A double-sided aluminum foil reinforced PIR insulation board and its preparation process

By designing and manufacturing a double-sided aluminum foil reinforced PIR insulation board, and using a combined layer structure such as a polyester ether alcohol layer, the problems of insufficient strength and complex manufacturing of PIR insulation boards have been solved, achieving both strength improvement and process simplification.

CN117468592BActive Publication Date: 2026-11-17LONGYAN XINYONGHUA IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311437143.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-01
Publication Date
2026-11-17
Estimated Expiration
2043-11-01

AI Technical Summary

Technical Problem

Existing PIR insulation boards have low strength and complex manufacturing processes, making them prone to breakage after prolonged use and difficult to replace.

Method used

It adopts a double-sided aluminum foil reinforced structure, including a combination design of a polyester ether alcohol layer, a resin rubber layer, a soft auxiliary material layer, a silicate reinforcing layer and an adhesive layer, and is prepared through a specific ratio of raw material mixing, sterilization, molding, drying, slicing and compaction process.

Benefits of technology

This improved the strength of the PIR insulation board, prevented breakage, simplified the manufacturing process, and enhanced the quality of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117468592B_ABST
    Figure CN117468592B_ABST
Patent Text Reader

Abstract

This invention discloses a double-sided aluminum foil reinforced PIR insulation board and its manufacturing process, comprising an insulation board assembly. Aluminum foil assemblies are fixedly connected to both the front and back of the insulation board assembly. A reinforcing plate is fixedly connected to the outer side of the aluminum foil assemblies. A reinforcing frame is fitted onto the surface of the insulation board assembly. Adhesive plates are fixedly connected to both sides of the insulation board assembly. A polyester ether alcohol layer is disposed inside the reinforcing plate. This invention, through the inclusion of a polyester ether alcohol layer, a resin rubber layer, a soft auxiliary material layer, a silicate reinforcing layer, and an adhesive layer, improves the quality of the reinforcing plate and reinforcing frame, avoiding insufficient strength. This double-sided aluminum foil reinforced PIR insulation board and its manufacturing process solve the problems of low strength in traditional PIR insulation boards, which are prone to breakage after prolonged use, and the complex manufacturing process that affects the overall quality of use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of PIR insulation board technology, specifically to a double-sided aluminum foil reinforced PIR insulation board and its preparation process. Background Technology

[0002] According to a patent published on the China Patent Network, the patent title is: "A Double-Sided Reinforced PIR Insulation Board," patent number: 202221806343.3. This utility model belongs to the technical field of PIR insulation boards, specifically relating to a double-sided reinforced PIR insulation board, including an insulation board body. The insulation board body includes a sandwich assembly and metal protective layers installed on both sides of the sandwich assembly. A slot is formed in one of the metal protective layers, into which a placement block is inserted. A retractable slider is installed vertically in the slot, and a spring is installed between the slider and the metal protective layer. This utility model features a placement block, a slot, and a slider located on the rear side of the insulation board body that cooperate with each other. The placement block is installed on the wall, and the slot on the insulation board body is placed on one side of the placement block. The slot is pushed towards one side of the placement block, and when the slider is inserted into the placement block, the insulation board body is fixed. This solves the problem that existing insulation boards are usually fixed to the wall by adhesive, which is troublesome to disassemble and inconvenient to replace. In addition, the PIR insulation board mentioned above has low strength and is prone to breakage after long-term use. Moreover, its manufacturing process is also very complicated, which affects the overall quality of use.

[0003] Therefore, it is necessary to redesign and modify the PIR insulation board to effectively prevent its low strength and complex manufacturing process. Summary of the Invention

[0004] To address the problems mentioned in the background art, the present invention aims to provide a double-sided aluminum foil reinforced PIR insulation board and its preparation process, which has the advantages of increased strength and simple preparation, and solves the problems of low strength and complex preparation process.

[0005] To achieve the above objectives, the present invention provides the following technical solution: a double-sided aluminum foil reinforced PIR insulation board and its preparation process, comprising an insulation board assembly, wherein aluminum foil assemblies are fixedly connected to both the front and back sides of the insulation board assembly, a reinforcing plate is fixedly connected to the outer side of the aluminum foil assemblies, a reinforcing frame is sleeved on the surface of the insulation board assembly, and bonding plates are fixedly connected to both sides of the insulation board assembly.

[0006] As a preferred embodiment of the present invention, the reinforcing plate has a polyester ether alcohol layer inside, and a resin rubber layer is fixedly connected to the front side of the polyester ether alcohol layer. The reinforcing frame has a soft auxiliary material layer inside, and a silicate reinforcing layer is provided on the front side of the soft auxiliary material layer. An adhesive layer is provided on the front side of the silicate reinforcing layer.

[0007] As a preferred embodiment of the present invention, the polyester ether alcohol layer comprises: 20 parts of acid anhydride, 10 parts of catalyst, and 15 parts of propylene oxide; the resin rubber layer comprises: 50 parts of resin, 50 parts of rubber raw material, and 20 parts of natural silicone; the soft auxiliary material layer comprises: 100 parts of TPR particles and 50 parts of thermoplastic styrene-butadiene rubber; the silicate reinforcing layer comprises: 30 parts of plasticizer and 30 parts of thermoplastic particles; and the adhesive layer comprises: 10 parts of starch, 10 parts of protein, 6 parts of dextrin, 20 parts of animal glue, 10 parts of shellac, 10 parts of hide glue, and 15 parts of rosin.

[0008] As a preferred embodiment of the present invention, the steps include: a) proportioning raw materials; b) mixing raw materials sequentially; c) sterilization treatment; d) molding treatment; e) drying treatment; f) slicing treatment; and g) compaction treatment.

[0009] Step a) Proportioning raw materials: First, find out the materials required for each of the above-mentioned components and set them aside for later use.

[0010] Step b) Mix the raw materials in sequence: Take the above raw materials in proportion and then mix them by stirring at a speed of 150-200 r / min using a mixing device.

[0011] Step c) Sterilization: Collect the mixed raw materials and place them in a sterilization chamber for sterilization.

[0012] Step d) Molding process: After sterilization, place it in the molding mold and then shape it using the molding mold. After the process, set it aside for later use.

[0013] Step e) Drying treatment: Then place the shaped raw material in a dryer and dry it at a temperature of 80°C.

[0014] Step f) Slicing: After drying, the material is sliced ​​into layers, and the slice size should be kept between 2-3cm.

[0015] Step g) Compaction treatment: Then, the cut sheet and the outer board are compacted to make them completely bonded together and inseparable.

[0016] As a preferred embodiment of the present invention, the raw materials need to be kept warm during mixing, and the warming temperature is 30-35°C.

[0017] As a preferred embodiment of the present invention, when searching for the molding mold, the mold needs to be painted and the joints of the mold need to be confirmed to be flat and tight.

[0018] As a preferred embodiment of the present invention, the sterilization process requires multiple operations to avoid removing the product after only one sterilization.

[0019] As a preferred embodiment of the present invention, the compaction process must be carried out in a cleanroom to prevent dust from entering the gaps between the compacted parts.

[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0021] 1. The present invention, through the setting of a polyester ether alcohol layer, a resin rubber layer, a soft auxiliary material layer, a silicate reinforcing layer and an adhesive layer, can improve the texture of the reinforcing plate and the reinforcing frame, and avoid the phenomenon of insufficient strength. The double-sided aluminum foil reinforced PIR insulation board and its preparation process solve the problems mentioned above, such as the low strength of the PIR insulation board, which is easy to break after long-term use, and the complex preparation process, which affects the overall quality of use. Attached Figure Description

[0022] Figure 1 This is a schematic diagram of the structure of the present invention;

[0023] Figure 2 This is a top sectional view of the reinforcing plate of the present invention;

[0024] Figure 3 This is a top sectional view of the reinforcing frame of the present invention.

[0025] In the diagram: 1. Insulation board assembly; 2. Aluminum foil assembly; 3. Reinforcing plate; 4. Reinforcing frame; 5. Laminating board; 6. Polyester ether alcohol layer; 7. Resin rubber layer; 8. Flexible auxiliary material layer; 9. Silicate reinforcing layer; 10. Adhesive layer. Detailed Implementation

[0026] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0027] like Figures 1 to 3 As shown, the present invention provides a double-sided aluminum foil reinforced PIR insulation board and its preparation process, including an insulation board assembly 1, aluminum foil assemblies 2 are fixedly connected to the front and back of the insulation board assembly 1, a reinforcing plate 3 is fixedly connected to the outside of the aluminum foil assembly 2, a reinforcing frame 4 is sleeved on the surface of the insulation board assembly 1, and bonding plates 5 are fixedly connected to both sides of the insulation board assembly 1.

[0028] The present invention is further configured such that a polyester ether alcohol layer 6 is disposed inside the reinforcing plate 3, a resin rubber layer 7 is fixedly connected to the front side of the polyester ether alcohol layer 6, a soft auxiliary material layer 8 is disposed inside the reinforcing frame 4, a silicate reinforcing layer 9 is disposed on the front side of the soft auxiliary material layer 8, and an adhesive layer 10 is disposed on the front side of the silicate reinforcing layer 9.

[0029] The present invention is further configured such that the polyester ether alcohol layer 6 contains: 20 parts of acid anhydride, 10 parts of catalyst, and 15 parts of propylene oxide; the resin rubber layer 7 contains: 50 parts of resin, 50 parts of rubber raw material, and 20 parts of natural silicone; the soft auxiliary material layer 8 contains: 100 parts of TPR particles and 50 parts of thermoplastic styrene-butadiene rubber; the silicate reinforcing layer 9 contains: 30 parts of plasticizer and 30 parts of thermoplastic particles; and the adhesive layer 10 contains: 10 parts of starch, 10 parts of protein, 6 parts of dextrin, 20 parts of animal glue, 10 parts of shellac, 10 parts of hide glue, and 15 parts of rosin.

[0030] The present invention is further configured to include step a) proportioning raw materials; step b) mixing raw materials sequentially; step c) sterilization treatment; step d) molding treatment; step e) drying treatment; step f) slicing treatment; and step g) compaction treatment.

[0031] Step a) Proportioning raw materials: First, find out the materials required for each of the above-mentioned components and set them aside for later use.

[0032] Step b) Mix the raw materials in sequence: Take the above raw materials in proportion and then mix them by stirring at a speed of 150-200 r / min using a mixing device.

[0033] Step c) Sterilization: Collect the mixed raw materials and place them in a sterilization chamber for sterilization.

[0034] Step d) Molding process: After sterilization, place it in the molding mold and then shape it using the molding mold. After the process, set it aside for later use.

[0035] Step e) Drying treatment: Then place the shaped raw material in a dryer and dry it at a temperature of 80°C.

[0036] Step f) Slicing: After drying, the material is sliced ​​into layers, and the slice size should be kept between 2-3cm.

[0037] Step g) Compaction treatment: Then, the cut sheet and the outer board are compacted to make them completely bonded together and inseparable.

[0038] The present invention is further configured such that the raw materials need to be kept warm during mixing, and the warming temperature is 30-35°C.

[0039] The invention is further configured such that when searching for a molding die, the die needs to be painted and the joints of the die need to be confirmed to be flat and tight.

[0040] The present invention is further configured such that multiple operations are required during sterilization to avoid removing the product after only one sterilization.

[0041] The present invention is further configured such that the compaction process must be carried out in a clean room to prevent dust from entering the gaps between the compacted parts.

[0042] The working principle and usage process of this invention are as follows: First, identify the materials required for each of the above-mentioned components and set them aside for later use. Then, take the above-mentioned raw materials according to the proportions and mix them using a mixing device at a speed of 150-200 r / min. Collect the mixed raw materials and place them in a sterilization chamber for sterilization. After sterilization, place them in a molding mold and shape them using the molding mold. After shaping, set them aside for later use. Then, place the shaped raw materials in a dryer and dry them at a temperature of 80°C. After drying, cut the material into layers, and the cut size should be kept between 2-3 cm. Then, press the cut sheets and the outer plate together to make them completely bonded together and inseparable, thus achieving the effect of increased strength and simple preparation.

[0043] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0044] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A double-sided aluminum foil reinforced PIR insulation board, comprising an insulation board assembly (1), characterized in that: The insulation board assembly (1) has aluminum foil assemblies (2) fixedly connected to both its front and back sides. A reinforcing plate (3) is fixedly connected to the outer side of the aluminum foil assembly (2). A reinforcing frame (4) is fitted onto the surface of the insulation board assembly (1). Adhesive plates (5) are fixedly connected to both sides of the insulation board assembly (1). A polyester ether alcohol layer (6) is disposed inside the reinforcing plate (3). A resin rubber layer (7) is fixedly connected to the front side of the polyester ether alcohol layer (6). A soft auxiliary material layer (8) is disposed inside the reinforcing frame (4). A silicate reinforcing layer (9) is disposed on the front side of the soft auxiliary material layer (8). An adhesive layer (10) is disposed on the front side of the silicate reinforcing layer (9). The content of the polyester ether alcohol layer (6) is... The contents of the following are as follows: 20 parts of acid anhydride, 10 parts of catalyst, and 15 parts of propylene oxide; the contents of the resin rubber layer (7) are: 50 parts of resin, 50 parts of rubber raw material, and 20 parts of natural silicone; the contents of the soft auxiliary material layer (8) are: 100 parts of TPR particles and 50 parts of thermoplastic styrene-butadiene rubber; the contents of the silicate reinforcing layer (9) are: 30 parts of plasticizer and 30 parts of thermoplastic particles; the contents of the adhesive layer (10) are: 10 parts of starch, 10 parts of protein, 6 parts of dextrin, 20 parts of animal glue, 10 parts of shellac, 10 parts of hide glue, and 15 parts of rosin, including step a) proportioning raw materials; step b) mixing raw materials in sequence; step c) sterilization treatment; step d) molding treatment; step e) drying treatment; step f) slicing treatment; and step g) compaction treatment. Step a) Proportioning raw materials: First, find out the materials required for each of the above-mentioned components and set them aside for later use; Step b) Mix the raw materials in sequence: Take the above raw materials in proportion and mix them by stirring at a speed of 150-200 r / min using a mixing device; Step c) Sterilization: Collect the mixed raw materials and place them in a sterilization chamber for sterilization. Step d) Molding process: After sterilization, place it in the molding mold and then shape it using the molding mold. After processing, set it aside for later use. Step e) Drying treatment: Then place the shaped raw material in a dryer and dry it at a temperature of 80°C; Step f) Slicing: After drying, the material is sliced ​​into layers, and the slice size should be between 2-3cm. Step g) Compaction treatment: Then, the cut sheet and the outer board are compacted to make them completely bonded together and inseparable.

2. The double-sided aluminum foil reinforced PIR insulation board and its preparation process according to claim 1, characterized in that: The raw materials need to be kept warm during mixing, with a temperature of 30-35°C. When finding the molding mold, the mold needs to be painted and the joints of the mold need to be confirmed to be flat and tight. The sterilization process needs to be performed multiple times to avoid removing the mold after only one sterilization.

3. The double-sided aluminum foil reinforced PIR insulation board and its preparation process according to claim 1, characterized in that: The compaction process must be carried out in a cleanroom to prevent dust from getting into the gaps between the compacted parts.

Citation Information

Patent Citations

  • Polyurethane heat preservation composite board

    CN204983465U