A method for surfacing a valve stem surface of a steam turbine
By overlaying cobalt-based alloy powder with submicron reinforcing phases precipitated on the surface of turbine valve stems, the problem of easy cracking of the valve stem surface overlay was solved, achieving high-performance high-temperature resistance, wear resistance and corrosion resistance, and reducing production costs.
Patent Information
- Application Number
- CN202311573591.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-23
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-23
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallic materials and relates to a method for overlaying welding materials on the surface of steam turbine valve stems. Background Technology
[0002] With the development of steam turbine manufacturing technology, steam temperatures are increasing, requiring sealing components to possess excellent high-temperature resistance, wear resistance, and corrosion resistance. Valves, as core components of steam turbines, involve multiple parts requiring superior sealing performance, such as the dynamic contact seal between the valve stem and seat. These contact areas must exhibit good resistance to high temperatures, steam corrosion, and vibration wear. Considering manufacturing economics, key components like the valve stem and seat are typically made of heat-resistant steel. To increase the reliability of the contact areas, cobalt-based Stellite alloy is usually welded onto the valve stem and seat contact areas. Stellite alloy possesses high high-temperature resistance, wear resistance, and corrosion resistance. Welding it onto the valve head surface of the valve stem and the valve seat surface ensures that the contact between the valve stem and seat is actually with Stellite alloy, significantly improving the reliability of the dynamic seal between the valve stem and the valve. The most common problem with Stellite alloy overlay welding on valve stem surfaces is that the alloy layer is prone to cracking during welding, leading to weld failure. Although methods such as adding a transition layer or increasing the preheating temperature can improve the success rate to some extent, the process is complex and a certain percentage of cracking still occurs. Therefore, developing a material that possesses excellent material properties while being resistant to weld cracking is urgently needed. Summary of the Invention
[0003] This invention designs a novel cobalt-based alloy material for valve stem cladding. The design concept involves precipitating multiple submicron-scale reinforcing phases in the cobalt matrix through compositional design, replacing conventional carbide reinforcing phases. This reduces the risk of cracking. The designed reinforcing phases exhibit excellent high-temperature stability and are dispersed throughout the matrix. By controlling the composition, content, and type of the precipitated phases, the cladding layer possesses excellent high-temperature resistance, wear resistance, and corrosion resistance. When the alloy powder designed in this invention is cladding onto the valve stem surface, no cracking occurs, and excellent performance is observed, significantly improving yield and reducing production costs.
[0004] A method for overlaying a welding material onto the surface of a steam turbine valve stem is characterized by: preparing the welding material powder using water atomization or gas atomization processes; the powder composition being (2.5–3 wt%) Ni, (9–10 wt%) Fe, (13–15 wt%) Mn, (7–8 wt%) Si, (2.5–3 wt%) W, (7.5–8 wt%) B, with the remainder being Co; sieving the powder to a particle size of 50–150 micrometers; then overlaying the powder onto the valve stem / valve head surface using laser cladding technology; and finally machining the surface of the overlay layer to meet dimensional requirements.
[0005] Furthermore, the aforementioned turbine valve stem surface overlay material is characterized in that the laser power for overlay is controlled at 400-800W, the scanning speed is controlled at 400-500mm / min, the laser spot diameter is controlled at 0.5-1mm, and the powder feeding rate is 30-40g / min.
[0006] The main mechanism of the alloy composition design in this invention is that by adding Si, Mn, W, Ni, Fe, and B alloying elements to a Co matrix and strictly controlling the content and proportion of each element, three submicron-scale dispersed strengthening phases with high hardness can be formed in the Co matrix, namely 35-37 wt% Co. 42 B 40 Fe 15 W3 precipitate, 14-15 wt% Mn 33 B 66 Precipitated phase and 8-9 wt% Ni 30 Fe 25 Si 25 Mn 20 The precipitated phases, through the synergistic effect of these three high-strength, high-hardness phases, ensure that the weld overlay possesses excellent comprehensive properties such as impact resistance, wear resistance, and corrosion resistance. The weld overlay obtained using the above process has a hardness of 700-800 HV. 0.3 It has a higher hardness than cobalt-based Stellite alloys, resulting in low stress during the welding process and no cracking. The weld layer is also less likely to fall off during operation, effectively protecting the valve stem and thus significantly improving its lifespan and reliability. Detailed Implementation
[0007] Example 1: A 2mm thick alloy layer is deposited on the surface of the GH2132 high-temperature alloy valve stem.
[0008] The first step involves preparing an alloy powder with the following composition: 3wt% Ni, 10wt% Fe, 15wt% Mn, 8wt% Si, 3wt% W, 8wt% B, and the remainder being Co, using an air atomization process. The powder is then sieved to obtain a particle size of 50-150 micrometers.
[0009] The second step involves using laser cladding to deposit powder onto the surface of the GH2132 high-temperature alloy valve stem that requires welding after aging treatment. The laser power for the welding is 800W, the scanning speed is 400mm / min, the laser spot diameter is 1mm, the powder feeding rate is 30g / min, and the welding thickness is 2.2mm. Then, the 2.2mm thick alloy layer is processed to a thickness of 2mm to obtain the finished valve stem.
[0010] Example 2: A 2.2mm thick alloy layer was welded onto the surface of the 30Cr1Mo1V heat-resistant steel valve stem.
[0011] The first step involves preparing an alloy powder with the following composition: 2.5 wt% Ni, 9 wt% Fe, 13 wt% Mn, 7 wt% Si, 2.5 wt% W, 7.5 wt% B, and the remainder Co, using an air atomization process. The powder is then sieved to obtain a particle size of 50-150 micrometers.
[0012] The second step involves using laser cladding to deposit powder onto the surface of the 30Cr1Mo1V heat-resistant steel valve stem that requires welding, after heat treatment. The laser power for the welding is 400W, the scanning speed is 500mm / min, the laser spot diameter is 1mm, the powder feeding rate is 40g / min, and the welding thickness is 2.4mm. Then, the 2.4mm thick alloy layer is processed to a thickness of 2.2mm to obtain the finished valve stem.
Claims
1. A method of surfacing a steam turbine valve stem surface with a surfacing material, the method comprising: The powder of the surfacing material is prepared by water atomization or gas atomization process, and the powder composition is 2.5-3wt% of Ni, 9-10wt% of Fe, 13-15wt% of Mn, 7-8wt% of Si, 2.5-3wt% of W, 7.5-8wt% of B, and the rest is Co; the powder with a particle size of 50-150 microns is screened, and then the powder is surfacing to the surface of the valve stem and the valve head by using the laser cladding technology; after the surfacing is completed, the surface of the surfacing layer is machined to meet the size requirements; The specific surfacing process is that the surfacing laser power is controlled at 400-800W, the scanning speed is controlled at 400-500mm / min, the laser spot diameter is controlled at 0.5-1mm, and the powder feeding rate is 30-40g / min.
Citation Information
Patent Citations
Laser-cladding cobalt-based alloy powder and method for preparing same
CN102912189A