Modified silicon anode materials and their preparation methods, anode sheets and batteries
By coating the surface of silicon anode materials with sulfonamide small molecules and caffeic acid to form a stable SEI film, the problem of electrolyte consumption caused by volume changes in silicon anode materials in lithium-ion batteries is solved, thereby improving battery performance and lifespan.
Patent Information
- Application Number
- CN202311608391.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-28
AI Technical Summary
Silicon anode materials in lithium-ion batteries suffer from large volume changes and continuous SEI film repair, leading to electrolyte consumption and affecting battery performance and lifespan.
The silicon core is coated with sulfonamide small molecules and caffeic acid to form a coating layer, which participates in the formation of SEI film and improves conductivity. It is tightly bonded to the binder through chemical bonds to alleviate volume expansion and electrolyte erosion.
It improves the rate performance and initial coulombic efficiency of the battery, extends the battery cycle life, and prevents electrode breakage and loss of active lithium.
Smart Images

Figure CN117438565B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery materials technology, and more specifically, to modified silicon anode materials, their preparation methods, anode sheets, and batteries. Background Technology
[0002] Silicon (Si) is considered one of the most promising and attractive anodes for next-generation lithium-ion batteries (LIBs) due to its high natural reserves, low discharge potential, and high theoretical specific capacity. However, it also has some inherent drawbacks, such as rapid capacity decay, low coulombic efficiency, and poor rate performance, which hinder its commercial application. Furthermore, silicon's lithium intercalation potential is below 0.5V, and during charge and discharge, the electrolyte decomposes on the silicon surface to form a natural solid electrolyte interphase (SEI) film. Simultaneously, silicon undergoes nearly 300% volume change during lithium-ion insertion and extraction. The SEI film is continuously damaged and regenerated during cycling, leading to continuous electrolyte consumption and battery failure. Naturally formed SEI films mainly include LiF and Li... x PF y Composed of PFy, it has very low ionic conductivity, which may hinder the diffusion and transfer of lithium ions during cycling, resulting in insufficient utilization of active materials and limited rate performance.
[0003] In view of this, the present invention is proposed. Summary of the Invention
[0004] The purpose of this invention is to provide modified silicon anode materials and their preparation methods, anode sheets, and batteries, aiming to improve at least one of the problems mentioned in the background art.
[0005] This invention is implemented as follows:
[0006] In a first aspect, the present invention provides a modified silicon anode material, comprising a silicon core and a coating layer covering the silicon core, wherein the coating layer contains sulfonamide small molecules and caffeic acid;
[0007] The sulfonamide small molecules are selected from at least one of N-methyl-N-nitroso-toluenesulfonamide, N-propyl-N-nitroso-toluenesulfonamide and N-methyl-toluenesulfonamide.
[0008] In an optional embodiment, the mass ratio of caffeic acid to silicon core is 0.01 to 0.1:1, preferably 0.01 to 0.08:1.
[0009] In an optional embodiment, the mass ratio of sulfonamide small molecules to silicon core is 0.01 to 0.08:1, preferably 0.01 to 0.05:1.
[0010] In a second aspect, the present invention provides a method for preparing a modified silicon anode material as described in any of the foregoing embodiments, comprising:
[0011] By using sulfonamide small molecules and caffeic acid to coat silicon particles, a coating layer is formed on the surface of the silicon particles.
[0012] In an optional embodiment, coating the silicon particles to form a coating layer on the surface of the silicon particles specifically includes:
[0013] Under an inert gas protective atmosphere, pre-oxidized silicon particles are placed in a solution containing sulfonamide small molecules, mixed evenly, and the solvent is evaporated to obtain primary modified silicon particles.
[0014] Under an inert gas protective atmosphere, primary modified silicon particles are placed in a solution containing caffeic acid, mixed evenly, and then the solvent is evaporated to obtain the modified anode material.
[0015] Optionally, before obtaining the primary modified silicon particles, the method further includes: pre-oxidizing the silicon particles in a hydrogen peroxide solution;
[0016] Optionally, the caffeic acid content in the solution is 1-10% by mass;
[0017] Optionally, when placing the pre-oxidized silicon particles in a solution containing sulfonamide molecules, the temperature of the solution containing sulfonamide molecules is controlled at 25-60°C, and the reaction is stirred for 2-5 hours before the solvent is evaporated; alternatively, the solvent is evaporated by stirring and heating in an oil bath at 60-100°C under inert gas conditions.
[0018] Optionally, in the solution containing sulfonamide small molecules, the solvent is selected from at least one of ethanol, methanol, acetone, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, and N-methylpyrrolidone;
[0019] Optionally, the mass percentage of sulfonamide small molecules in the solution is 1-10%;
[0020] Optionally, when placing the primary modified silicon particles in a solution containing caffeic acid, the temperature of the solution containing caffeic acid is controlled at 25–60°C, and the reaction is stirred for 2–5 hours before the solvent is evaporated.
[0021] Optionally, the solvent is evaporated by freeze drying; optionally, the freeze drying time is 2 to 8 hours.
[0022] In an optional embodiment, coating the silicon particles to form a coating layer on the surface of the silicon particles specifically includes:
[0023] Under an inert gas protective atmosphere, pre-oxidized silicon particles are placed in a solution containing sulfonamide small molecules, mixed evenly, and the solvent is evaporated to obtain primary modified silicon particles.
[0024] Under an inert gas protective atmosphere, primary modified silicon particles are placed in a solution containing caffeic acid, mixed evenly, and then the solvent is evaporated to obtain the modified anode material.
[0025] Optionally, before obtaining the primary modified silicon particles, the method further includes: pre-oxidizing the silicon particles in a hydrogen peroxide solution;
[0026] Optionally, the caffeic acid content in the solution is 1-10% by mass;
[0027] Optionally, when placing the pre-oxidized silicon particles in a solution containing sulfonamide small molecules, the ambient temperature is set to 25-60°C, and the reaction is stirred for 2-5 hours before the solvent is evaporated; alternatively, the solvent is evaporated by stirring and heating in an oil bath at 60-100°C under inert gas conditions.
[0028] Optionally, in the solution containing sulfonamide small molecules, the solvent is selected from at least one of ethanol, methanol, acetone, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, and N-methylpyrrolidone;
[0029] Optionally, the mass percentage of sulfonamide small molecules in the solution containing caffeic acid is 1-10%;
[0030] Optionally, when placing the primary modified silicon particles in a solution containing caffeic acid, the ambient temperature is set to 25–60°C, and the reaction is stirred for 2–5 hours before the solvent is evaporated.
[0031] Optionally, the solvent is evaporated by freeze drying; optionally, the freeze drying time is 2 to 8 hours.
[0032] Thirdly, the present invention provides a negative electrode sheet, which is prepared by using a modified silicon negative electrode material as described in any of the foregoing embodiments, or by using a modified silicon negative electrode material prepared by any of the foregoing embodiments as an active material.
[0033] Fourthly, the present invention provides a battery comprising a negative electrode sheet as described in the foregoing embodiments. The present invention has the following beneficial effects:
[0034] Sulfonamide small molecules are coated on the surface of the silicon core. Their special functional groups can participate in the formation of the SEI film and change its composition, thereby improving the conductivity of the negative electrode material and thus improving the rate performance of the battery. Since the coating layer contains sulfonamide small molecules, during the manufacturing process of the negative electrode, the sulfonamide small molecules can also be tightly bonded to the binder through bonding, which can effectively improve the adhesion between silicon particles and binder, ensure the integrity of the silicon electrode during charging and discharging, and prevent the electrode from cracking or falling off due to volume expansion. The sulfonamide small molecules are bonded to the surface of the silicon core through chemical bonds and will not fall off during the electrode preparation process, which can help to mitigate the corrosion of the electrode by the electrolyte. Caffeic acid and sulfonamide molecules can form new organic chain molecules rich in multifunctional groups through bonding. During charging and discharging, they undergo in-situ self-polymerization through the gain and loss of electrons from unsaturated chemical bonds, participating in the formation of a tough and stable SEI film. This alleviates the volume change of silicon during charging and discharging, reduces electrolyte consumption caused by repairing the SEI film, reduces the loss of active lithium, improves the initial coulombic efficiency of the battery, and extends the cycle life of the battery. Attached Figure Description
[0035] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0036] Figure 1 The first charge-discharge curves for the examples and comparative examples;
[0037] Figure 2 The diagram shows the long-term cycling performance specific capacity of the examples and comparative examples. Detailed Implementation
[0038] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0039] The modified silicon anode material, its preparation method, anode sheet, and battery provided by this invention will be described in detail below.
[0040] The modified silicon anode material provided in this embodiment of the invention includes a silicon core and a coating layer covering the silicon core, wherein the coating layer contains sulfonamide small molecules and caffeic acid;
[0041] The sulfonamide small molecules are selected from at least one of N-methyl-N-nitroso-toluenesulfonamide, N-propyl-N-nitroso-toluenesulfonamide and N-methyl-toluenesulfonamide.
[0042] The modified silicon anode material provided in this invention has sulfonamide small molecules coated on the surface of the silicon core. Their special functional groups can participate in the formation of the SEI film and change its composition, improving the conductivity of the anode material and thus improving the rate performance of the battery. Because the coating layer contains sulfonamide small molecules, during the manufacturing process of the anode sheet, the sulfonamide small molecules and the binder can also be tightly bonded through bonding, effectively improving the adhesion between silicon particles and the binder, ensuring the integrity of the silicon electrode during charging and discharging, and preventing electrode cracking and material loss due to volume expansion. The sulfonamide small molecules are chemically bonded to the surface of the silicon core and will not detach during electrode preparation, thus mitigating electrolyte erosion of the electrode. Caffeic acid and sulfonamide molecules can form new organic chain molecules rich in multifunctional groups through bonding. During charging and discharging, they undergo in-situ self-polymerization through the gain and loss of electrons from unsaturated chemical bonds, participating in the formation of a tough and stable SEI film. This alleviates the volume change of silicon during charging and discharging, reduces electrolyte consumption caused by repairing the SEI film, reduces the loss of active lithium, improves the initial coulombic efficiency of the battery, and extends the cycle life of the battery.
[0043] Preferably, the mass ratio of caffeic acid to the silicon core is 0.01 to 0.1:1 (e.g., 0.01:1, 0.02:1, 0.05:1, 0.08:1, or 0.1:1), more preferably 0.01 to 0.08:1. The optimal mass ratio of sulfonamide small molecules to the silicon core within the above range yields the best results. If the coating amount of sulfonamide small molecules is too low, the improvement in electrochemical performance will not be significant enough. If the coating amount exceeds the above range, the binder function will decrease, affecting battery performance.
[0044] Preferably, the mass ratio of sulfonamide small molecules to the silicon core is 0.01–0.08:1 (e.g., 0.01:1, 0.02:1, 0.05:1, or 0.08:1), more preferably 0.01–0.05:1. The optimal mass ratio of caffeic acid to the silicon core within the above range yields the best results. If the caffeic acid coating amount is too low, the improvement in electrochemical performance is not significant enough. If the coating amount exceeds the above range, it will lead to a decrease in electrode conductivity, affecting battery capacity. This embodiment of the invention provides a method for preparing the above-mentioned modified silicon anode material, comprising:
[0045] By using sulfonamide small molecules and caffeic acid to coat silicon particles, a coating layer is formed on the surface of the silicon particles.
[0046] Specifically, the methods include:
[0047] S1, Pre-oxidation
[0048] Silicon particles are pre-oxidized in a hydrogen peroxide solution.
[0049] Specifically, silicon particles are placed in 30% hydrogen peroxide solution and reacted for 120 minutes, then centrifuged. The resulting solid material is then dried to obtain pre-oxidized silicon particles.
[0050] Optionally, silicon particles with a particle size of 100–150 nm can be used as raw materials.
[0051] It should be noted that the concentration of hydrogen peroxide and the reaction time used can be adjusted as needed, and are not limited to the concentration and reaction time mentioned above.
[0052] S2, Initial Covering
[0053] Under an inert gas protective atmosphere, pre-oxidized silicon particles are placed in a solution containing sulfonamide small molecules, mixed evenly, and then the solvent is evaporated to obtain primary modified silicon particles.
[0054] Preferably, to ensure high reaction efficiency and uniform coating, in this step, the temperature of the solution containing sulfonamide small molecules is controlled at 25-60°C (e.g., 25°C, 40°C, 50°C or 60°C), and the reaction is stirred for 2-5 hours (e.g., 2 hours, 3 hours or 5 hours) before the solvent is allowed to evaporate.
[0055] Optionally, in the solution containing sulfonamide small molecules, the solvent is selected from at least one of ethanol, methanol, acetone, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, and N-methylpyrrolidone;
[0056] Preferably, to ensure that solvent evaporation is achieved while ensuring uniform coating and the binding of sulfonamide small molecules to silicon particles, the solvent evaporation method is to dry the solvent under inert gas conditions by stirring and heating in an oil bath at 60–120°C (e.g., 60°C, 80°C, 100°C, or 1200°C) for 4–8 hours (e.g., 4 hours, 6 hours, or 8 hours).
[0057] Optionally, the mass percentage of sulfonamide small molecules in the solution containing sulfonamide small molecules is 1% to 10% (e.g., 1%, 3%, 5%, 8% or 10%).
[0058] Optionally, in the solution containing sulfonamide small molecules, the solvent is selected from at least one of ethanol, methanol, acetone, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, and N-methylpyrrolidone.
[0059] Specifically, the inert gas can be at least one of nitrogen and argon.
[0060] S3, Wrap again
[0061] Under an inert gas protective atmosphere, primary modified silicon particles are placed in a solution containing caffeic acid, mixed evenly, and then the solvent is evaporated to obtain the modified anode material.
[0062] Preferably, to ensure high reaction efficiency and uniform coating, in this step, the temperature of the solution containing caffeic acid is controlled at 25-60°C (e.g., 25°C, 40°C, 50°C, or 60°C), and the reaction is stirred for 2-5 hours (e.g., 2 hours, 3 hours, or 5 hours) before the solvent is allowed to evaporate.
[0063] Preferably, to ensure solvent evaporation while maintaining uniform coating and good adhesion between caffeic acid and silicon particles, the solvent evaporation method is freeze-drying. Optionally, the freeze-drying time is 2–8 hours (e.g., 2 hours, 4 hours, 6 hours, or 8 hours).
[0064] Optionally, the caffeic acid content in the solution is 1% to 10% by mass (e.g., 1%, 3%, 5%, 8% or 10%).
[0065] Optionally, in the solution containing sulfonamide small molecules, the solvent is selected from at least one of ethanol, methanol, acetone, N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, and N-methylpyrrolidone; specifically, the inert gas can be at least one of nitrogen and argon.
[0066] It should be noted that steps S2 and S3 can be interchanged; that is, caffeic acid can be coated first, followed by the coating of small flavonoid molecules.
[0067] The negative electrode sheet provided in this embodiment of the invention uses the modified silicon negative electrode material provided in this embodiment of the invention, or the modified silicon negative electrode material prepared by the preparation method provided in this embodiment of the invention, as the active material. Because this negative electrode sheet uses the modified silicon negative electrode material provided in this invention as the active material, it has superior electrochemical performance.
[0068] The preparation method of the negative electrode sheet is as follows: using CMC or PVA as a binder, SP as a conductive agent, and modified silicon negative electrode material and solvent to prepare a negative electrode slurry, which is then further prepared into a negative electrode sheet.
[0069] The battery provided in this embodiment of the invention includes a negative electrode sheet provided in this embodiment of the invention. Because the battery includes the negative electrode sheet provided in this embodiment of the invention, it has superior electrochemical performance.
[0070] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0071] Example 1
[0072] Silicon particles were placed in 30% hydrogen peroxide solution and reacted for 120 minutes, then centrifuged. The resulting solid was dried to obtain pre-oxidized silicon particles.
[0073] Under an argon protective atmosphere, pre-oxidized silicon particles were placed in a solution containing N-methyl-N-nitroso-p-toluenesulfonamide (concentration 5%, solvent N-methylpyrrolidone) at 25°C and stirred for 4 hours. Then, the mixture was dried by stirring and heating in an oil bath at 80°C for 6 hours to obtain primary modified silicon particles.
[0074] Under an argon protective atmosphere, primary modified silicon particles were placed in a solution containing caffeic acid (concentration of 5%, solvent of deionized water) at 40°C, stirred and mixed for 5 hours, and then freeze-dried for 5 hours to obtain modified silicon anode material.
[0075] In this embodiment, the mass ratio of caffeic acid to silicon particles in the solution containing caffeic acid is 0.05:1; the mass ratio of N-methyl-N-nitroso-toluenesulfonamide to silicon particles in the solution containing N-methyl-N-nitroso-toluenesulfonamide is 0.03:1.
[0076] Example 2
[0077] Silicon particles were placed in 30% hydrogen peroxide solution and reacted for 120 minutes, then centrifuged. The resulting solid was dried to obtain pre-oxidized silicon particles.
[0078] Under an argon protective atmosphere, pre-oxidized silicon particles were placed in a solution containing N-methyl-N-nitroso-p-toluenesulfonamide (concentration 5%, solvent N-methylpyrrolidone) at 25°C and stirred for 2 hours. Then, the mixture was dried by stirring and heating in an oil bath at 60°C for 4 hours to obtain primary modified silicon particles.
[0079] Under an argon protective atmosphere, primary modified silicon particles were placed in a solution containing caffeic acid (concentration of 5%, solvent of deionized water) at 25°C. After stirring and mixing for 2 hours, the mixture was freeze-dried for 2 hours to obtain the modified silicon anode material.
[0080] In this embodiment, the mass ratio of caffeic acid to silicon particles in the solution containing caffeic acid is 0.01:1; the mass ratio of N-methyl-N-nitroso-toluenesulfonamide to silicon particles in the solution containing N-methyl-N-nitroso-toluenesulfonamide is 0.01:1.
[0081] Example 3
[0082] Silicon particles were placed in 30% hydrogen peroxide solution and reacted for 120 minutes, then centrifuged. The resulting solid was dried to obtain pre-oxidized silicon particles.
[0083] Under an argon protective atmosphere, pre-oxidized silicon particles were placed in a solution containing N-methyl-N-nitroso-p-toluenesulfonamide (concentration 5%, solvent N-methylpyrrolidone) at 25°C. After stirring and mixing for 5 hours, the mixture was dried by stirring and heating in an oil bath at 120°C for 8 hours to obtain primary modified silicon particles.
[0084] Under an argon protective atmosphere, primary modified silicon particles were placed in a solution containing caffeic acid (concentration of 5%, solvent of deionized water) at 60°C. After stirring and mixing for 5 hours, the mixture was freeze-dried for 8 hours to obtain the modified silicon anode material.
[0085] In this embodiment, the mass ratio of caffeic acid to silicon particles in the solution containing caffeic acid is 0.08:1; the mass ratio of N-methyl-p-toluenesulfonamide to silicon particles in the solution containing N-methyl-p-toluenesulfonamide is 0.05:1.
[0086] Example 4
[0087] This embodiment is basically the same as Embodiment 1, except that the mass ratio of caffeic acid to silicon particles in the solution containing caffeic acid is 0.1:1.
[0088] Example 5
[0089] This embodiment is basically the same as Embodiment 1, except that the mass ratio of sulfonamide small molecules to silicon particles in the solution containing sulfonamide small molecules is 0.08:1.
[0090] Comparative Example 1
[0091] This comparative example provides silicon particles that have not undergone any modification treatment and are the same as the raw material silicon particles used in Example 1.
[0092] Comparative Example 2
[0093] This comparative example is basically the same as Example 1, except that after the caffeic acid coating, no sulfonamide small molecule coating was performed.
[0094] Comparative Example 3
[0095] This comparative example is basically the same as Example 1, except that: sulfonamide small molecules are directly coated on the outside of the silicon particles, and caffeic acid is not coated.
[0096] Experimental Example
[0097] Using PVA as a binder and SP as a conductive agent, the silicon anode material, binder, and conductive agent prepared or provided in the above-mentioned embodiments and comparative examples are mixed in a ratio of 80:10:10 to form the anode. The counter electrode is lithium metal, and a coin cell is assembled. The electrochemical performance of the battery is tested.
[0098] Specific testing methods:
[0099] The test conditions for the first reversible capacity and the first coulombic efficiency were: discharge to 0.01V at a constant current of 0.05C at 25℃, and charge to 1V at a constant current of 0.05C (1C=4200mAh / g);
[0100] The test conditions for 200 cycles were as follows: at 25℃, discharge at a constant current of 0.05C to 0.01V, charge at a constant current of 0.05C to 1V, repeat this charge / discharge cycle 3 times. Then, switch the current to discharge at a constant current of 0.1C to 0.01V, charge at a constant current of 0.1C to 1V, repeat this charge / discharge cycle 5 times. Finally, discharge at a constant current of 0.2C to 0.01V, charge at a constant current of 0.5C to 1V for a complete charge / discharge cycle.
[0101] The test conditions for rate performance are as follows: discharge test at 0.1C and charge test at 0.1 to 20C. If the ratio of the test result to the reversible capacity is ≥70%, it is recorded as "excellent"; if the ratio of the test result to the reversible capacity is ≥50%, it is recorded as "good"; if the ratio of the test result to the reversible capacity is <50%, it is recorded as "poor".
[0102] Record the test results in Table 1 and plot the curves as shown below. Figure 1 and Figure 2 .
[0103] Table 1 Electrochemical performance of each example and comparative example
[0104]
[0105]
[0106] As shown in Table 1, the reversible capacity, initial coulombic efficiency, rate capability, and reversible capacity after 200 cycles of the modified silicon anode materials prepared in each embodiment of the present invention are significantly higher than those before modification (Comparative Example 1). Comparing Example 4 with the corresponding embodiment, its initial efficiency and cycle performance are slightly worse, while the caffeic acid coating amount in Example 4 is slightly higher, exceeding the range required by the preferred embodiment of this application. This indicates that excessively high caffeic acid coating amount does not further improve the electrochemical performance of the silicon anode material. Comparing Example 5 with the corresponding embodiment, its initial efficiency and cycle performance are slightly worse, while the sulfonamide small molecule coating amount in Example 5 is slightly higher, exceeding the range required by the preferred embodiment of this application. This indicates that excessively high sulfonamide small molecule coating amount does not further improve the electrochemical performance of the silicon anode material. Comparing Example 1 with Comparative Example 2, Comparative Example 2 only coated with caffeic acid, and its rate performance was significantly worse than that of Example 1. Comparing Comparative Example 1 with Comparative Example 2, Comparative Example 1 showed worse performance in all aspects, indicating that caffeic acid coating can effectively improve the electrochemical performance of silicon anode materials. Comparing Comparative Example 3 with Example 1, Comparative Example 3 had worse initial efficiency and cycle performance, but its rate performance was the same as that of Example 1. This indicates that simultaneously coating with sulfonamide small molecules and caffeic acid can improve the electrochemical performance of silicon anode materials.
[0107] from Figure 1 The graphs show the initial charge-discharge curves of the original silicon half-cell and the surface-modified silicon half-cells from Examples 1-4. The original silicon half-cell exhibits a low initial coulombic efficiency of only 82.5% and a discharge capacity of 2258.3 mAh / g. The silicon anode cell with the surface-grafted layered modification layer achieves the highest initial coulombic efficiency of 85.6% and a discharge capacity of 2586.2 mAh / g. This indicates that the effective modification layer formed on the surface of the grafted silicon particles can significantly reduce lithium consumption of the silicon anode during the initial charge-discharge process, thereby improving the initial coulombic efficiency and discharge capacity of the battery.
[0108] Figure 2 The graphs show the initial charge-discharge curves of the original silicon half-cell and the surface-modified silicon half-cells from Examples 1-4. Due to the significant volume expansion of silicon during lithium insertion / extraction, the SEI film ruptures. The continuous repair of the SEI significantly increases lithium consumption during cycling, ultimately leading to poor battery cycle performance; after 200 cycles, the capacity decays to 1173.7 mAh / g. In contrast, the silicon anode half-cell with the surface-grafted layered structure exhibits significantly improved cycle stability. After optimization and improvement of the coating layer, the battery capacity reaches 1889.4 mAh / g after 200 cycles. This indicates that the synergistic effect of caffeic acid and sulfonamide small molecules effectively suppresses silicon particle expansion, prevents electrode pulverization and cycle decay, and extends battery cycle life.
[0109] In summary, the modified silicon anode material provided in the embodiments of the present invention has the following advantages:
[0110] 1. Sulfonamide small molecules are coated on the surface of silicon core. Their special functional groups can participate in the formation of SEI film and change the composition of SEI film, improve the lithium conductivity of SEI film, and thus improve the rate performance of battery.
[0111] 2. Because the coating layer contains sulfonamide small molecules, during the manufacturing process of the negative electrode, the sulfonamide small molecules and the binder can also be tightly bonded through bonding, which can effectively improve the adhesion between silicon particles and binder, ensure the integrity of silicon electrode during charging and discharging, and prevent electrode cracking and material loss due to volume expansion;
[0112] 3. Sulfonamide small molecules bind to the silicon core surface through chemical bonds and will not detach during electrode preparation, thus mitigating electrolyte corrosion of the electrode.
[0113] In a preferred embodiment, the coating layer of the modified silicon anode material also contains caffeic acid. Caffeic acid and sulfonamide small molecules can form new organic chain-like small molecules rich in multifunctional groups through bonding. During the charge and discharge process, they undergo in-situ self-polymerization through the gain and loss of electrons from unsaturated chemical bonds to participate in the formation of a tough and stable SEI film, which alleviates the volume change of silicon during the charge and discharge process, reduces electrolyte consumption caused by repairing the SEI film and reduces the loss of active lithium, thereby improving the first coulombic efficiency of the battery and extending the cycle life of the battery.
[0114] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A modified silicon negative electrode material, characterized in that, It includes a silicon core and a coating layer covering the silicon core, wherein the coating layer contains sulfonamide small molecules and caffeic acid; The sulfonamide small molecule is selected from at least one of N-methyl-N-nitroso-toluenesulfonamide, N-propyl-N-nitroso-toluenesulfonamide, and N-methyl-toluenesulfonamide; The mass ratio of caffeic acid to the silicon core is 0.01~0.1:1; The mass ratio of the sulfonamide small molecule to the silicon core is 0.01~0.08:1; The method for preparing the modified silicon anode material includes coating silicon particles with the sulfonamide small molecules and caffeic acid to form the coating layer on the surface of the silicon particles. Specifically, coating the silicon particles to form the coating layer includes: Under an inert gas protective atmosphere, the pre-oxidized silicon particles are placed in a solution containing caffeic acid, mixed evenly, and the solvent is evaporated to obtain primary modified silicon particles. Under an inert gas protective atmosphere, the primary modified silicon particles are placed in a solution containing sulfonamide small molecules, mixed evenly, and then the solvent is evaporated to obtain the modified silicon anode material.
2. The modified silicon anode material of claim 1, wherein, The mass ratio of caffeic acid to the silicon core is 0.01~0.08:
1.
3. The modified silicon anode material of claim 1, wherein, The mass ratio of the sulfonamide small molecules to the silicon core is 0.01~0.05:
1.
4. The modified silicon anode material of claim 1, wherein, The process further includes, prior to obtaining the primary modified silicon particles, pre-oxidizing the silicon particles in a hydrogen peroxide solution.
5. The modified silicon anode material of claim 1, wherein, The caffeic acid content in the solution is 1-10% by mass.
6. The modified silicon anode material of claim 1, wherein, When the pre-oxidized silicon particles are placed in a solution containing caffeic acid, the temperature of the caffeic acid solution is controlled at 25~60℃, and the reaction is stirred for 2~5 hours before the solvent is evaporated.
7. The modified silicon anode material of claim 1, wherein, In the solution containing caffeic acid, the solvent is selected from at least one of deionized water and ethanol.
8. The modified silicon anode material according to claim 1, characterized in that, The mass percentage of sulfonamide small molecules in the solution is 1-10%.
9. The modified silicon anode material according to claim 1, characterized in that, When the primary modified silicon particles are placed in a solution containing sulfonamide molecules, the temperature of the solution containing sulfonamide molecules is controlled at 25~60℃, and the reaction is stirred for 2~5 hours before the solvent is evaporated.
10. The modified silicon anode material according to claim 9, characterized in that, The solvent is evaporated by freeze drying.
11. The modified silicon anode material according to claim 10, characterized in that, The freeze-drying time is 2 to 8 hours.
12. A negative electrode sheet, characterized in that, It is prepared using the modified silicon anode material as described in any one of claims 1 to 11 as the active material.
13. A battery, characterized in that, Includes the negative electrode as described in claim 12.
Citation Information
Patent Citations
Graphene modified silicon negative electrode material and preparation method and application thereof
CN114613955A
Silicon negative electrode material and preparation method thereof, negative electrode and lithium ion battery