A weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries and a method for preparing the same
Preparing porous carbon nanospheres by sintering biological waste and depositing graphene networks, combined with thermosetting resin and graphene oxide coating, solves the problems of conductivity and mechanical strength of bipolar plates in flow batteries, and realizes low-cost and efficient liquid flow batteries. Flow battery materials.
Patent Information
- Application Number
- CN202311397343.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-10-26
AI Technical Summary
Existing redox flow battery bipolar plate materials have poor electrical conductivity, low mechanical strength, and high cost, resulting in short cycle life and self-discharge problems, and there is a lack of effective highly conductive material solutions.
Porous carbon nanospheres are prepared from biological waste through high-temperature sintering, and a three-dimensional graphene network is deposited on the surface, combined with thermosetting resin filling and graphene oxide slurry thermal spray coating, to form a weldable bipolar with high conductivity and high mechanical strength. board material.
A flow battery bipolar plate with high conductivity, good mechanical strength and low cost is realized, which is suitable for acidic, alkaline and neutral flow batteries, extending the cycle life of the battery and reducing the preparation cost.
Smart Images

Figure CN117457932B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of liquid flow batteries, and relates to a weldable conductive bipolar plate for acidic, alkaline and neutral liquid flow batteries and a preparation method thereof. Background Art
[0002] Due to its advantages of separation of energy and power, long cycle life, low cost, less maintenance time, high safety, and environmental protection, redox flow batteries are one of the first choices for large-scale energy storage technology. Its basic structure includes core key materials such as electrodes, bipolar plates, and ion exchange membranes, as well as auxiliary components such as sealing structures and electrode frames. Among them, bipolar plates, as one of the key materials of flow batteries, play a vital role in improving the energy efficiency and voltage efficiency of batteries. With the rapid increase in the output value of redox flow batteries, the demand for bipolar plate materials is bound to gradually increase.
[0003] Problems such as poor conductivity of bipolar plates and increased surface resistance of bipolar plates caused by electrochemical corrosion will affect the cycle life, power density, and energy conversion efficiency of redox flow batteries. Currently, the most widely used direct way to improve the conductivity of bipolar plates is to increase the content of conductive agents in the bipolar plates. However, excessive conductive agents will significantly reduce the flexibility of the bipolar plates, reduce their compressive and erosion resistance, and cause the bipolar plates to rupture, thereby leading to severe self-discharge of the battery. In addition, the preparation cost is high, resulting in the lack of mature bipolar plate materials for redox flow batteries at this stage.
[0004] Prior art 1 (CN 113571715 A) soaks carbon fiber in lignin slurry and then sintering it. The lignin turns into carbon particles and adheres to the carbon fiber to enhance the electrochemical properties of the carbon fiber.
[0005] Up to now, there is still no suitable method to solve the above key problems. It is urgent to develop a bipolar plate material for liquid flow batteries that can effectively prepare high conductivity, which will make an important contribution to the large-scale development of redox flow batteries. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a weldable conductive bipolar plate for acidic, alkaline and neutral liquid flow batteries, which has the advantages of good conductivity, high mechanical strength, good air tightness, strong corrosion resistance, thin thickness and low preparation cost, and solves the problems existing in the prior art.
[0007] Another object of the present invention is to provide a method for preparing weldable conductive bipolar plates for acidic, alkaline and neutral liquid flow batteries.
[0008] The technical solution adopted by the present invention is a weldable conductive bipolar plate for acidic, alkaline and neutral liquid flow batteries, including a main body of the weldable conductive bipolar plate, wherein the main body includes porous carbon nano-microspheres obtained by high-temperature sintering using biological waste as raw materials, and a three-dimensional graphene network is stably deposited on the surface of the porous carbon nano-microspheres; and a graphene oxide slurry coating is thermally sprayed on the surface of the main body.
[0009] Furthermore, the main body thickness of the weldable conductive bipolar plate is 0.6-1.2 mm, and the thickness of the graphene oxide coating is 5-20% of the main body thickness.
[0010] A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries comprises the following steps:
[0011] Step 1, treating the biological waste into slurry;
[0012] Step 2, sintering the slurry at high temperature to obtain porous carbon nanospheres, and stably depositing a three-dimensional graphene network on the surface by chemical vapor deposition to obtain graphene-porous carbon nanospheres;
[0013] Step 3, obtaining a graphene-porous carbon composite resin layer by filling and molding with a thermosetting resin;
[0014] Step 4, evenly thermally spraying the graphene oxide slurry on both sides of the graphene-porous carbon composite resin layer to form a surface coating with high hydrophilicity and electrochemical activity, and molding after the coating is cooled.
[0015] Furthermore, after step 4, the step further includes: placing the prepared bipolar plate in a tubular furnace, continuously introducing an inert gas, starting a plasma power of 500-800w, introducing a volume flow rate of 200-300sccm of carbon dioxide and a volume flow rate of 400-600sccm of hydrogen, the introduction time is 5-25min, and then naturally cooling to room temperature, and depositing graphene-porous carbon nanospheres on the graphene oxide coating.
[0016] Furthermore, in step 1, the biological waste is a mixture of one or more of lignin, lotus seed shells, peanut shells or bamboo shoot shells in equal proportions.
[0017] Furthermore, in step 1, the method for treating biological waste is:
[0018] The biological waste is washed with deionized water for 10-15 times, immersed in an ethanol solution for ultrasonic treatment for 30-50s, and then dried in a forced air drying oven at a drying temperature of 40-60°C and a drying time of 6-8h; the dried biological waste is mixed with a sucrose solution with a mass fraction of 18-22% in a mass volume ratio of 0.8-1.2g:1ml, and fully stirred to form a slurry; the formed slurry is placed in a ball mill container with a ball-to-material ratio of 1.5-2.5:1, and ball milled at a rotation speed of 400-600r / min for 20-30min.
[0019] Furthermore, the step 2 comprises the following steps:
[0020] The slurry of biological waste is placed in a tubular furnace, and an inert gas is continuously introduced. The temperature is raised to 1200-1500°C and kept constant for 20-30 minutes. During the constant temperature process, carbon dioxide with a volume flow rate of 200-300sccm and hydrogen with a volume flow rate of 400-600sccm are introduced for 5-15 minutes. The furnace is then naturally cooled to room temperature to obtain graphene-porous carbon nanospheres.
[0021] Further, the step 3 comprises the following steps:
[0022] Acetone, a curing agent and graphene-porous carbon nanospheres are added to a thermosetting resin to obtain two portions of liquid graphene-porous carbon composite resins with different contents of graphene-porous carbon nanospheres, wherein the volume ratios of the thermosetting resin, acetone, the curing agent and the graphene-porous carbon nanospheres are 1:20%-30%:1.0-1.2%:30-50% and 1:20%-30%:1.0-1.2%:60-90%;
[0023] The obtained liquid graphene-porous carbon composite resin with a higher content of graphene-porous carbon nanospheres is added to the center of the mold, and another portion of liquid graphene-porous carbon composite resin is added to the edge of the mold, and molded to obtain a graphene-porous carbon composite resin layer; wherein the molding process parameters are: curing at room temperature for 4-6 hours, then applying a pressure of 0.5-1.0 kPa, and curing for 12-24 hours.
[0024] Furthermore, in step 4, the preparation of graphene oxide slurry: plasma-treating commercial graphene oxide with a particle size of 1-3 μm, and then adding it to a dispersion solvent, the mass volume ratio of graphene oxide to dispersion solvent is 100-150 g: 100-200 mL, and ultrasonicating for 20-40 min to obtain graphene oxide slurry;
[0025] The preparation of the dispersion solvent is as follows: ethanol, DMF, NMP or THF and deionized water are mixed at a volume ratio of 1.5-2.5:1.
[0026] Furthermore, in the step 4, uniform thermal spraying is performed by a spray gun, and the spraying temperature is 60-80° C.; the molding time is 6-8 hours, and the molding pressure is 0.5-1.0 kPa.
[0027] The beneficial effects of the present invention are:
[0028] The present invention obtains porous carbon nano-microspheres by pretreating and carbonizing biological waste; the conductivity can be further improved by depositing a three-dimensional graphene network on the surface of the porous carbon nano-microspheres; the stability of the three-dimensional graphene network can be improved by curing the graphene network structure with a thermosetting resin; the mechanical properties of the resin layer can be changed by adjusting the content of the conductive material in the thermosetting resin, so that the edges of the bipolar plate material can be welded; the structural purity of the graphene oxide powder can be significantly improved by plasma treatment of the graphene oxide powder, and the wrinkled graphite structure at the edge of the graphene oxide powder can be ensured to be completely oxidized; the uniformity of the coating can be ensured by thermal spraying of the graphene slurry, and compared with the graphene structure, the graphene oxide structure with high purity on the surface coating has better hydrophilicity and electrocatalytic performance, and is more suitable for aqueous liquid flow batteries.
[0029] In the treatment method of the present invention, biological waste is widely available and low in cost, the equipment cost is low in the entire preparation process, the process flow is simple and convenient, and it is easy to expand production in batches, which is conducive to the large-scale production of commercial bipolar plates for liquid flow batteries. At the same time, it realizes the resource recycling of biological waste, which has significant social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 Schematic diagram of the structure of a weldable conductive bipolar plate in an embodiment of the present invention.
[0032] Figure 2 The AC impedance curves of the weldable conductive bipolar plates obtained in Examples 1-4 of the present invention in an acidic vanadium redox flow battery system.
[0033] Figure 3 This is an efficiency diagram of an acidic all-vanadium redox flow battery assembled with weldable conductive bipolar plates obtained in Example 1 of the present invention.
[0034] Figure 4 This is a comparison chart of the efficiency of the neutral iron-sulfur redox flow battery with weldable conductive bipolar plates obtained in Example 2 of the present invention.
[0035] Figure 5 This is a comparison chart of the efficiency of an alkaline zinc-iron redox flow battery assembled with weldable conductive bipolar plates obtained in Example 3 of the present invention.
[0036] Figure 6 This is a comparison chart of the efficiencies of alkaline manganese-sulfur redox flow batteries assembled with weldable conductive bipolar plates obtained in Example 14 and Example 1 of the present invention.
[0037] Figure 7 This is a comparison chart of the efficiencies of alkaline manganese-sulfur redox flow batteries assembled with weldable conductive bipolar plates obtained in Example 15 and Example 2 of the present invention.
[0038] Figure 8 This is a comparison chart of the efficiencies of alkaline manganese-sulfur redox flow batteries assembled with weldable conductive bipolar plates obtained in Example 16 and Example 3 of the present invention.
[0039] Fig. 9 This is a comparison chart of the efficiencies of alkaline manganese-sulfur redox flow batteries assembled with weldable conductive bipolar plates obtained in Examples 4-8 of the present invention.
[0040] Fig.10 It is a comparison chart of the efficiency of the acidic all-vanadium redox flow battery assembled with the weldable conductive bipolar plates obtained in Example 1 of the present invention and Comparative Example 9.
[0041] Fig.11 It is a comparison chart of the efficiency of the acidic all-vanadium redox flow battery assembled with the weldable conductive bipolar plates obtained in Example 1 of the present invention and Comparative Example 10.
[0042] Fig.12 It is a comparison chart of the efficiency of the acidic all-vanadium redox flow battery assembled with the weldable conductive bipolar plates obtained in Example 1 of the present invention and Comparative Example 11.
[0043] Fig.13 This is a comparison chart of the efficiencies of the acidic all-vanadium redox flow batteries assembled with the weldable conductive bipolar plates obtained in Example 1 of the present invention and Comparative Example 12.
[0044] Fig.14 This is an electron microscope image of the weldable conductive bipolar plate obtained in Example 1 of the present invention.
[0045] Fig.15 This is an electron microscope image of the weldable conductive bipolar plate obtained in Example 1 of the present invention after assembled battery cycle testing. DETAILED DESCRIPTION
[0046] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0047] The design concept of the present invention is: low-cost biological waste is used as raw material, porous carbon nanospheres are obtained through high-temperature sintering, and a layer of highly conductive three-dimensional graphene network is stably deposited on the surface by chemical vapor deposition, followed by thermosetting resin filling and molding to obtain the main material of weldable conductive bipolar plates, and finally through thermal spraying of graphene oxide slurry to form a surface coating with high hydrophilicity and electrochemical activity, thereby obtaining a graphene composite bipolar plate material for liquid flow batteries with high conductivity, good electrochemical activity and excellent stability. The results of cyclic voltammetry curves, AC impedance spectra and constant current charge and discharge tests show that the bipolar plate material synthesized by this method has excellent conductivity and electrocatalytic ability, and is suitable for the application requirements of liquid flow batteries.
[0048] The weldable conductive bipolar plate material for liquid flow batteries prepared by the present invention has the advantages of low cost, high conductivity, good stability, etc., and is widely applicable to many liquid flow battery systems. In the specific embodiments of the present invention, only three systems, namely, all-vanadium redox liquid flow battery, iron-sulfur redox liquid flow battery (Fe-S), and zinc-iron redox liquid flow battery (Zn-Fe), are selected as partial embodiments. All other redox liquid flow battery system bipolar plate materials prepared by this method belong to the protection scope of the present invention.
[0049] A weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries prepared in an embodiment of the present invention, such as Figure 1 As shown, it includes a main body of a weldable conductive bipolar plate, the main body includes porous carbon nanospheres obtained by high-temperature sintering using biological waste as raw materials, and a three-dimensional graphene network is stably deposited on the surface of the porous carbon nanospheres; and a graphene oxide slurry coating is thermally sprayed on the surface of the main body. Among them, the thickness of the main body of the weldable conductive bipolar plate can be adjusted according to the structural requirements of the liquid flow battery, generally 0.6-1.2mm, and the thickness of the graphene oxide coating is 5-20% of the thickness of the main body.
[0050] Example 1
[0051] A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries comprises the following steps:
[0052] (1) The lignin was washed 12 times with deionized water, immersed in an ethanol solution for 40 seconds, and then dried in a forced air drying oven at a temperature of 50°C for 7 hours. The dried lignin was mixed with a 20% by mass sucrose solution at a mass volume ratio of 1 g:1 ml and stirred thoroughly to form a slurry. The formed slurry was placed in a ball mill container with a ball-to-material ratio of 2:1 and ball milled at a speed of 500 r / min for 25 minutes.
[0053] (2) The slurry of step (1) is placed in a tubular furnace, and an inert gas is continuously introduced, and the temperature is raised to 1300°C, and the temperature is kept constant for 25 minutes. During the constant temperature process, carbon dioxide with a volume flow rate of 200sccm and hydrogen with a volume flow rate of 400sccm are introduced for a time of 10 minutes, and then naturally cooled to room temperature to obtain graphene-porous carbon nanospheres. Using high-purity carbon dioxide as a carbon source, graphene nanosheets are grown on the surface through high-temperature cracking. The nanosheets are larger in size and have better conductivity. The nanosheets are intertwined with each other to form a three-dimensional network structure.
[0054] (3) Add acetone in an amount of 25% by volume of the thermosetting resin (epoxy resin or polyester resin), add NL curing agent (a universal curing agent whose main component is phenolic resin) in an amount of 1.1% by volume of the thermosetting resin, add the graphene-porous carbon nanospheres prepared in step (2), wherein the volume of the graphene-porous carbon nanospheres is 40% or 80% of the volume of the thermosetting resin, respectively, and stir evenly at room temperature to obtain two portions of liquid graphene-porous carbon composite resins having different contents of graphene-porous carbon nanospheres.
[0055] The liquid graphene-porous carbon composite resin with a volume content of 80% of the volume of the thermosetting resin was slowly added to the center of the mold, and the liquid graphene-porous carbon composite resin with a volume content of 40% of the volume of the thermosetting resin was slowly added to the edge of the mold and cured at room temperature for 5 hours. Subsequently, a pressure of 0.8 kPa was applied and cured for 18 hours to obtain a graphene-porous carbon composite resin layer.
[0056] (4) Place 120g of commercial graphene oxide powder with a particle size of 1-3μm in a muffle furnace and keep it at 100℃ for 10h. After natural cooling, evenly spread the graphene oxide powder in a container, introduce oxygen with a volume flow rate of 18sccm, turn on the plasma switch, adjust the plasma power to 150w, and plasma treat for 4min at room temperature (18-22℃). Then take out the graphene oxide powder and stir it thoroughly, evenly spread it again, and repeat the plasma treatment 3-4 times. Mix ethanol, DMF, NMP or THF with deionized water in a volume ratio of 2:1 to form a dispersion solvent, then add the plasma-treated graphene oxide into 150mL of the dispersion solvent, and perform rod ultrasonication for 30min to obtain a graphene oxide slurry. The obtained graphene slurry was placed in a spray gun, the spraying temperature was set to 70°C, and it was evenly thermally sprayed on both sides of the graphene-porous carbon composite resin layer obtained in step (3). After the coating was cooled, it was molded for 7 hours at a molding pressure of 0.8 kPa.
[0057] The conductive material of the embodiment of the present invention is a combination of a porous carbon material with larger particles and a three-dimensional graphene structure, which has high conductivity. Therefore, the content of the conductive material in the composite process can be significantly reduced, the toughness of the graphite plate can be improved, and the cost can be reduced. In addition, the composite carbon material as a conductive material has strong acid and alkali resistance. Figure 2 As shown, the contact resistance of sample 1 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 0.49Ω, and the charge transfer resistance is 0.71Ω. Figure 3 As shown in the figure, the voltage efficiency of the acidic vanadium flow battery assembled with sample 1 is 88.3%, the energy efficiency is 87.4%, and it can be stably cycled for more than 100 times, indicating that sample 1 meets the application requirements of bipolar plate materials for flow batteries and can promote the industrial development of flow batteries. The microstructure of sample 1 before and after cycling is shown in the figure. Figure 14-15 As shown, from Fig.14 It can be seen that the graphene oxide coating on the surface is smooth and there are no obvious holes; after a long period of battery cycle testing, its surface microscopic morphology has not changed significantly ( Fig.15 ), which fully verifies the electrochemical stability and corrosion resistance of its structure.
[0058] Example 2
[0059] A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries comprises the following steps:
[0060] (1) The lotus seed shell was washed 10 times with deionized water, immersed in an ethanol solution for 50 seconds, and then dried in a forced air drying oven at 60°C for 6 hours. The dried lotus seed shell was mixed with 18% sucrose solution at a mass volume ratio of 0.8 g:1 ml and stirred thoroughly to form a slurry. The formed slurry was placed in a ball mill container with a ball-to-material ratio of 2.5:1 and ball milled at a speed of 400 r / min for 30 min.
[0061] (2) The slurry of step (1) is placed in a tubular furnace, and an inert gas is continuously introduced, and the temperature is raised to 1500°C, and the temperature is kept constant for 20 minutes. During the constant temperature process, carbon dioxide with a volume flow rate of 240sccm and hydrogen with a volume flow rate of 600sccm are introduced for 7 minutes, and then naturally cooled to room temperature to obtain graphene-porous carbon nanospheres. Using high-purity carbon dioxide as a carbon source, graphene nanosheets are grown on the surface through high-temperature cracking. The nanosheets are larger in size and have better conductivity. The nanosheets are intertwined to form a three-dimensional network structure.
[0062] (3) Add acetone in an amount of 30% by volume of the thermosetting resin (epoxy resin or polyester resin), add NL curing agent (a universal curing agent whose main component is phenolic resin) in an amount of 1.0% by volume of the thermosetting resin, add the graphene-porous carbon nanospheres prepared in step (2), wherein the volume of the graphene-porous carbon nanospheres is 30% or 60% of the volume of the thermosetting resin, respectively, and stir evenly at room temperature to obtain two portions of liquid graphene-porous carbon composite resins having different contents of graphene-porous carbon nanospheres.
[0063] The liquid graphene-porous carbon composite resin with a volume content of 60% of the volume of the thermosetting resin was slowly added to the center of the mold, and the liquid graphene-porous carbon composite resin with a volume content of 30% of the volume of the thermosetting resin was slowly added to the edge of the mold, and cured at room temperature for 4 hours, and then a pressure of 1.0 kPa was applied and cured for 24 hours to obtain a graphene-porous carbon composite resin layer.
[0064] (4) Place 100g of commercial graphene oxide powder with a particle size of 1-3μm in a muffle furnace and keep it at 100℃ for 8h. After natural cooling, evenly spread the graphene oxide powder in a container, introduce oxygen with a volume flow rate of 15sccm, turn on the plasma switch, adjust the plasma power to 100w, and plasma treat for 5min at room temperature (18-22℃). Then take out the graphene oxide powder and stir it thoroughly, evenly spread it again, and repeat the plasma treatment 3-4 times. Mix ethanol, DMF, NMP or THF with deionized water in a volume ratio of 1.5:1 to form a dispersion solvent, then add the plasma-treated graphene oxide into 180mL of the dispersion solvent, and perform rod ultrasonication for 40min to obtain a graphene oxide slurry. The obtained graphene slurry was placed in a spray gun, the spraying temperature was set to 60°C, and it was evenly thermally sprayed on both sides of the graphene-porous carbon composite resin layer obtained in step (3). After the coating was cooled, it was molded for 8 hours at a molding pressure of 1.0 kPa; and sample 2 was obtained.
[0065] like Figure 2 As shown, the contact resistance of sample 2 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 0.55Ω, and the charge transfer resistance is 0.83Ω. Figure 4 As shown, the neutral iron-sulfur liquid flow battery assembled using sample 2 has a voltage efficiency of 87.2%, an energy efficiency of 86.6%, and can be stably cycled for more than 100 times, indicating that sample 2 is adapted to the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries.
[0066] Example 3
[0067] A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries comprises the following steps:
[0068] (1) The peanut shells were washed 15 times with deionized water, immersed in an ethanol solution for 30 seconds, and then dried in a forced air drying oven at 40°C for 8 hours. The dried peanut shells were mixed with a 22% sucrose solution at a mass volume ratio of 1.2 g:1 ml and stirred thoroughly to form a slurry. The formed slurry was placed in a ball mill container with a ball-to-material ratio of 1.5:1, and ball milled at a speed of 600 r / min for 20 minutes.
[0069] (2) The slurry of step (1) is placed in a tubular furnace, and an inert gas is continuously introduced, and the temperature is raised to 1200°C, and the temperature is kept constant for 30 minutes. During the constant temperature process, carbon dioxide with a volume flow rate of 300sccm and hydrogen with a volume flow rate of 500sccm are introduced for 8 minutes, and then naturally cooled to room temperature to obtain graphene-porous carbon nanospheres. Using high-purity carbon dioxide as a carbon source, graphene nanosheets are grown on the surface through high-temperature cracking. The nanosheets are larger in size and have better conductivity. The nanosheets are intertwined to form a three-dimensional network structure.
[0070] (3) Add acetone in an amount of 20% by volume of the thermosetting resin (epoxy resin or polyester resin), add NL curing agent (a universal curing agent whose main component is phenolic resin) in an amount of 1.2% by volume of the thermosetting resin, add the graphene-porous carbon nanospheres prepared in step (2), wherein the volume of the graphene-porous carbon nanospheres is 50% or 90% of the volume of the thermosetting resin, respectively, and stir evenly at room temperature to obtain two portions of liquid graphene-porous carbon composite resins having different contents of graphene-porous carbon nanospheres.
[0071] The liquid graphene-porous carbon composite resin with a volume content of 90% of the volume of the thermosetting resin was slowly added to the center of the mold, and the liquid graphene-porous carbon composite resin with a volume content of 50% of the volume of the thermosetting resin was slowly added to the edge of the mold and cured at room temperature for 6 hours. Subsequently, a pressure of 0.5 kPa was applied and cured for 12 hours to obtain a graphene-porous carbon composite resin layer.
[0072] (4) Place 150g of commercial graphene oxide powder with a particle size of 1-3μm in a muffle furnace and keep it at 100℃ for 12h. After natural cooling, evenly spread the graphene oxide powder in a container, introduce oxygen with a volume flow rate of 20sccm, turn on the plasma switch, adjust the plasma power to 200w, and plasma treat for 3min at room temperature (18-22℃). Then take out the graphene oxide powder and stir it thoroughly, evenly spread it again, and repeat the plasma treatment 3-4 times. Ethanol, DMF, NMP or THF and deionized water are mixed in a volume ratio of 2.5:1 to form a dispersion solvent. Then, add the plasma-treated graphene oxide into 130mL of the dispersion solvent and perform rod ultrasonication for 20min to obtain a graphene oxide slurry. The obtained graphene slurry was placed in a spray gun, the spraying temperature was set to 80°C, and it was evenly thermally sprayed on both sides of the graphene-porous carbon composite resin layer obtained in step (3). After the coating was cooled, it was molded for 6 hours at a molding pressure of 0.5 kPa; and sample 3 was obtained.
[0073] like Figure 2 As shown, the contact resistance of sample 3 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 0.58Ω, and the charge transfer resistance is 0.81Ω. Figure 5 As shown, the alkaline zinc-iron flow battery assembled using sample 3 has a voltage efficiency of 90.1% and an energy efficiency of 89.3%, and can be stably cycled for more than 100 times, indicating that sample 3 is adapted to the application requirements of bipolar plate materials for flow batteries and can promote the industrial development of flow batteries.
[0074] Example 4
[0075] Except that the lignin used in (1) is bamboo shoot shell (bamboo shoots), the rest is the same as Example 1, and Sample 4 is obtained.
[0076] like Figure 2 As shown, the contact resistance of sample 4 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 0.59Ω, and the charge transfer resistance is 0.79Ω. The voltage efficiency of the acidic vanadium liquid flow battery assembled with sample 4 is 84.1%, the energy efficiency is 82.7%, and it can be stably cycled for more than 100 times, indicating that sample 4 meets the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries.
[0077] Example 5
[0078] Except that the biological waste used in (1) is lignin + lotus seeds + peanut shells, and the weight ratio is 1:1:1; the rest is the same as Example 1.
[0079] At room temperature, the contact resistance of sample 5 prepared in this embodiment in the acidic vanadium liquid flow battery system was measured to be 0.55Ω, and the charge transfer resistance was 0.85Ω. The voltage efficiency of the acidic vanadium liquid flow battery assembled using sample 5 was 84.9%, and the energy efficiency was 83.1%, and it could be stably cycled for more than 100 times, indicating that sample 5 is adapted to the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries.
[0080] Example 6
[0081] Except that the biological waste used in (1) is lotus seed shell + peanut shell + bamboo shoot shell, and the weight ratio is 1:1:1; the rest is the same as Example 1.
[0082] The contact resistance of sample 6 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 0.50Ω, the charge transfer resistance of sample 6 is 0.71Ω, the voltage efficiency of the acidic vanadium liquid flow battery assembled using sample 6 is 85.5%, the energy efficiency is 83.7%, and it can be stably cycled for more than 100 times, indicating that sample 6 is adapted to the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries.
[0083] Example 7
[0084] Except that the biological waste used in (1) is lignin + lotus seed shell + bamboo shoot shell, and the weight ratio is 1:1:1; the rest is the same as Example 1.
[0085] The contact resistance of sample 7 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 0.49Ω, the charge transfer resistance of sample 7 is 0.72Ω, the voltage efficiency of the acidic vanadium liquid flow battery assembled using sample 7 is 84.6%, the energy efficiency is 83.0%, and it can be stably cycled for more than 100 times, indicating that sample 7 is adapted to the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries.
[0086] Example 8
[0087] Except that the biological waste used in (1) is lignin + peanut shell + bamboo shoot shell, and the weight ratio is 1:1:1; the rest is the same as Example 1.
[0088] The contact resistance of sample 8 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 0.50Ω, and the charge transfer resistance is 0.70Ω. The voltage efficiency of the acidic vanadium liquid flow battery assembled using sample 8 is 83.7%, and the energy efficiency is 82.8%. It can be stably cycled for more than 100 times, indicating that sample 8 is suitable for the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries. Fig. 9 shown.
[0089] Example 9
[0090] Except that the biological waste used in (1) is lignin + lotus seed shell + peanut shell + bamboo shoot shell, and the weight ratio is 1:1:1:1; the rest is the same as Example 1.
[0091] At room temperature, the contact resistance of sample 9 prepared in this embodiment in the acidic vanadium liquid flow battery system was measured to be 0.50Ω, and the charge transfer resistance was 0.71Ω. The voltage efficiency of the acidic vanadium liquid flow battery assembled using sample 9 was 85.1%, and the energy efficiency was 83.8%, and it could be stably cycled for more than 100 times, indicating that sample 9 is adapted to the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries.
[0092] Example 10
[0093] Except that the time for introducing carbon dioxide and hydrogen in (2) is 5 min, the rest is the same as Example 1.
[0094] At room temperature, the contact resistance of sample 10 prepared in this embodiment in the acidic vanadium liquid flow battery system was measured to be 0.49Ω, and the charge transfer resistance was 0.72Ω. The voltage efficiency of the acidic vanadium liquid flow battery assembled using sample 10 was 84.6%, and the energy efficiency was 82.8%, and it could be stably cycled for more than 100 times, indicating that sample 10 is adapted to the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries.
[0095] Embodiment 11
[0096] Except that the time for introducing carbon dioxide and hydrogen in (2) is 15 min, the rest is the same as Example 1.
[0097] The contact resistance of sample 11 prepared in this embodiment in the acidic vanadium liquid flow battery system measured at room temperature is 0.52Ω, the charge transfer resistance of sample 11 is 0.71Ω, the voltage efficiency of the acidic vanadium liquid flow battery assembled using sample 11 is 83.8%, the energy efficiency is 81.9%, and it can be stably cycled for more than 100 times, indicating that sample 11 is adapted to the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries.
[0098] Example 12
[0099] Except that the volume of the dispersion solvent in (4) is 100 mL, the rest is the same as Example 1.
[0100] At room temperature, the contact resistance of sample 12 prepared in this embodiment in the acidic vanadium liquid flow battery system was measured to be 0.49Ω, and the charge transfer resistance was 0.74Ω. The voltage efficiency of the acidic vanadium liquid flow battery assembled using sample 12 was 85.5%, and the energy efficiency was 83.7%, and it could be stably cycled for more than 100 times, indicating that sample 12 is adapted to the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries.
[0101] Embodiment 13
[0102] Except that the volume of the dispersion solvent in (4) is 200 mL, the rest is the same as Example 1.
[0103] The contact resistance of existing bipolar plate materials is 0.5-1.5Ω, and the charge transfer resistance varies greatly, with some reaching tens of ohms. At room temperature, the contact resistance of sample 13 prepared in this embodiment in the acidic vanadium liquid flow battery system is measured to be 0.52Ω, and the charge transfer resistance is 0.72Ω. The voltage efficiency of the acidic vanadium liquid flow battery assembled using sample 13 is 82.7%, and the energy efficiency is 80.2%, and it can be stably cycled for more than 100 times, indicating that sample 13 is adapted to the application requirements of liquid flow battery bipolar plate materials and can promote the industrial development of liquid flow batteries.
[0104] The contact resistance mainly depends on the conductivity and wettability of the material itself. The conductivity of the bipolar plate mainly depends on the internal carbon content. The higher the carbon content, the better the conductivity, but the wettability will decrease, so a balance must be achieved. The charge transfer resistance will be affected by the catalytic activity of the material. Too high resistance will hinder the transmission of electrons, the battery polarization will be too large, and the performance will decrease.
[0105] Embodiment 14
[0106] The bipolar plate material of Example 1 was placed in a tubular furnace, inert gas was continuously introduced, the plasma power was turned on to 800w, carbon dioxide with a volume flow rate of 200sccm and hydrogen with a volume flow rate of 400sccm were introduced for 25min, and then naturally cooled to room temperature to obtain a corrosion-resistant bipolar plate material.
[0107] At room temperature, the contact resistance of sample 14 prepared in this embodiment in the alkaline manganese-sulfur-based flow battery system was measured to be 0.41Ω, and the charge transfer resistance was 0.65Ω, while the contact resistance of sample 1 in the alkaline manganese-sulfur-based flow battery system was 0.58Ω, and the charge transfer resistance was 0.79Ω. Figure 6 As shown, the voltage efficiency of the alkaline manganese-sulfur flow battery assembled using sample 14 is 87.8%, and the energy efficiency is 86.4%, indicating that sample 14 is suitable for the high corrosion environment of the manganese-sulfur flow battery system and can promote the industrial development of flow batteries.
[0108] Embodiment 15
[0109] The bipolar plate material of Example 1 was placed in a tubular furnace, inert gas was continuously introduced, the plasma power was turned on to 500w, carbon dioxide with a volume flow rate of 300sccm and hydrogen with a volume flow rate of 600sccm were introduced for 5min, and then naturally cooled to room temperature to obtain a corrosion-resistant bipolar plate material.
[0110] The contact resistance of sample 15 prepared in this embodiment in the alkaline manganese-sulfur-based flow battery system was measured at room temperature to be 0.44Ω, and the charge transfer resistance was 0.67Ω. Figure 7 As shown, the alkaline manganese-sulfur flow battery assembled using sample 15 has a voltage efficiency of 85.4% and an energy efficiency of 83.7%, which is suitable for the high corrosion environment of the manganese-sulfur flow battery system and can promote the industrial development of flow batteries.
[0111] Example 16
[0112] The bipolar plate material of Example 1 was placed in a tubular furnace, inert gas was continuously introduced, the plasma power was turned on to 700w, carbon dioxide with a volume flow rate of 150sccm and hydrogen with a volume flow rate of 500sccm were introduced for 15min, and then naturally cooled to room temperature to obtain a corrosion-resistant bipolar plate material.
[0113] The contact resistance of sample 16 prepared in this embodiment in the alkaline manganese-sulfur-based flow battery system was measured at room temperature to be 0.46Ω, and the charge transfer resistance was 0.66Ω. Figure 8 As shown, the alkaline manganese-sulfur flow battery assembled using sample 16 has a voltage efficiency of 85.6% and an energy efficiency of 84.0%, which is suitable for the high corrosion environment of the manganese-sulfur flow battery system and can promote the industrial development of flow batteries.
[0114] The electrolyte of some flow batteries is extremely corrosive and oxidizing, such as high-concentration vanadium electrolyte and permanganate electrolyte, such as zinc-manganese flow battery and manganese-sulfur flow battery. For such electrolytes, a layer of graphene network is deposited on the surface of the graphene oxide coating of the embodiment of the present invention by chemical vapor deposition. Compared with the graphene oxide coating, it has a more ordered carbon structure and better corrosion resistance. Figure 6-9 It can be seen that the alkaline manganese-sulfur flow battery assembled with bipolar plate materials with surface-deposited graphene networks has a more stable energy efficiency, while the energy efficiency of the alkaline manganese-sulfur flow battery assembled using samples 1-8 is only 82.9% at most, and the energy efficiency shows varying degrees of decline and fluctuation, indicating that samples 14-16 with surface-deposited graphene networks are more adaptable to the high corrosion environment of the manganese-sulfur flow battery system.
[0115] Comparative Example 1
[0116] Except for the step of adding 20% sucrose solution in (1), the rest is the same as Example 1.
[0117] The contact resistance in the acidic vanadium liquid flow battery system was measured to be 0.75Ω and the charge transfer resistance was 0.98Ω at room temperature.
[0118] Comparative Example 2
[0119] Except that the mass volume ratio of lignin to 20% sucrose solution in (1) is 0.6 g:1 ml, the rest is the same as that in Example 1.
[0120] The contact resistance in the acidic vanadium liquid flow battery system measured at room temperature was 0.74Ω, and the charge transfer resistance was 0.91Ω.
[0121] Except that the mass volume ratio of lignin to 20% sucrose solution in (1) is 1.4 g:1 ml, the rest is the same as that in Example 1.
[0122] The contact resistance in the acidic vanadium liquid flow battery system measured at room temperature was 0.72Ω, and the charge transfer resistance was 0.88Ω.
[0123] Except that the step of depositing the three-dimensional graphene network structure in (2) is omitted, the rest is the same as Example 1.
[0124] The contact resistance in the acidic vanadium liquid flow battery system measured at room temperature was 0.94Ω, and the charge transfer resistance was 1.88Ω.
[0125] Except that the volume flow rate of carbon dioxide in (2) is 200 sccm and the volume flow rate of hydrogen is 300 sccm, the rest is the same as that of Example 1.
[0126] The contact resistance in the acidic vanadium liquid flow battery system was measured to be 0.67Ω and the charge transfer resistance was 0.90Ω at room temperature.
[0127] Comparative Example 6
[0128] Except that the volume flow rate of carbon dioxide in (2) is 200 sccm and the volume flow rate of hydrogen is 700 sccm, the rest is the same as that of Example 1.
[0129] The contact resistance in the acidic vanadium liquid flow battery system was measured to be 0.65Ω and the charge transfer resistance was 0.98Ω at room temperature.
[0130] Comparative Example 7
[0131] Except that the time for introducing carbon dioxide and hydrogen at constant temperature in (2) is 2 minutes, the rest is the same as Example 1.
[0132] The contact resistance in the acidic vanadium liquid flow battery system was measured to be 0.69Ω and the charge transfer resistance was 0.81Ω at room temperature.
[0133] Comparative Example 8
[0134] Except that the time for introducing carbon dioxide and hydrogen at constant temperature in (2) is 20 minutes, the rest is the same as Example 1.
[0135] The contact resistance in the acidic vanadium liquid flow battery system was measured to be 0.61Ω and the charge transfer resistance was 0.78Ω at room temperature.
[0136] Comparative Example 9
[0137] Except for the step of adding acetone and NL curing agent in (3), the rest is the same as Example 1.
[0138] like Fig.10 As shown, the contact resistance in the acidic vanadium flow battery system was measured to be 0.56Ω and the charge transfer resistance was 0.79Ω at room temperature. The energy efficiency of the assembled acidic all-vanadium redox flow battery was 82.0%, but after 5 cycles, the battery efficiency dropped rapidly and the battery failed.
[0139] Comparative Example 10
[0140] Except for the step of adding acetone in (3), the rest is the same as Example 1.
[0141] like Fig.11 As shown, the contact resistance in the acidic vanadium flow battery system was measured to be 0.60Ω and the charge transfer resistance was 0.81Ω at room temperature. The energy efficiency of the assembled acidic all-vanadium redox flow battery was 80.6%, but after 9 cycles, the battery efficiency dropped rapidly and the battery failed.
[0142] Comparative Example 11
[0143] Except for the step of adding NL curing agent in (3), the rest is the same as Example 1.
[0144] like Fig.12 As shown, the contact resistance in the acidic vanadium flow battery system was measured to be 0.58Ω and the charge transfer resistance was 0.76Ω at room temperature. The energy efficiency of the assembled acidic all-vanadium redox flow battery was 81.2%, but after 5 cycles, the battery efficiency dropped rapidly and the battery failed.
[0145] Comparative Example 12
[0146] Except that the molding step in (3) is omitted, the rest is the same as Example 1.
[0147] like Fig.13 As shown, the contact resistance in the acidic vanadium flow battery system measured at room temperature was 0.76Ω, the charge transfer resistance was 1.36Ω, and the energy efficiency of the assembled acidic all-vanadium redox flow battery was 80.9%. However, after 32 cycles, the battery efficiency dropped rapidly and the battery failed.
[0148] Comparative Example 13
[0149] Except for omitting the step of plasma treatment of commercial graphene oxide in (4), the rest is the same as Example 1.
[0150] The contact resistance in the acidic vanadium liquid flow battery system was measured to be 0.86Ω and the charge transfer resistance was 0.96Ω at room temperature.
[0151] Comparative Example 14
[0152] Except for omitting the step of depositing a three-dimensional graphene network structure in (2) and the step of subjecting commercial graphene oxide to plasma treatment in (4), the rest are the same as in Example 1.
[0153] The contact resistance in the acidic vanadium liquid flow battery system was measured to be 1.05Ω and the charge transfer resistance was 1.47Ω at room temperature.
[0154] The embodiment of the present invention uses purchased graphene oxide powder as a raw material (generally prepared by the Hummer method, with low process cost), and uses a plasma process to optimize only the carbon structure of the graphene oxide powder. The obtained graphene oxide has better conductivity and hydrophilicity, and oxygen-containing functional groups are grafted during the plasma process, thereby improving the electrocatalytic performance of the graphene oxide powder. The weldable conductive bipolar plate prepared by the embodiment of the present invention can be widely used in various systems such as all-vanadium liquid flow batteries, iron-sulfur liquid flow batteries, and zinc-iron liquid flow batteries. The liquid flow battery assembled with weldable conductive bipolar plates has high power density and energy efficiency, excellent rate performance and long cycle performance. The preparation method of the weldable conductive bipolar plate for full liquid flow batteries provided by the present invention is simple and easy to operate, environmentally friendly, low in raw material cost, easy to large-scale industrial production, and can be widely used in the commercialization of various liquid flow battery bipolar plate materials.
[0155] The embodiment of the present invention directly sintered lignin into a porous carbon material, and then in-situ grew graphene nanosheets on its surface. Compared with the prior art 1, the structure of the embodiment of the present invention is more stable and the preparation parameters are easier to control.
[0156] Biowaste includes lignin, lotus seed shells, peanut shells, and bamboo shoot shells. Different types of biowaste have different molecular structures of raw materials and different contents of elements, so the final product performance is different. The ratio of carbon dioxide and hydrogen will affect the pressure of the entire preparation process. The embodiment of the present invention has been verified by a large number of technical solutions that the optimal volume ratio of carbon dioxide and hydrogen should be (0.8-1.2):2. At this time, the obtained graphene sheets have a high number of layers, good growth quality, easy to control morphology and structure, and good conductivity.
[0157] The time of introducing carbon dioxide and hydrogen directly determines the content of graphene. A high content means high conductivity, but too high a content will reduce hydrophilicity, resulting in a larger interfacial energy in the aqueous electrolyte, which will increase resistance. On the other hand, too high a graphene content will make the material brittle and easy to break, so it is necessary to ensure an appropriate graphene content.
[0158] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.
Claims
1. A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries, characterized in that: The following steps are involved: Step 1, treating the biological waste into slurry; Step 2, sintering the slurry at high temperature to obtain porous carbon nanospheres, and stably depositing a three-dimensional graphene network on the surface by chemical vapor deposition to obtain graphene-porous carbon nanospheres; Step 3, obtaining a graphene-porous carbon composite resin layer by filling and molding with a thermosetting resin; Step 4, evenly thermally spraying the graphene oxide slurry on both sides of the graphene-porous carbon composite resin layer to form a surface coating with high hydrophilicity and electrochemical activity, and molding after the coating is cooled.
2. A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries according to claim 1, characterized in that: After step 4, the method further includes: placing the prepared bipolar plate in a tubular furnace, continuously introducing an inert gas, starting a plasma power of 500-800w, introducing carbon dioxide with a volume flow rate of 200-300sccm and hydrogen with a volume flow rate of 400-600sccm, the introduction time is 5-25min, and then naturally cooling to room temperature to deposit graphene-porous carbon nanospheres on the graphene oxide coating.
3. A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries according to claim 1, characterized in that: In step 1, the biological waste is a mixture of one or more of lignin, lotus seed shells, peanut shells or bamboo shoot shells in equal proportions.
4. A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries according to claim 1, characterized in that: In step 1, the method for treating biological waste is: The biological waste is washed with deionized water for 10-15 times, immersed in an ethanol solution for ultrasonic treatment for 30-50s, and then dried in a forced air drying oven at a drying temperature of 40-60°C and a drying time of 6-8h; the dried biological waste is mixed with a sucrose solution with a mass fraction of 18-22% in a mass volume ratio of 0.8-1.2g:1ml, and fully stirred to form a slurry; the formed slurry is placed in a ball mill container with a ball-to-material ratio of 1.5-2.5:1, and ball milled at a rotation speed of 400-600r / min for 20-30min.
5. A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries according to claim 1, characterized in that: The step 2 comprises the following steps: The slurry of biological waste is placed in a tubular furnace, and an inert gas is continuously introduced. The temperature is raised to 1200-1500°C and kept constant for 20-30 minutes. During the constant temperature process, carbon dioxide with a volume flow rate of 200-300sccm and hydrogen with a volume flow rate of 400-600sccm are introduced for 5-15 minutes. The furnace is then naturally cooled to room temperature to obtain graphene-porous carbon nanospheres.
6. A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries according to claim 1, characterized in that: The step 3 comprises the following steps: Acetone, a curing agent and graphene-porous carbon nanospheres are added to a thermosetting resin to obtain two portions of liquid graphene-porous carbon composite resins with different contents of graphene-porous carbon nanospheres, wherein the volume ratios of the thermosetting resin, acetone, the curing agent and the graphene-porous carbon nanospheres are 1:20%-30%:1.0-1.2%:30-50% and 1:20%-30%:1.0-1.2%:60-90%; The obtained liquid graphene-porous carbon composite resin with a higher content of graphene-porous carbon nanospheres is added to the center of the mold, and another portion of liquid graphene-porous carbon composite resin is added to the edge of the mold, and molded to obtain a graphene-porous carbon composite resin layer; wherein the molding process parameters are: curing at room temperature for 4-6 hours, then applying a pressure of 0.5-1.0 kPa, and curing for 12-24 hours.
7. A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries according to claim 1, characterized in that: In the step 4, the graphene oxide slurry is prepared by subjecting commercial graphene oxide with a particle size of 1-3 μm to plasma treatment, and then adding the resultant to a dispersion solvent, wherein the mass volume ratio of the graphene oxide to the dispersion solvent is 100-150 g:100-200 mL, and ultrasonication is performed for 20-40 min to obtain a graphene oxide slurry; The preparation of the dispersing solvent is as follows: ethanol, DMF, NMP or THF and deionized water are mixed at a volume ratio of 1.5-2.5:
1.
8. A method for preparing a weldable conductive bipolar plate for acidic, alkaline and neutral flow batteries according to claim 1, characterized in that: In the step 4, uniform thermal spraying is performed by a spray gun, and the spraying temperature is 60-80° C.; the molding time is 6-8 hours, and the molding pressure is 0.5-1.0 kPa.
Citation Information
Patent Citations
Macro biomass modified electrode material and preparation method thereof
CN113571715A
Modified hard carbon composite material and preparation method thereof
CN108023075A
Preparation method of conductive graphene oxide plate which can be used for a bipolar plate of an all-vanadium liquid flow battery
CN109192993A
Method for preparing low-density flexible graphite plate for bipolar plate of high-conductivity hydrogen fuel cell from graphene-doped expanded graphite
CN109574004A
Weldable bipolar plate for flow battery and preparation and application thereof
CN111261891A