A seawater corrosion-resistant MXene composite film and wireless communication antenna
By combining graphene oxide nanosheets and MXene nanosheets and using laser engraving technology, a seawater-resistant MXene composite film was prepared, which solved the problems of mechanical stability and conductivity decline of the MXene film, and realized the use of wireless communication antennas in seawater environments. High performance is maintained under high pressure, and metal material loss is reduced.
Patent Information
- Application Number
- CN202311306221.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-10-10
AI Technical Summary
The MXene film is prone to cracks after repeated bending, and exposure to the atmospheric environment will cause structural changes due to oxidation reactions, reducing its mechanical properties and conductivity. When existing wireless communication antennas are used in marine environments, metal materials are prone to corrosion, affecting Performance and stability.
By combining graphene oxide nanosheets with different diameters and MXene nanosheets, a dense and smooth-surfaced MXene composite film is prepared. Laser engraving technology is used to produce wireless communication antennas, replacing conventional metal materials, and improving its seawater corrosion resistance and high conductivity. rate retention rate.
The MXene composite film achieves high conductivity and strong environmental stability, reducing the loss of metal materials. The antenna maintains excellent performance in seawater environments, and is suitable for wireless communication systems in ocean and offshore high-salt and high-humidity environments.
Smart Images

Figure CN117458118B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanocomposite materials, and in particular to a MXene composite film resistant to seawater corrosion and a wireless communication antenna. Background Art
[0002] MXene is short for two-dimensional transition metal carbide / nitride / carbonitride, which is prepared by selectively etching certain atoms from a layered matrix (MAX phase) and was first discovered by scientists at Drexel University in 2011. The MXene family has the general formula M n+1 X n T X , where M is an early transition metal (such as Ti, V, Mo, etc.), X represents C and / or N, n=1, 2 or 3, T X Represents the surface termination group (-OH, -O, -F). MXene materials have high electrical conductivity, but the mechanical stability and environmental stability of the MXene macrofilm itself need to be improved. Pure MXene films are prone to cracks after repeated bending. MXene films exposed to the atmosphere will change their structure due to oxidation reactions, thereby affecting their mechanical properties and conductive properties and reducing their conductivity.
[0003] With the continuous advancement of communication technology, antennas, as basic components in the field of communications, are constantly expanding their application scope. In radio equipment, the device used to radiate and receive radio waves is called an antenna. Radio equipment such as communications, radar, navigation, broadcasting, and television all use antennas as a medium to transmit and receive radio waves to transmit information. There are currently many types of wireless communication antennas, including directional antennas, omnidirectional antennas, microstrip antennas, helical antennas, patch antennas, etc. Different types of antennas are suitable for different scenarios and needs, including applications in marine environments. At present, the material of wireless communication antennas is usually metal material. When used in a marine environment, metal materials are prone to corrosion, resulting in a decrease in the conductivity of the wireless communication antenna, which in turn affects its performance and stability.
[0004] Based on the above-mentioned defects of the current wireless communication antennas made of MXene films and metal materials, it is necessary to improve them. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a MXene composite film resistant to seawater corrosion and a wireless communication antenna based on the composite film. By compounding graphene oxide and MXene nanosheets of different diameters, the obtained composite film structure is denser and the surface is smoother, which solves the problem that the pure MXene film is easily oxidized, and has a high conductivity that exceeds the MXene film itself, and has corrosion resistance and high conductivity retention rate in the seawater environment. The composite film is used instead of conventional metal materials for the production of wireless communication antennas, which can reduce the loss of conventional metals; the wireless communication antenna of the present invention has good performance and can maintain excellent performance after being immersed in seawater. Therefore, the wireless communication antenna based on the MXene composite film of the present invention has good application prospects in wireless communication systems in high-salt and high-humidity environments in the ocean and offshore.
[0006] In a first aspect, the present invention provides a MXene composite film resistant to seawater corrosion, and the preparation method of the MXene composite film resistant to seawater corrosion is:
[0007] The small-sized graphene oxide nanosheet solution, the large-sized graphene oxide nanosheet solution and the MXene nanosheet solution are mixed to form a mixed solution, the mixed solution is subjected to a film-forming treatment, and the film is dried after the film is formed to obtain the MXene composite film;
[0008] Wherein, the diameter of the small-sized graphene oxide nanosheets is 300 to 500 nm;
[0009] The diameter of the large-size graphene oxide nanosheet is 1000-1500nm.
[0010] Preferably, the MXene composite film resistant to seawater corrosion, the MXene nanosheets include Ti3C2T X 、Ti3CNT X 、Ti3N2T X 、Ti3C2T X or Ti4N3T X One or more of the .
[0011] And / or, the diameter of the MXene nanosheet is 3 to 5 μm.
[0012] Preferably, in the seawater corrosion-resistant MXene composite film, the mass ratio of small-sized graphene oxide nanosheets, large-sized graphene oxide nanosheets, and MXene nanosheets in the mixed solution is (5-10):(10-15):(75-85).
[0013] Preferably, the preparation method of the MXene composite film resistant to seawater corrosion, the small-sized graphene oxide nanosheet solution, and the large-sized graphene oxide nanosheet solution is:
[0014] adding graphene oxide to water to obtain a graphene oxide solution;
[0015] The graphene oxide solution is subjected to refinement treatment to obtain a small-sized graphene oxide nanosheet solution and a large-sized graphene oxide nanosheet solution.
[0016] Preferably, in the seawater corrosion-resistant MXene composite film, the mass fraction of the graphene oxide solution is 3 to 5%;
[0017] The graphene oxide solution is subjected to refinement treatment to obtain a small-sized graphene oxide nanosheet solution and a large-sized graphene oxide nanosheet solution, which specifically includes: treating the graphene oxide solution with an ultrasonic cleaner or a high-pressure nano-homogenizer so that the graphene oxide is exfoliated and refined to reach the required diameter, thereby obtaining a small-sized graphene oxide nanosheet solution and a large-sized graphene oxide nanosheet solution.
[0018] Preferably, the film-forming treatment of the seawater corrosion-resistant MXene composite film includes any one of blade coating, spin coating, spray coating or vacuum filtration;
[0019] and / or, the drying temperature is 30 to 60° C. and the drying time is 6 to 12 hours;
[0020] And / or, the preparation method of the MXene nanosheet solution is: adding MXene nanosheets into water to obtain the MXene nanosheet solution.
[0021] In a second aspect, the present invention also provides an application of the seawater corrosion-resistant MXene composite film in the preparation of a wireless communication antenna.
[0022] In a third aspect, the present invention further provides a wireless communication antenna having an operating frequency of 5.8 GHz, wherein a method for preparing the wireless communication antenna comprises the following steps:
[0023] Providing the seawater corrosion-resistant MXene composite film;
[0024] Laminating the MXene composite film on a substrate to obtain a composite;
[0025] The composite body is laser engraved to obtain the designed antenna structure, which is a wireless communication antenna.
[0026] Preferably, the process parameters of laser engraving of the wireless communication antenna are: laser wavelength of 350-360 μm, power frequency of 100 KHz-300 KHz, power of 2-5 W, pulse width of 1 ps-10 ps, and engraving speed of 50-200 mm / s.
[0027] Preferably, the process parameters of laser engraving of the wireless communication antenna are: laser wavelength of 355 μm, power frequency of 100 KHz, power of 3 W, pulse width of 1.5 ps, and engraving speed of 100 mm / s.
[0028] The present invention has the following beneficial effects:
[0029] 1. The present invention prepares a MXene composite film by compounding graphene oxide nanosheets and MXene nanosheets of different diameters. Compared with the pure MXene film, the composite film prepared by the present invention has a denser structure and a smoother surface, and has a high electrical conductivity and strong environmental stability exceeding the pure MXene film. While improving the electrical conductivity, it solves the pain point problem of the MXene film's inability to resist oxidation. It also has a high conductivity retention rate in seawater and is resistant to seawater corrosion, which can meet the application conditions of the antenna in a seawater environment.
[0030] 2. The present invention utilizes MXene composite film to replace conventional metal materials for the production of wireless communication antennas, thereby reducing the loss of conventional metals. Laser engraving technology is used in the process of preparing wireless communication antennas, and there is no need to prepare a mask, and processes such as photolithography, development, and etching are also omitted, greatly reducing time costs and processing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art descriptions. Obviously, the drawings described below are only some embodiments of the present invention, and for those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 It is a processing schematic diagram of the wireless communication antenna in the present invention;
[0033] Figure 2 This is a scanning electron microscope image of the MXene composite film prepared in Example 1 of the present invention;
[0034] Figure 3 This is a scanning electron microscope image of the MXene composite film prepared in Comparative Example 2;
[0035] Figure 4 This is a scanning electron microscope image of the MXene composite film prepared in Comparative Example 6;
[0036] Figure 5 This is a scanning electron microscope image of the MXene film prepared in Comparative Example 8;
[0037] Figure 6The conductivity diagram of the MXene composite film prepared from graphene oxide nanosheets of different diameters in Comparative Examples 1 to 7;
[0038] Figure 7 This is a comparison chart of the electrical conductivity of the MXene composite film prepared in Example 1 of the present invention and the MXene film prepared in Comparative Example 8;
[0039] Figure 8 This is a comparison chart of the electrical conductivity retention rates of the MXene composite films prepared in Example 1, Comparative Example 2, Comparative Example 6 and the MXene film prepared in Comparative Example 8 placed in an air environment;
[0040] Fig. 9 This is a comparison chart of the conductivity retention rates of the MXene composite films prepared in Example 1, Comparative Example 2, Comparative Example 6 and the MXene film prepared in Comparative Example 8 placed in seawater;
[0041] Fig.10 is the S of the wireless communication antenna prepared by the present invention 11 Parameter diagram;
[0042] Fig.11 The E-plane radiation pattern of the wireless communication antenna of the present invention before being immersed in seawater;
[0043] Fig.12 The H-plane radiation pattern of the wireless communication antenna of the present invention before being immersed in seawater;
[0044] Fig.13 The E-plane radiation pattern of the wireless communication antenna of the present invention after being immersed in seawater;
[0045] Fig.14 The H-plane radiation pattern of the wireless communication antenna of the present invention after being immersed in seawater;
[0046] Fig.15 This is a physical picture of the wireless communication antenna prepared in the application example. DETAILED DESCRIPTION
[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the numbered ranges, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0049] The present invention provides a MXene composite film resistant to seawater corrosion, and the preparation method thereof is as follows:
[0050] A small-sized graphene oxide nanosheet solution, a large-sized graphene oxide nanosheet solution and a MXene nanosheet solution are mixed to prepare a mixed solution, the mixed solution is subjected to a film-forming treatment, and after the film is formed, it is dried to obtain a MXene composite film;
[0051] Among them, the diameter of small-sized graphene oxide nanosheets is 300 to 500 nm;
[0052] The diameter of large-sized graphene oxide nanosheets is 1000-1500nm.
[0053] It should be noted that the defects, edges and vacancies of MXene nanosheets are easily oxidized, and the oxygen-containing functional groups on the surface of MXene nanosheets will cause MXene to be oxidized to TiO2 in an oxygen and water environment, thereby greatly reducing its conductivity and destroying its inherent high conductivity. The present invention uses graphene oxide (GO) with a similar structure to MXene nanosheets to prepare a graphene oxide-modified MXene-based composite film. The surface of graphene oxide nanosheets contains rich functional groups, which can be connected to MXene nanosheets at the interface by strong hydrogen bond interaction. The composite graphene oxide stabilizes the oxygen-containing functional groups on the surface of MXene nanosheets and reduces their contact with oxygen. In addition, the large-sized graphene oxide flattens the wrinkled parts of MXene through electrostatic repulsion, and the layers The spacing is reduced, thereby improving the conductivity of the composite film; further, the present invention uses large-diameter graphene oxide nanosheets and small-diameter graphene oxide nanosheets for compounding, the diameter of the small-size graphene oxide nanosheets is 300-500nm, and the diameter of the large-size graphene oxide nanosheets is 1000-1500nm. The small-size graphene oxide nanosheets fill the gaps through intercalation to make the composite membrane structure denser, and the dense composite membrane structure is not easy to collapse; at the same time, compared with the MXene membrane, the surface of the composite membrane of the present invention is smoother, has high conductivity and strong environmental stability, while improving the conductivity, it solves the pain point problem of the MXene membrane's inability to resist oxidation, and has a high conductivity retention rate in seawater, is resistant to seawater corrosion, and can meet the application conditions of the antenna in a seawater environment.
[0054] In some embodiments, the MXene nanosheets include Ti3C2T X 、Ti3CNT X 、Ti3N2T X 、Ti3C2T X or Ti4N3T X One or more of the .
[0055] In some embodiments, the diameter of the MXene nanosheets is 3 to 5 μm.
[0056] In some embodiments, the mass ratio of small-sized graphene oxide nanosheets, large-sized graphene oxide nanosheets, and MXene nanosheets in the mixed solution is (5-10):(10-15):(75-85).
[0057] In some embodiments, the preparation method of the small-sized graphene oxide nanosheet solution and the large-sized graphene oxide nanosheet solution is:
[0058] adding graphene oxide to water to obtain a graphene oxide solution;
[0059] The graphene oxide solution is subjected to refinement treatment to obtain a small-sized graphene oxide nanosheet solution and a large-sized graphene oxide nanosheet solution.
[0060] Specifically, in the above embodiment, graphene oxide is added to ultrapure water to obtain a graphene oxide solution.
[0061] In some embodiments, the mass fraction of the graphene oxide solution is 3-5%.
[0062] In some embodiments, the graphene oxide solution is subjected to a refinement treatment to obtain a small-sized graphene oxide nanosheet solution and a large-sized graphene oxide nanosheet solution, which specifically includes: treating the graphene oxide solution with an ultrasonic cleaner or a high-pressure nano-homogenizer so that the graphene oxide is exfoliated and refined to a required diameter, thereby obtaining a small-sized graphene oxide nanosheet solution and a large-sized graphene oxide nanosheet solution.
[0063] In some embodiments, the film forming process includes any one of blade coating, spin coating, spray coating or vacuum filtration.
[0064] Specifically, in the above embodiments, the mixed solution is scraped, spin-coated or sprayed on a substrate to obtain a composite film, which is then dried, and the composite film is peeled off from the substrate to obtain a graphene oxide / MXene composite film; wherein the substrate is a polymer film material, specifically, the polymer film material includes one of PET (polyethylene terephthalate), PVC (polyvinyl chloride), PC (polycarbonate), and PI (polyimide).
[0065] In some embodiments, the drying temperature is 30-60° C. and the drying time is 6-12 hours.
[0066] In some embodiments, the preparation method of the MXene nanosheet solution is: adding MXene nanosheets to water and mixing well to obtain the MXene nanosheet solution.
[0067] Specifically, in the above embodiment, MXene nanosheets are added into ultrapure water and mixed to obtain a MXene nanosheet solution.
[0068] Based on the same inventive concept, the present invention also provides an application of the above-mentioned seawater corrosion-resistant MXene composite film in the preparation of a wireless communication antenna.
[0069] Specifically, the MXene composite film of the present invention has good seawater corrosion resistance and high conductivity retention rate. The composite film is used to replace conventional metal materials for the production of wireless communication antennas, which can reduce the loss of conventional metals; the wireless communication antenna of the present invention has good performance and can maintain excellent performance after being immersed in seawater. Therefore, the wireless communication antenna based on the MXene composite film of the present invention has good application prospects in wireless communication systems in high-salt and high-humidity environments in the ocean and offshore.
[0070] Specifically, the MXene composite film of the present invention can be used to prepare a wireless communication antenna with an operating frequency of 5.8 GHz.
[0071] Based on the same inventive concept, the present invention also provides a wireless communication antenna, and the preparation method thereof comprises the following steps:
[0072] S1. providing the above-mentioned MXene composite film resistant to seawater corrosion;
[0073] S2, laminating the MXene composite film on a substrate to obtain a composite;
[0074] S3. Laser engraving the complex to obtain the designed antenna structure, which is a wireless communication antenna.
[0075] Conventional antenna processing will use a die-cutting solution, which will involve the step of antenna transfer, resulting in deviations in the antenna structure. Wireless communication antennas are small in size (15mm×15mm) and the insulation gap is generally narrow (about 70μm), which is difficult to achieve using conventional processing solutions. The present invention selects a laser engraving solution to directly engrave the non-antenna part of the film. The pattern retained after engraving is the antenna structure (that is, the radiator mentioned above). During the processing, there is no need to prepare a mask, and the processes of photolithography, development, and etching are also omitted, which greatly reduces the time cost (the entire processing time is 3 minutes) and processing cost (equipment loss cost).
[0076] Specifically, the material of the substrate of the present invention is a high molecular polymer film material. Specifically, the high molecular polymer film material includes one of PET (polyethylene terephthalate), PVC (polyvinyl chloride), PC (polycarbonate), and PI (polyimide).
[0077] In some embodiments, the process parameters of laser engraving are: laser wavelength of 350-360 μm, power frequency of 100 KHz-300 KHz, power of 2-5 W, pulse width of 1 ps-10 ps, and engraving speed of 50-200 mm / s.
[0078] In some embodiments, the process parameters of laser engraving are: laser wavelength of 355 μm, power frequency of 100 KHz, power of 3 W, pulse width of 1.5 ps, and engraving speed of 100 mm / s.
[0079] Specifically, laser engraving is based on CNC technology and uses laser as the processing medium to make the processing material melt and vaporize instantly under the laser irradiation to achieve the purpose of processing. It has the characteristics of "wide range, safe and reliable, precise and meticulous, environmentally friendly, high speed and low cost"; Figure 1 As shown, the present invention uses a computer to generate the structural data of the designed wireless communication antenna, converts the data into direct writing system control data, transmits it to the DMD chip, and controls the computer to control the high-precision laser beam to directly scan and engrave the complex, and the remaining part is the designed antenna structure.
[0080] The wireless communication antenna preparation method of the present invention has the following advantages: 1) The processing accuracy can reach 0.02mm, and high-speed engraving and cutting can be performed immediately according to the computer output pattern, and the processing effect of the same batch is guaranteed to be completely consistent, reducing the time cost and economic cost of detection, greatly reducing the error rate, and reducing waste; 2) The beam and spot diameter are small, generally less than 0.5mm, and the preparation process has the characteristics of low energy consumption, material saving, safety and hygiene.
[0081] The following further describes the preparation method of the seawater corrosion-resistant MXene composite film and wireless communication antenna of the present application with specific examples. This section further illustrates the content of the present invention in conjunction with specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0082] The raw materials used in the following examples and comparative examples are graphene oxide purchased from Huaxing Chemical (Wuhan) Co., Ltd., MXene nanosheets purchased from Sanya Hanxi Graphene Technology Research Institute Co., Ltd., and MXene nanosheets are specifically Ti3C2T X , the diameter of MXene nanosheets is 3 to 5 μm.
[0083] Example 1
[0084] This embodiment provides a MXene composite film, and a preparation method thereof comprises the following steps:
[0085] S1. adding graphene oxide to ultrapure water to obtain a graphene oxide solution with a mass fraction of 5%;
[0086] S2, placing the graphene oxide solution in S1 in a high-pressure nano-homogenizer for treatment at different pressures to exfoliate and refine the graphene oxide, and obtaining a graphene oxide nanosheet solution with a diameter of 1400 nm and a graphene oxide nanosheet solution with a diameter of 400 nm, respectively;
[0087] S3, MXene nanosheets (specifically Ti3C2T X ) is added into ultrapure water to prepare a MXene nanosheet solution;
[0088] S4, mixing the graphene oxide nanosheet solution with a diameter of 1400 nm in S2, the graphene oxide nanosheet solution with a diameter of 400 nm, and the MXene nanosheet solution in S3 to obtain a mixed solution; wherein the mass ratio of the graphene oxide nanosheet with a diameter of 1400 nm, the graphene oxide nanosheet with a diameter of 400 nm, and the MXene nanosheet in the mixed solution is 13:6:81;
[0089] S5. Stir the mixed solution in S4 evenly under a magnetic stirring speed of 600 rpm for 1 hour, then apply the mixed solution to the PET substrate to form a film, put it into a 50°C oven for drying for 8 hours, peel off the composite film from the PET substrate, and obtain a MXene composite film.
[0090] Example 2
[0091] This embodiment provides a MXene composite film, and a preparation method thereof comprises the following steps:
[0092] S1. adding graphene oxide to ultrapure water to obtain a graphene oxide solution with a mass fraction of 3%;
[0093] S2, placing the graphene oxide solution in S1 in a high-pressure nano-homogenizer for treatment at different pressures to exfoliate and refine the graphene oxide, and obtaining a graphene oxide nanosheet solution with a diameter of 1500 nm and a graphene oxide nanosheet solution with a diameter of 300 nm, respectively;
[0094] S3, MXene nanosheets (specifically Ti3C2T X ) is added into ultrapure water to prepare a MXene nanosheet solution;
[0095] S4, mixing the graphene oxide nanosheet solution with a diameter of 1500 nm, the graphene oxide nanosheet solution with a diameter of 300 nm, and the MXene nanosheet solution of S3 to obtain a mixed solution; wherein the mass ratio of the graphene oxide nanosheet with a diameter of 1500 nm, the graphene oxide nanosheet with a diameter of 300 nm, and the MXene nanosheet in the mixed solution is 12:10:78;
[0096] S5. Stir the mixed solution in S4 evenly under a magnetic stirring speed of 600 rpm for 1 hour, then spin-coat the mixed solution onto a PET substrate to form a film. After the film is formed, put it into a 50°C oven for drying for 8 hours, and peel off the composite film from the PET substrate to obtain a MXene composite film.
[0097] Example 3
[0098] This embodiment provides a MXene composite film, and a preparation method thereof comprises the following steps:
[0099] S1. adding graphene oxide to ultrapure water to obtain a graphene oxide solution with a mass fraction of 5%;
[0100] S2, placing the graphene oxide solution in S1 in a high-pressure nano-homogenizer for treatment at different pressures to exfoliate and refine the graphene oxide, and obtaining a graphene oxide nanosheet solution with a diameter of 1200 nm and a graphene oxide nanosheet solution with a diameter of 300 nm, respectively;
[0101] S3, MXene nanosheets (specifically Ti3C2T X ) is added into ultrapure water to prepare a MXene nanosheet solution;
[0102] S4, mixing the graphene oxide nanosheet solution with a diameter of 1200 nm, the graphene oxide nanosheet solution with a diameter of 300 nm, and the MXene nanosheet solution in S3 to obtain a mixed solution; wherein the mass ratio of the graphene oxide nanosheet with a diameter of 1200 nm, the graphene oxide nanosheet with a diameter of 300 nm, and the MXene nanosheet in the mixed solution is 10:10:80;
[0103] S5. Stir the mixed solution in S4 evenly under a magnetic stirring speed of 600 rpm for 1 hour, then pour the mixed solution into a vacuum filtration bottle and vacuum filter for 2 hours (use a 0.22 μm water-based microporous filter membrane during vacuum filtration). After filtration to form a membrane, put it into a 60°C oven and dry it for 6 hours to obtain a MXene composite membrane.
[0104] Example 4
[0105] This embodiment provides a MXene composite film, and a preparation method thereof comprises the following steps:
[0106] S1. adding graphene oxide to ultrapure water to obtain a graphene oxide solution with a mass fraction of 5%;
[0107] S2, placing the graphene oxide solution in S1 in a high-pressure nano-homogenizer for treatment at different pressures to exfoliate and refine the graphene oxide, and obtaining a graphene oxide nanosheet solution with a diameter of 1300 nm and a graphene oxide nanosheet solution with a diameter of 500 nm, respectively;
[0108] S3, MXene nanosheets (specifically Ti3C2T X ) is added into ultrapure water to prepare a MXene nanosheet solution;
[0109] S4, mixing the graphene oxide nanosheet solution with a diameter of 1300 nm in S2, the graphene oxide nanosheet solution with a diameter of 500 nm, and the MXene nanosheet solution in S3 to obtain a mixed solution; wherein the mass ratio of the graphene oxide nanosheet with a diameter of 1300 nm, the graphene oxide nanosheet with a diameter of 500 nm, and the MXene nanosheet in the mixed solution is 15:5:80;
[0110] S5. Stir the mixed solution in S4 evenly under a magnetic stirring speed of 600 rpm for 1 hour, then spray the mixed solution onto a PET substrate to form a film. After the film is formed, put it into a 40°C oven for drying for 12 hours, and peel off the composite film from the PET substrate to obtain a MXene composite film.
[0111] Comparative Example 1
[0112] This comparative example provides a MXene composite film, and its preparation method comprises the following steps:
[0113] S1. adding graphene oxide to ultrapure water to obtain a graphene oxide solution with a mass fraction of 5%;
[0114] S2, placing the graphene oxide solution in S1 in a high-pressure nano-homogenizer for treatment at different pressures to exfoliate and refine the graphene oxide to obtain a graphene oxide nanosheet solution with a diameter of 200 nm;
[0115] S3, MXene nanosheets (specifically Ti3C2T X ) is added into ultrapure water to prepare a MXene nanosheet solution;
[0116] S4, mixing the graphene oxide nanosheet solution with a diameter of 200 nm in S2 and the MXene nanosheet solution in S3 to obtain a mixed solution; wherein the mass ratio of the graphene oxide nanosheet with a diameter of 200 nm to the MXene nanosheet in the mixed solution is 19:81;
[0117] S5. Stir the mixed solution in S4 evenly under a magnetic stirring speed of 600 rpm for 1 hour, then apply the mixed solution to the PET substrate to form a film, put it into a 50°C oven for drying for 8 hours, peel off the composite film from the PET substrate, and obtain a MXene composite film.
[0118] Comparative Example 2
[0119] This comparative example provides a MXene composite film, which is the same as comparative example 1, except that a graphene oxide nanosheet solution with a diameter of 400 nm is prepared in step S2; in step S4, the graphene oxide nanosheet solution with a diameter of 400 nm is mixed with a MXene nanosheet solution, and the mass ratio of the graphene oxide nanosheets with a diameter of 400 nm to the MXene nanosheets in the mixed solution is 19:81; and finally a MXene composite film is prepared, and the other process conditions are the same as those in comparative example 1.
[0120] Comparative Example 3
[0121] This comparative example provides a MXene composite film, which is the same as comparative example 1, except that a graphene oxide nanosheet solution with a diameter of 600 nm is prepared in step S2; in step S4, the graphene oxide nanosheet solution with a diameter of 600 nm is mixed with a MXene nanosheet solution, and the mass ratio of the graphene oxide nanosheets with a diameter of 600 nm to the MXene nanosheets in the mixed solution is 19:81; and finally a MXene composite film is prepared, and the other process conditions are the same as those in comparative example 1.
[0122] Comparative Example 4
[0123] This comparative example provides a MXene composite film, which is the same as comparative example 1, except that a graphene oxide nanosheet solution with a diameter of 800 nm is prepared in step S2; in step S4, the graphene oxide nanosheet solution with a diameter of 800 nm is mixed with a MXene nanosheet solution, and the mass ratio of the graphene oxide nanosheets with a diameter of 800 nm to the MXene nanosheets in the mixed solution is 19:81; and finally a MXene composite film is prepared, and the other process conditions are the same as those in comparative example 1.
[0124] Comparative Example 5
[0125] This comparative example provides a graphene oxide / MXene composite film, which is the same as comparative example 1, except that a graphene oxide nanosheet solution with a diameter of 1000 nm is prepared in step S2; in step S4, the graphene oxide nanosheet solution with a diameter of 1000 nm is mixed with a MXene nanosheet solution, and the mass ratio of the graphene oxide nanosheets with a diameter of 1000 nm to the MXene nanosheets in the mixed solution is 19:81; and finally a MXene composite film is prepared, and the other process conditions are the same as those in comparative example 1.
[0126] Comparative Example 6
[0127] This comparative example provides a graphene oxide / MXene composite film, which is the same as comparative example 1, except that a graphene oxide nanosheet solution with a diameter of 1400 nm is prepared in step S2; in step S4, the graphene oxide nanosheet solution with a diameter of 1400 nm is mixed with a MXene nanosheet solution, and the mass ratio of the graphene oxide nanosheets with a diameter of 1400 nm to the MXene nanosheets in the mixed solution is 19:81; and finally a MXene composite film is prepared, and the other process conditions are the same as those in comparative example 1.
[0128] Comparative Example 7
[0129] This comparative example provides a graphene oxide / MXene composite film, which is the same as comparative example 1, except that a graphene oxide nanosheet solution with a diameter of 2000 nm is prepared in step S2; in step S4, the graphene oxide nanosheet solution with a diameter of 2000 nm is mixed with a MXene nanosheet solution, and the mass ratio of the graphene oxide nanosheets with a diameter of 2000 nm to the MXene nanosheets in the mixed solution is 19:81; and finally a MXene composite film is prepared, and the other process conditions are the same as those in comparative example 1.
[0130] Comparative Example 8
[0131] This comparative example provides a MXene film, and the preparation method thereof comprises the following steps:
[0132] S1. MXene nanosheets (specifically Ti3C2T X ) was added into ultrapure water to prepare a MXene nanosheet solution with a mass fraction of 5%;
[0133] S2. Stir the MXene nanosheet solution in S1 evenly under a magnetic stirring speed of 600 rpm for 1 hour, then scrape the MXene nanosheet solution onto the PET substrate to form a film, put it into a 50°C oven for drying for 8 hours, peel off the composite film from the PET substrate, and obtain the MXene film.
[0134] Performance Testing
[0135] Figure 2 This is a scanning electron microscope image of the MXene composite film prepared in Example 1.
[0136] Figure 3 This is a scanning electron microscope image of the MXene composite film prepared in Comparative Example 2.
[0137] Figure 4 This is a scanning electron microscope image of the MXene composite film prepared in Comparative Example 6.
[0138] Figure 5 This is a scanning electron microscope image of the MXene film prepared in Comparative Example 8.
[0139] pass Figures 2 to 5 By comparison, it can be seen that the surface of the pure MXene film has large wrinkles, while the surface of the MXene composite film prepared by the present invention is smoother. This is because the large-diameter graphene oxide flattens the wrinkled part of the MXene through the electrostatic repulsion, and at the same time, the small-diameter graphene oxide fills the gaps through intercalation to make the composite film structure denser. Finally, the surface of the MXene composite film formed is smoother and the structure is denser.
[0140] The conductivity of the MXene composite films prepared from graphene oxide nanosheets of different diameters in Comparative Examples 1 to 7 was tested, and the results were as follows: Figure 6 Specifically, the conductivity of the MXene composite films prepared in Comparative Examples 1 to 7 was measured using an RTS-8 four-probe tester. Figure 6 The horizontal axis in the middle represents graphene oxide nanosheets with different diameters.
[0141] from Figure 6 It can be seen that the conductivity of graphene oxide with diameters of 300-500nm and 1000-1500nm is significantly improved when it is composited with MXene. This is because the action mechanism of graphene oxide with different diameters is different when it is composited with MXene.
[0142] The conductivity of the MXene composite film prepared in Example 1 and the MXene film prepared in Comparative Example 8 were measured using an RTS-8 four-probe tester. The results are as follows: Figure 7 shown. Figure 7 The MXene in the above-mentioned example is the MXene film prepared in Comparative Example 8, and the MXene-GO is the MXene composite film prepared in Example 1.
[0143] from Figure 7 It can be seen that compared with the pure MXene film, the conductivity of the MXene composite film of the present invention is greatly improved, reaching 5.2×10 5 S / m.
[0144] The MXene composite films prepared in Example 1, Comparative Example 2, Comparative Example 6 and the MXene film prepared in Comparative Example 8 were placed in an air environment (normal temperature 25° C.), and their conductivity was tested using an RTS-8 four-probe tester, and the conductivity retention rate was calculated. The results are as follows: Figure 8 shown.
[0145] The calculation formula of the conductivity retention rate is: the conductivity of the composite film after being placed in an air environment / the initial conductivity of the composite film.
[0146] Figure 8 The MXene in the above formula is the MXene film in Comparative Example 8, MXene-Ⅰ represents the MXene composite film prepared in Comparative Example 6, MXene-Ⅱ represents the MXene composite film prepared in Comparative Example 2, and MXene-Ⅲ represents the MXene composite film prepared in Example 1. Figure 8 The middle abscissa represents the number of days (d) that different membranes are placed in an air environment. Figure 8 The vertical axis represents the conductivity retention rate of different membranes.
[0147] from Figure 8 It can be seen that the electrical conductivity of the MXene composite film prepared in Example 1 remains almost unchanged in an air environment, indicating that the MXene composite film prepared in the present invention has good oxidation resistance.
[0148] The MXene composite films prepared in Example 1, Comparative Example 2, Comparative Example 6 and the MXene film prepared in Comparative Example 8 were placed in seawater (specifically seawater from a certain area in Sanya), and their conductivity was tested using an RTS-8 four-probe tester, and the conductivity retention rate was calculated. The results are as follows: Fig. 9 The calculation formula of the conductivity retention rate is: the conductivity of the composite membrane after immersion in seawater / the initial conductivity of the composite membrane.
[0149] Fig. 9 The MXene in the above formula is the MXene film in Comparative Example 8, MXene-Ⅰ represents the MXene composite film prepared in Comparative Example 6, MXene-Ⅱ represents the MXene composite film prepared in Comparative Example 2, and MXene-Ⅲ represents the MXene composite film prepared in Example 1. Fig. 9 The middle horizontal axis represents the time (h) that different membranes are placed in seawater. Fig. 9 The vertical axis represents the conductivity retention rate of different membranes.
[0150] from Fig. 9It can be seen that the MXene composite membrane of the present invention still has a high conductivity retention rate in a complex and corrosive environment and has good seawater corrosion resistance; the composite membrane prepared by combining the large and small diameter graphene oxide combination and MXene of the present invention has strong environmental stability and seawater corrosion resistance.
[0151] Application Examples
[0152] The MXene composite film prepared in Example 1 is applied to a microwave antenna to prepare a wireless communication antenna, which specifically includes the following steps:
[0153] S1. The MXene composite film prepared in Example 1 is pasted and laminated with a substrate (specifically PET) to obtain a composite;
[0154] S2, using a laser engraving machine LPKF ProtoLaser U4 to laser engrave the complex in S1 to obtain the designed antenna structure, which is a wireless communication antenna;
[0155] Among them, the process parameters of laser engraving are: laser wavelength is 355μm, power frequency is 100KHz, power is 3W, pulse width is 1.5ps, and structuring speed is 100mm / s.
[0156] The S of the wireless communication antenna prepared in the above embodiment was measured using a vector network analyzer and a microwave darkroom. 11 and E and H surface radiation, the results are as follows Figures 10 to 14 shown.
[0157] Fig.10 S of wireless communication antenna 11 The simulation results of the value are close to the actual test results. 11 The value is much smaller than the -10dB required for antenna resonance.
[0158] Fig.11 This is the E-plane radiation pattern of the wireless communication antenna of the present invention before being immersed in seawater.
[0159] Fig.12 This is the H-plane radiation pattern of the wireless communication antenna of the present invention before being immersed in seawater.
[0160] Fig.13 This is the E-plane radiation pattern of the wireless communication antenna of the present invention after being immersed in seawater for 2 hours.
[0161] Fig.14 This is the H-plane radiation pattern of the wireless communication antenna of the present invention after being immersed in seawater for 2 hours.
[0162] from Figures 11 to 14It can be seen that the simulation results of the E and H surface radiation of the wireless communication antenna of the present invention before and after being immersed in seawater are close to the actual test results. The radiation performance attenuation of the wireless communication antenna of the present invention is small after being immersed in seawater, and still meets the antenna performance requirements. In summary, the wireless communication antenna prepared by the present invention exhibits a return loss of less than -10dB in 5G millimeter wave communication and has excellent resistance to seawater corrosion.
[0163] Fig.15 This is a physical picture of the wireless communication antenna prepared in the application example.
[0164] The wireless communication antenna prepared by the present invention has excellent conformal capability, and its operating frequency and performance meet the requirements of 5G communication. In addition, the wireless communication antenna is small in size, low in processing cost, excellent in radiation performance, and has the characteristics of seawater corrosion resistance. Therefore, the wireless communication antenna provides a valuable reference for the wider commercial application of flexible electronic integration and 5G communication.
[0165] In summary, the present invention prepares a composite membrane by combining large and small-sized graphene oxide and MXene. Compared with the MXene membrane, the composite membrane has the characteristics of smooth surface and dense structure, and at the same time has high conductivity and strong environmental stability. While improving the conductivity, it solves the problem that the MXene membrane is not resistant to oxidation. In addition, the composite membrane shows a high conductivity retention rate in seawater and has seawater corrosion resistance. The composite membrane is applied to wireless communication antennas, which can effectively reduce the loss of metal materials and meet the requirements of antenna performance. Based on the characteristics of the composite membrane's resistance to seawater corrosion, its application in the field of radio frequency can also be expanded.
[0166] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A graphene oxide / MXene composite film resistant to seawater corrosion, characterized in that: The preparation method of the seawater corrosion-resistant graphene oxide / MXene composite film is as follows: A small-sized graphene oxide nanosheet solution, a large-sized graphene oxide nanosheet solution and a MXene nanosheet solution are mixed to form a mixed solution, the mixed solution is subjected to a film-forming treatment, and the film is dried after the film is formed to obtain the graphene oxide / MXene composite film; Wherein, the diameter of the small-sized graphene oxide nanosheets is 300 to 500 nm; The diameter of the large-sized graphene oxide nanosheets is 1000-1500 nm; The preparation method of the small-sized graphene oxide nanosheet solution and the large-sized graphene oxide nanosheet solution is: adding graphene oxide to water to obtain a graphene oxide solution; The graphene oxide solution is subjected to refinement treatment to obtain a small-sized graphene oxide nanosheet solution and a large-sized graphene oxide nanosheet solution; The film forming process includes any one of blade coating, spin coating, spray coating or vacuum filtration; The drying temperature is 30-60°C and the drying time is 6-12h; The preparation method of the MXene nanosheet solution is: adding MXene nanosheets into water to obtain the MXene nanosheet solution.
2. The seawater corrosion-resistant graphene oxide / MXene composite film according to claim 1, characterized in that: The MXene nanosheets include Ti3C2T X 、Ti3CNT X 、Ti3N2T X 、Ti3C2T X or Ti4N3T X One or more of the following; And / or, the diameter of the MXene nanosheet is 3 to 5 μm.
3. The seawater corrosion-resistant graphene oxide / MXene composite film according to any one of claims 1 to 2, characterized in that: The mass ratio of small-sized graphene oxide nanosheets, large-sized graphene oxide nanosheets and MXene nanosheets in the mixed solution is (5-10):(10-15):(75-85).
4. The seawater corrosion-resistant graphene oxide / MXene composite film according to claim 1, characterized in that: The mass fraction of the graphene oxide solution is 3-5%; The graphene oxide solution is subjected to refinement treatment to obtain a small-sized graphene oxide nanosheet solution and a large-sized graphene oxide nanosheet solution, which specifically includes: treating the graphene oxide solution with an ultrasonic cleaner or a high-pressure nano-homogenizer so that the graphene oxide is exfoliated and refined to reach the required diameter, thereby obtaining a small-sized graphene oxide nanosheet solution and a large-sized graphene oxide nanosheet solution.
5. Use of the seawater corrosion-resistant graphene oxide / MXene composite film as claimed in any one of claims 1 to 4 in the preparation of a patch antenna.
6. A patch antenna, characterized in that: The method for preparing the patch antenna comprises the following steps: Providing a seawater corrosion-resistant graphene oxide / MXene composite film as claimed in any one of claims 1 to 4; Laminating the graphene oxide / MXene composite film on a substrate to obtain a composite; The composite body is laser engraved to obtain the designed antenna structure, namely the patch antenna.
7. The patch antenna according to claim 6, characterized in that: The process parameters of laser engraving are: laser wavelength is 350~360μm, power frequency is 100KHz~300KHz, power is 2~5W, pulse width is 1ps-10ps, and engraving speed is 50~200mm / s.
8. The patch antenna according to claim 7, characterized in that: The process parameters of laser engraving are: laser wavelength is 355μm, power frequency is 100KHz, power is 3W, pulse width is 1.5ps, and engraving speed is 100mm / s.
Citation Information
Patent Citations
MXene / rGO complex 3D structure based high-sensitivity sensor
CN108489644A
TiO2 / graphene multi-element modified Mxene composite material and preparation method thereof
CN109192940A