T-die casting method from two three-layer extruders equipped with a T-die width of 600 mm and a die lip opening of 0.2 to 1.0 mm, to form two three-layer films with intermediate layers having the thicknesses listed in Table 24. The two surface polycarbonate films were peeled off from the formed three-layer films using a winding line to obtain the LCP extruded films for stretching treatment in Examples 1C to 3C, each with a melting point of 315°C.

[0446] The LCP extruded films of Examples 1C to 3C were stretched 2.0 times (total stretch ratio: 2.0 times) along the TD direction at 130°C using a uniaxial stretching machine, and then heat-set at 130°C for 30 seconds to obtain LCP stretched films of Examples 1C to 3C. Then, with each pair of LCP stretched films of Examples 1C to 3C sandwiched between glass cloth (IPC No. #1037), they were heat-pressed at 300°C for 5 minutes using a hot press to obtain insulating materials for circuit boards of Examples 1C to 3C.

[0447] (Comparative Example 1C)

[0448] Under conditions of shear stress of 50 kPa and draw ratio of 6.0, liquid crystal polymer was extruded at 330°C from a single-layer extruder with a T-die having a die width of 600 mm and a die lip opening of 0.2 to 1.0 mm using a T-die casting method. Otherwise, the process was carried out in the same manner as in Example 1C to obtain the stretch-treated LCP extruded film of Comparative Example 1C with a melting point of 315°C.

[0449] Using the LCP extruded film for stretching obtained in Comparative Example 1C, except that the process was the same as in Example 1C, an attempt was made to obtain an LCP stretched film, but uniform stretching was not achieved.

[0450] The results are shown in Table 24.

[0451] [Table 24]

[0452]

[0453] (Examples 4C-6C)

[0454] Specifically, a type II thermoplastic liquid crystal polymer (a copolymer of 74 mol% p-hydroxybenzoic acid and 26 mol% 6-hydroxy-2-naphthoic acid monomers) was used at a temperature of 300°C and a shear rate of 500 sec. -1 Using a resin with a melt viscosity of 80 Pa·sec as the intermediate layer, and polycarbonate PC (Panlite L-1225L manufactured by Teijin Corporation) as the surface layers on both sides of the intermediate layer, under a shear stress of 40 kPa and a draw ratio of 2.0, the resins were co-extruded at 300°C using a T-die casting method from two three-layer extruders equipped with a T-die width of 600 mm and a die lip opening of 0.2 to 1.0 mm, to form two three-layer films with intermediate layers having the thicknesses described in Table 25. The two surface polycarbonate films were peeled off from the formed three-layer films using a winding line to obtain the LCP extruded films for stretching treatment in Examples 4C to 6C, each with a melting point of 280°C.

[0455] The LCP extruded films of Examples 4C to 6C were stretched 2.0 times (total stretch ratio: 2.0 times) along the TD direction at 130°C using a uniaxial stretching machine, and then heat-set at 130°C for 30 seconds to obtain LCP stretched films of Examples 4C to 6C. Then, with a pair of LCP stretched films of Examples 4C to 6C each sandwiched between glass cloth (IPC No. #1037), they were hot-pressed at 300°C for 5 minutes to obtain insulating materials for circuit boards of Examples 4C to 6C.

[0456] (Comparative Example 2C)

[0457] Under conditions of shear stress of 60 kPa and draw ratio of 6.0, liquid crystal polymer was extruded at 300°C from a single-layer extruder with a T-die having a die width of 600 mm and a die lip opening of 0.2 to 1.0 mm using a T-die casting method. Otherwise, the process was carried out in the same manner as in Example 4C to obtain the stretch-treated LCP extruded film of Comparative Example 2C with a melting point of 280°C.

[0458] Using the LCP extruded film for stretching obtained in Comparative Example 2C, except that the process was the same as in Example 4C, an attempt was made to obtain an LCP stretched film, but uniform stretching was not achieved.

[0459] The results are shown in Table 25.

[0460] [Table 25]

[0461]

[0462] Industrial availability

[0463] The LCP extruded film of the present invention can be widely and effectively used in electronic circuit boards, multilayer boards, high heat dissipation boards, flexible printed wiring boards, antenna boards, optoelectronic hybrid boards, IC packaging and other applications. In particular, due to its suitability for ultra-fine processing and high reliability, it can be widely and effectively used as an insulating material for flexible printed wiring boards (FPCs) in fifth-generation mobile communication systems (5G), millimeter-wave radar and other applications, as well as for metal foil laminates.

[0464] Explanation of reference numerals in the attached figures

[0465] 100 LCP extruded film

[0466] 100a noodles

[0467] 100b side

[0468] S1 membrane surface

[0469] S2 membrane surface with a depth of 5 μm

[0470] Hardness at a depth of 1μm (H1)

[0471] Hardness at the center point of H2 thickness

[0472] 200 Insulating material for circuit boards

[0473] 300 Foil-Clad Laminate

[0474] 400 Foil-coated laminate

[0475] WF woven fabric

[0476] MF metal foil

[0477] X Yield point strength

[0478] Y fracture point strength

[0479] 100 LCP stretch film

[0480] 200 Insulating material for circuit boards

[0481] 300 Foil-Clad Laminate

[0482] 400 Foil-coated laminate

[0483] WF woven fabric

[0484] MF metal foil

Claims

1. A stretchable LCP extruded film, comprising a thermoplastic liquid crystal polymer, wherein the yield strength X and fracture strength Y of the stretchable LCP extruded film in the TD direction satisfy the following formula (I) in the stress-strain curve determined by a constant temperature bath tensile test. 0.75≤fracture point strength Y / yield point strength X≤1.50 (I), The constant temperature bath tensile test was conducted according to JIS K7161-1:2014, at 200℃ and a tensile speed of 200 mm / min. The yield strength X in the TD direction is in MPa, and the fracture strength Y is in MPa. The linear expansion coefficient in the MD direction of the LCP extruded film used for stretching treatment is -30 to 10 ppm / K.

2. The LCP extruded film for stretching treatment as described in claim 1, wherein, The linear expansion coefficient in the TD direction of the LCP extruded film used for stretching treatment is 5 to 55 ppm / K.

3. The LCP extruded film for stretching treatment as described in claim 1 or 2, wherein, The LCP extrusion film used for the stretching process is a T-die extrusion film.

4. The LCP extruded film for stretching as described in claim 1 or 2, wherein, The LCP extruded film for stretching is the intermediate layer obtained by removing the two outer layers from a laminated extruded film having an outer layer, an intermediate layer, and an outer layer.

5. The LCP extruded film for stretching treatment as described in claim 1 or 2, wherein, The LCP extruded film used for stretching treatment does not have a skin layer on its surface that would cause tape peeling during a tightness test using the cross-cutting method according to JIS K5600-5-6.

6. The LCP extruded film for stretching as described in claim 1 or 2, wherein, The LCP extruded film for stretching has a thickness of 15 μm to 300 μm.

7. The LCP extruded film for stretching as described in claim 1 or 2, wherein, The LCP extruded film used for stretching also contains inorganic fillers.

8. A heat-shrinkable LCP stretch film comprising a stretch body of an LCP extruded film for stretching treatment according to any one of claims 1 to 7, wherein the coefficient of linear expansion in the TD direction of the stretch body is in the range of -20 ppm / K or more and less than 0 ppm / K, and the coefficient of linear expansion in the MD direction of the stretch body is in the range of -20 ppm / K or more and less than 0 ppm / K.

9. The heat-shrinkable LCP stretch film as described in claim 8, wherein, The stretched body has a stretch ratio of 1.3 to 2.5 times relative to the LCP extruded film for stretching treatment in the TD direction.

10. An insulating material for a circuit board, comprising a laminate having at least the heat-shrinkable LCP stretch film as described in claim 8 or 9 and a woven fabric disposed on at least one side of the heat-shrinkable LCP stretch film.

11. A metal foil laminate comprising the heat-shrinkable LCP stretch film as described in claim 8 or 9, and metal foil disposed on one and / or both sides of the heat-shrinkable LCP stretch film.

12. A metal foil laminate comprising at least a laminate of a heat-shrinkable LCP stretch film and a woven fabric as described in claim 8 or 9, and metal foil disposed on one and / or both sides of the laminate.

Citation Information

Patent Citations

  • Manufacture of liquid crystal film

    JP1988031729A

  • Liquid crystalline polymer film and manufacture thereof

    JP1990178016A

  • Method for manufacturing laminate for flexible printed wiring board, laminate for flexible printed wiring board and flexible printed wiring board

    JP2010221694A

  • Liquid crystal polymer film and its laminate

    JP1998034742A

  • Metal clad laminated plate, manufacturing method of the same, printed wiring board using the same, and manufacturing method of printed wiring board

    JP2014116593A