Production process of base paper for U-shaped drinking straws

By preferring the combination of bleached sulfate broadleaf pulp and disc grinding sheet, the concentration of the glue agent is reduced and the pressure of the film transfer glue applicator is increased, and the problem of high stiffness of the U-shaped straw is solved, and the softness and toughness of the paper page are achieved. Improve to meet the production needs of U-shaped paper straws.

CN117449123BActive Publication Date: 2024-11-29SHANDONG RENFENG SPECIAL MATERIALS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311430304.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-31
Publication Date
2024-11-29
Estimated Expiration
2043-10-31

AI Technical Summary

Technical Problem

The existing U-shaped straw base paper has high stiffness, is easy to break, has poor plasticity, and it is difficult to make soft U-shaped straw paper.

Method used

Using the preferred bleached sulfate broadleaf slurry, disk grinding sheet combination and beating process, reduce the concentration of the surface glue sizing agent, select a small metering rod, increase the pressure of the membrane transfer glue sizing machine, and control the surface strength and softness of the paper page. sex.

Benefits of technology

By increasing the fiber brooming rate and lateral arrangement and increasing the fiber softness, the softness and toughness of the U-shaped straw base paper are ensured, meeting the production requirements of U-shaped paper straws.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the field of papermaking technology, and specifically relates to a production process for U-shaped straw base paper. The production process for U-shaped straw base paper comprises pulp board → chain conveyor → pulper → discharge tank → pulper → pulping tank → pre-papering tank → pulping pump → pressure screen → head box → wire section → pressing section → large cylinder → sizing machine → cylinder assembly → calender → winding section → rewinding → packaging and storage. This process ensures the softness of the paper sheet by optimizing bleached sulfate broadleaf pulp, optimizing the selection and process of pulping and grinding discs, reducing the concentration of the surface sizing agent, selecting a smaller metering rod, and increasing the pressure of the film transfer sizing machine, so as to moderately reduce the amount of sizing while ensuring the surface strength of the paper sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of papermaking, and in particular relates to a production process of U-shaped straw base paper. Background Art

[0002] Most of the existing U-shaped straws are made of plastic because plastic is soft and has good plasticity. With the implementation of the national plastic ban, replacing plastic with paper is an inevitable trend. However, the base paper for straws is generally stiff, easy to break, and has poor plasticity, making it difficult to make U-shaped straws with paper.

[0003] Patent application CN112297514A was published on September 29, 2020. A large-scale production method for oblique U-shaped paper straws is disclosed, comprising the following steps: S1: base paper slitting, cutting the base paper into paper suitable for producing paper straws; S2: tube rolling, rolling the cut paper and glue into paper straws through equipment; S3: tube blank aging treatment, controlling the moisture content of paper straws; S4: tube blank slitting oblique mouth, cutting straight tubes into oblique tubes; S5: U-shaped paper straw molding, bending straight tubes into U-shaped paper straws; S6: packaging, drying and packaging, and then sealing and storing. However, it only prepares U-shaped straws, and does not limit the production process of base paper. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a production process for U-shaped straw base paper, by preferentially selecting bleached sulfate broadleaf pulp, adopting a reasonable disc grinding plate combination and pulping process, reducing the concentration of the surface sizing agent, selecting a smaller metering rod, and increasing the pressure of the film transfer sizing machine, the amount of sizing can be appropriately reduced while ensuring the surface strength of the paper sheet, thereby ensuring the softness of the paper sheet.

[0005] The technical solution adopted by the present invention is:

[0006] The production process of the U-shaped straw base paper comprises pulp board → chain conveyor → pulper → discharge tank → pulper → pulping tank → pre-slurry tank → pulping pump → pressure screen → head box → wire part → pressing part → large cylinder → sizing machine → cylinder assembly → calender → winding part → rewinding → packaging and storage;

[0007] In the sizing machine process, a surface sizing agent is added, and the formula of the surface sizing agent is composed of the following raw materials in parts by weight:

[0008] 90-100 parts of amphoteric surface tapioca starch;

[0009] Chitosan 6-10 parts;

[0010] Water 1159-1219 parts;

[0011] In the pulp board process, the pulp board ratio is 100% bleached kraft hardwood pulp, 0.5-1 kg / ton of caustic soda is added during pulping, and the pH is adjusted to 7.5-8.0, which is conducive to fiber water absorption and swelling and reduces cutting.

[0012] Cationic starch is added between the stock forming tank and the pre-slurry tank, wet strength agent and AKD are added in sequence between the pre-slurry tank and the pulp flushing pump, and silica sol is added between the pressure screen and the headbox.

[0013] The preparation method of the surface sizing agent is:

[0014] Add 1 / 3 of water to the formulated amount of amphoteric surface cassava starch, stir evenly in a surface glue cooking tank, ventilate, heat to 90-95°C, keep warm for 15-20 minutes, move to a surface glue dilution barrel, cool to 65-70°C, mix with chitosan and 2 / 3 of water to form a surface sizing agent. The amphoteric surface cassava starch is preferably amphoteric surface cassava starch LS-2, and the chitosan is chitosan CK-5525.

[0015] The bleached sulphate broadleaf pulp is bleached sulphate eucalyptus broadleaf pulp, preferably Brazilian Bull brand or Parrot brand bleached sulphate broadleaf eucalyptus pulp.

[0016] In the pulping process, two DD720 double-disc refiners are used in series for pulping, both of which use broom fin-type refiners, with a beating degree of 35-38° SR and a wet weight of 2.0-3.0 g.

[0017] The amount of cationic starch added is 10-12 kg / ton of pulp, the amount of AKD added is 15-20 kg / ton of pulp, the amount of silica sol added is 2-4 kg / ton of pulp, and the amount of wet strength agent added is 15-18 kg / ton of pulp. AKD is preferably kemira KD324TP, the cationic starch is a conventional commercial product with a degree of substitution of 0.03, and the wet strength agent is food grade, and its main component is polyamide polyamine epichlorohydrin.

[0018] The surface sizing agent has a solid content of 7-9%, a viscosity of 5-15 MPa.s, a pH of 5-6, and a temperature of 65-70°C.

[0019] The production process of the U-shaped straw base paper, the operating parameters of the paper machine are:

[0020] (1) Machine speed 200-250m / min, pulp-to-net speed ratio 0.9;

[0021] (2) The steam pressure of the large cylinder is 500-550KPa, and the pressure of the double rollers is set at 100-110KN / m;

[0022] (3) Film transfer sizing machine control parameters;

[0023] Metering rod model and pressure;

[0024] Front metering rod V24, line pressure 30KN / m;

[0025] The reverse metering rod is V24, with a line pressure of 30KN / m;

[0026] The paper pick-up amount of the new surface sizing agent is 1-1.5g / ㎡ on the front side and 1-1.5g / ㎡ on the back side;

[0027] The paper dryness of the paper entering the film transfer sizing machine is ≥92%, and the paper dryness of the paper leaving the film transfer sizing machine is ≥75%.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) By selecting Brazilian Bull or Parrot bleached sulphate broadleaf eucalyptus pulp, the finished paper has greater flexibility; by adding 0.5-1 kg / ton of caustic soda during pulping, the pH value is adjusted to increase the fiber's water absorption and swelling, reduce fiber cutting during pulping, and improve the toughness of the finished paper.

[0030] (2) By increasing the pulping beating degree and the fiber brooming rate, while increasing the pulp-to-net speed ratio and increasing the lateral arrangement of the fibers, the fiber softness is ensured to meet the requirements of U-shaped paper straws.

[0031] (3) By controlling the moisture content of the finished paper at around 7.5-8.0%, the softness of the straw base paper is increased.

[0032] (4) By reducing the concentration of the surface sizing agent, selecting a smaller metering rod, and increasing the pressure of the film transfer sizing machine, the softness of the paper sheet is ensured while ensuring the surface strength of the paper sheet. DETAILED DESCRIPTION

[0033] The present invention is further described below with reference to the embodiments, but they do not limit the implementation of the present invention.

[0034] Amphoteric surface cassava starch LS-2 Jiangxi Liuhe Chemical Industry Co., Ltd.;

[0035] Chitosan CK-5525 Linyi Sanshui Technology Co., Ltd.;

[0036] kemiraKD324TP Kemira Chemicals (Shanghai) Co., Ltd.;

[0037] Wet strength agent Japan Kurita Water Treatment New Materials Co., Ltd.;

[0038] Bleached sulphate eucalyptus hardwood pulp (Brazilian Bull brand) Eldorado Brasil;

[0039] Bleached sulphate eucalyptus hardwood pulp (Parrot brand) Aracmz, Brazil;

[0040] Test method:

[0041] Smoothness: GB / T 456-2002 "Determination of smoothness of paper and paperboard (Buick method)";

[0042] Tensile strength: GB / T12914-2008 "Determination of tensile strength of paper and paperboard";

[0043] Whiteness: GB / 7974-1987 "Determination of whiteness of paper and paperboard (diffuse vertical method)"

[0044] Tear resistance: GB / T 455-2002 "Determination of tear resistance of paper and paperboard";

[0045] Burst strength: GB / T 454-2020 "Determination of burst strength of paper";

[0046] Water absorption: GB / T 1540-2002 "Determination of water absorption of paper and paperboard - Cobber method";

[0047] Stiffness: GB / T 2679.3-1996 "Determination of stiffness of paper and paperboard".

[0048] Example 1

[0049] The production process is as follows: pulp board → chain conveyor → pulper → unloading tank → pulper → pulping tank → pre-pulping tank → pulping pump → pressure screen → head box → wire section → pressing section → large cylinder → sizing machine → cylinder assembly → calender → winding section → rewinding → packaging and storage;

[0050] The formula of the surface sizing agent is composed of the following raw materials in parts by weight:

[0051] 100 parts of amphoteric surface tapioca starch;

[0052] Chitosan 6 parts;

[0053] Water 1219 parts;

[0054] In the pulp board process, the pulp board ratio is 100% bleached kraft eucalyptus hardwood pulp (Brazilian Bull brand), 1 kg / ton of caustic soda is added during pulping, and the pH is adjusted to 7.8.

[0055] The preparation method of the surface sizing agent is:

[0056] Add 1 / 3 of water to the formulated amount of amphoteric surface cassava starch in a surface glue cooking tank, stir evenly, ventilate, and heat to 95°C, keep warm for 20 minutes, move to a surface glue dilution barrel, cool to 68°C, and mix with chitosan and 2 / 3 of water to form a surface sizing agent.

[0057] In the pulping process, two DD720 double-disc refiners were used in series for pulping, both of which adopted broom fin-type refiners, with a beating degree of 36°SR and a wet weight of 2.5g.

[0058] The amount of cationic starch added is 10 kg / ton of pulp, the amount of AKD added is 16 kg / ton of pulp, the amount of silica sol added is 2.5 kg / ton of pulp, and the amount of wet strength agent added is 15 kg / ton of pulp.

[0059] The standards for the surface sizing agent are 8.2% solid content, 7 MPa.s viscosity, 5.2 pH and 66°C temperature.

[0060] The paper machine operating parameters are:

[0061] (1) Machine speed 210m / min, pulp-to-web speed ratio 0.9;

[0062] (2) The steam pressure of the large cylinder is 520KPa, and the pressure of the double rollers is set at 100KN / m;

[0063] (3) Film transfer sizing machine control parameters;

[0064] Metering rod model and pressure;

[0065] Front metering rod V24, line pressure 30KN / m;

[0066] The reverse metering rod is V24, with a line pressure of 30KN / m;

[0067] The paper pick-up amount of the new surface sizing agent is 1.2g / ㎡ on the front side and 1.2g / ㎡ on the back side;

[0068] The paper dryness of the paper entering the film transfer sizing machine is 92.5%, and the paper dryness of the paper leaving the film transfer sizing machine is 76%.

[0069] The test results are shown in Table 1.

[0070] Example 2

[0071] The production process is as follows: pulp board → chain conveyor → pulper → unloading tank → pulper → pulping tank → pre-pulping tank → pulping pump → pressure screen → head box → wire section → pressing section → large cylinder → sizing machine → cylinder assembly → calender → winding section → rewinding → packaging and storage;

[0072] The formula of the surface sizing agent is composed of the following raw materials in parts by weight:

[0073] Amphoteric surface tapioca starch 95 parts;

[0074] Chitosan 8 parts;

[0075] 1200 parts of water;

[0076] In the pulping process, the pulping ratio is 100% bleached kraft eucalyptus hardwood pulp (Brazilian Parrot brand), and 0.6 kg / ton of caustic soda is added during pulping to adjust the pH to 7.8.

[0077] The preparation method of the surface sizing agent is:

[0078] Add 1 / 3 of water to the formulated amount of amphoteric surface cassava starch in a surface glue cooking tank, stir evenly, ventilate, and heat to 95°C, keep warm for 20 minutes, move to a surface glue dilution barrel, cool to 68°C, and mix with chitosan and 2 / 3 of water to form a surface sizing agent.

[0079] In the pulping process, two DD720 double-disc refiners were used in series for pulping, both of which adopted broom fin-type refiners, with a beating degree of 38°SR and a wet weight of 2.2g.

[0080] The amount of cationic starch added is 12 kg / ton of pulp, the amount of AKD added is 120 kg / ton of pulp, the amount of silica sol added is 3 kg / ton of pulp, and the amount of wet strength agent added is 17 kg / ton of pulp.

[0081] The standards for the surface sizing agent are 8.2% solid content, 10mPa.s viscosity, 5.8 pH and 67°C temperature.

[0082] The paper machine operating parameters are:

[0083] (1) Machine speed 230m / min, pulp-to-web speed ratio 0.9;

[0084] (2) The steam pressure of the large cylinder is 530KPa, and the pressure of the double rollers is set at 110KN / m;

[0085] (3) Film transfer sizing machine control parameters;

[0086] Metering rod model and pressure;

[0087] Front metering rod V24, line pressure 30KN / m;

[0088] The reverse metering rod is V24, with a line pressure of 30KN / m;

[0089] The paper pick-up amount of the new surface sizing agent is 1.5g / ㎡ on the front side and 1.5g / ㎡ on the back side;

[0090] The paper dryness of the paper entering the film transfer sizing machine is 94%, and the paper dryness of the paper leaving the film transfer sizing machine is 78%.

[0091] The test results are shown in Table 1.

[0092] Example 3

[0093] The production process is as follows: pulp board → chain conveyor → pulper → unloading tank → pulper → pulping tank → pre-pulping tank → pulping pump → pressure screen → head box → wire section → pressing section → large cylinder → sizing machine → cylinder assembly → calender → winding section → rewinding → packaging and storage;

[0094] The formula of the surface sizing agent is composed of the following raw materials in parts by weight:

[0095] Amphoteric surface tapioca starch 96 parts;

[0096] Chitosan 10 parts;

[0097] Water 1209 parts;

[0098] In the pulp board process, the pulp board ratio is 100% bleached kraft eucalyptus hardwood pulp (Brazilian Parrot brand), and 0.8 kg / ton of caustic soda is added during pulping to adjust the pH to 7.9.

[0099] The preparation method of the surface sizing agent is:

[0100] Add 1 / 3 of water to the formulated amount of amphoteric surface cassava starch in a surface glue cooking tank, stir evenly, ventilate, heat to 95°C, keep warm for 20 minutes, move to a surface glue dilution barrel, cool to 69°C, and mix with chitosan and 2 / 3 of water to form a surface sizing agent.

[0101] In the pulping process, two DD720 double-disc refiners were used in series for pulping, both of which adopted broom fin-type refiners, with a beating degree of 37°SR and a wet weight of 2.9g.

[0102] The amount of cationic starch added is 11 kg / ton of pulp, the amount of AKD added is 18 kg / ton of pulp, the amount of silica sol added is 4 kg / ton of pulp, and the amount of wet strength agent added is 18 kg / ton of pulp.

[0103] The standards for the surface sizing agent are 8.8% solid content, 15mPa.s viscosity, 6 ph and 70°C temperature.

[0104] The paper machine operating parameters are:

[0105] (1) Machine speed 250m / min, pulp-to-web speed ratio 0.9;

[0106] (2) The steam pressure of the large cylinder is 550KPa, and the pressure of the double rollers is set at 110KN / m;

[0107] (3) Film transfer sizing machine control parameters;

[0108] Metering rod model and pressure;

[0109] Front metering rod V24, line pressure 30KN / m;

[0110] The reverse metering rod is V24, with a line pressure of 30KN / m;

[0111] The paper pick-up amount of the new surface sizing agent is 1.4g / ㎡ on the front side and 1.3g / ㎡ on the back side;

[0112] The paper dryness of the paper entering the film transfer sizing machine is 95%, and the paper dryness of the paper leaving the film transfer sizing machine is 79%.

[0113] The test results are shown in Table 1.

[0114] Comparative Example 1

[0115] The production process is as follows: pulp board → chain conveyor → pulper → unloading tank → pulper → pulping tank → pre-pulping tank → pulping pump → pressure screen → head box → wire section → pressing section → large cylinder → sizing machine → cylinder assembly → calender → winding section → rewinding → packaging and storage;

[0116] The formula of the surface sizing agent is composed of the following raw materials in parts by weight:

[0117] Amphoteric surface tapioca starch 97 parts;

[0118] Chitosan 9 parts;

[0119] Water 1212 parts;

[0120] In the pulp board process, the pulp board ratio is 90% bleached sulfate hardwood pulp and 10% bleached sulfate softwood pulp. When pulping, 0.7 kg / ton of caustic soda is added to adjust the pH to 7.8.

[0121] The preparation method of the surface sizing agent is:

[0122] Add 1 / 3 of water to the formulated amount of amphoteric surface cassava starch in a surface glue cooking tank, stir evenly, ventilate, and heat to 96°C, keep warm for 20 minutes, move to a surface glue dilution barrel, cool to 69°C, and mix with chitosan and 2 / 3 of water to form a surface sizing agent.

[0123] In the pulping machine process, two DD720 double-disc refiners were used in series for pulping, both of which adopted broom fin-type refiners, with a beating degree of 37°SR and a wet weight of 3.5g.

[0124] The amount of cationic starch added is 10 kg / ton of pulp, the amount of AKD added is 17 kg / ton of pulp, the amount of silica sol added is 3.5 kg / ton of pulp, and the amount of wet strength agent added is 18 kg / ton of pulp.

[0125] The standards for the surface sizing agent are 8.7% solid content, 14 MPa.s viscosity, 6.1 pH and 70°C temperature.

[0126] The paper machine operating parameters are:

[0127] (1) Machine speed 245m / min, pulp-to-web speed ratio 0.9;

[0128] (2) The steam pressure of the large cylinder is 530KPa, and the pressure of the double rollers is set to 105KN / m;

[0129] (3) Film transfer sizing machine control parameters;

[0130] Metering rod model and pressure;

[0131] Front metering rod V24, line pressure 30KN / m;

[0132] The reverse metering rod is V24, with a line pressure of 30KN / m;

[0133] The paper pick-up amount of the new surface sizing agent is 1.3g / ㎡ on the front side and 1.3g / ㎡ on the back side;

[0134] The paper dryness of the paper entering the film transfer sizing machine is 94%, and the paper dryness of the paper leaving the film transfer sizing machine is 78%.

[0135] The test results are shown in Table 1.

[0136] Comparative Example 2

[0137] The production process is as follows: pulp board → chain conveyor → pulper → unloading tank → pulper → pulping tank → pre-pulping tank → pulping pump → pressure screen → head box → wire section → pressing section → large cylinder → sizing machine → cylinder assembly → calender → winding section → rewinding → packaging and storage;

[0138] The formula of the surface sizing agent is composed of the following raw materials in parts by weight:

[0139] Amphoteric surface tapioca starch 98 parts;

[0140] Chitosan 8 parts;

[0141] Water 1190 parts;

[0142] In the pulp board process, the pulp board ratio is 80% bleached kraft hardwood pulp and 20% bleached kraft softwood pulp. When pulping, 0.7 kg / ton of caustic soda is added to adjust the pH to 7.7.

[0143] The preparation method of the surface sizing agent is:

[0144] Add 1 / 3 of water to the formulated amount of amphoteric surface cassava starch in a surface glue cooking tank, stir evenly, ventilate, and heat to 98°C, keep warm for 18 minutes, move to a surface glue dilution barrel, cool to 69°C, and mix with chitosan and 2 / 3 of water to form a surface sizing agent.

[0145] In the pulping machine process, two DD720 double-disc refiners were used in series for pulping, both of which adopted broom fin-type refiners, with a beating degree of 38°SR and a wet weight of 4.0g.

[0146] The amount of cationic starch added is 12 kg / ton of pulp, the amount of AKD added is 19 kg / ton of pulp, the amount of silica sol added is 3.8 kg / ton of pulp, and the amount of wet strength agent added is 20 kg / ton of pulp.

[0147] The standards for the surface sizing agent are 8.7% solid content, 14 MPa.s viscosity, 6 ph and 70°C temperature.

[0148] The paper machine operating parameters are:

[0149] (1) Machine speed 240m / min, pulp-to-web speed ratio 0.9;

[0150] (2) The steam pressure of the large cylinder is 520KPa, and the pressure of the double rollers is set at 110KN / m;

[0151] (3) Film transfer sizing machine control parameters;

[0152] Metering rod model and pressure;

[0153] Front metering rod V24, line pressure 30KN / m;

[0154] The reverse metering rod is V24, with a line pressure of 30KN / m;

[0155] The paper pick-up amount of the new surface sizing agent is 1.25g / ㎡ on the front side and 1.35g / ㎡ on the back side;

[0156] The paper dryness of the paper entering the film transfer sizing machine is 96%, and the paper dryness of the paper leaving the film transfer sizing machine is 78%.

[0157] The test results are shown in Table 1.

[0158] Table 1 Test results of various embodiments and comparative examples.

[0159]

[0160] Comparative Example 1 uses 10% bleached kraft softwood pulp, and Comparative Example 2 uses 20% bleached kraft hardwood pulp. From the indicators, although the paper strength is improved, the stiffness exceeds the standard of 0.8 mN·m. When the customer uses it, the tube breaks during the bending process, so softwood pulp cannot be used.

Claims

1. A production process for U-shaped straw base paper, characterized in that: Including pulp board → chain conveyor → pulper → unloading tank → pulper → pulping tank → pre-pulping tank → pulping pump → pressure screen → head box → wire section → pressing section → large cylinder → sizing machine → cylinder assembly → calender → winding section → rewinding → packaging and storage; In the sizing machine process, a surface sizing agent is added, and the formula of the surface sizing agent is composed of the following raw materials in parts by weight: 90-100 parts of amphoteric surface tapioca starch; Chitosan 6-10 parts; 1159-1219 parts of water; In the pulping process, the pulping ratio is 100% bleached kraft hardwood pulp, 0.5-1 kg / ton of caustic soda is added during pulping, and the pH is adjusted to 7.5-8.0; The production process of the U-shaped straw base paper and the preparation method of the surface sizing agent are as follows: Add 1 / 3 of water to the formulated amount of amphoteric surface cassava starch in a surface glue cooking tank, stir evenly, ventilate, heat to 90-95°C, keep warm for 15-20 minutes, move to a surface glue dilution barrel, cool to 65-70°C, mix with chitosan and 2 / 3 of water to form a surface sizing agent; The bleached kraft hardwood pulp is bleached kraft eucalyptus hardwood pulp; In the pulping process, two DD720 double-disc refiners are used in series for pulping, both of which use broom fin-type refiners, with a beating degree of 35-38°SR and a wet weight of 2.0-3.0g; The process flow of the forestock pool → flushing pump → pressure screen → headbox → wire section → press section → large cylinder → sizing machine → cylinder assembly → calender → winding section is realized by a paper machine, and the operating parameters of the paper machine are: (1) Machine speed 200-250m / min, pulp-to-net speed ratio 0.9; (2) The steam pressure of the large cylinder is 500-550 kPa, and the pressure of the double rollers is set at 100-110 kN / m; (3) Film transfer sizing machine control parameters; Metering rod model and pressure; Front metering rod V24, line pressure 30kN / m; Reverse metering rod V24, line pressure 30kN / m; The paper pick-up amount of the new surface sizing agent is 1-1.5g / ㎡ on the front side and 1-1.5g / ㎡ on the back side; The dryness of the finished paper from the film transfer sizing machine is ≥92%, and the dryness of the finished paper from the film transfer sizing machine is ≥75%.

2. The production process of U-shaped straw base paper according to claim 1, characterized in that: Cationic starch is added between the pulping tank and the forestock tank, wet strength agent and AKD are added in sequence between the forestock tank and the pulping pump, and silica sol is added between the pressure screen and the headbox.

3. The production process of U-shaped straw base paper according to claim 1, characterized in that: The amount of cationic starch added is 10-12 kg / ton of pulp, the amount of AKD added is 15-20 kg / ton of pulp, the amount of silica sol added is 2-4 kg / ton of pulp, and the amount of wet strength agent added is 15-18 kg / ton of pulp.

4. The production process of U-shaped straw base paper according to claim 1, characterized in that: The surface sizing agent has a solid content of 7-9%, a viscosity of 5-15 mPa·s, a pH of 5-6, and a temperature of 65-70°C.

Citation Information

Patent Citations

  • Large-scale production method of beveled U-shaped paper straw

    CN112297514A

  • Manufacture method of straw raw paper

    CN109736128A

  • Manufacturing method of beverage drinking straw paper

    CN110318302A