High-temperature alloy waste powder recycling method
The treatment of high-temperature alloy waste powder through thermal isostatic pressure and vacuum self-consumption smelting methods has solved the problem of increasing non-metallic inclusions and gas content in the waste powder, and achieved efficient recycling and purity improvement of high-temperature alloy waste powder.
Patent Information
- Application Number
- CN202411237073.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-06
AI Technical Summary
After screening of high-temperature alloy powder, waste powder with particle size does not meet the requirements contains non-metallic inclusions, especially fine powder, which increases the gas content with the placement time, resulting in processing difficulties.
Using thermal isostatic pressure and vacuum self-consumption smelting methods, high-temperature alloy waste powder is loaded into the package for welding and thermal isostatic pressure treatment, and then electrode processing and vacuum self-consumption smelting are carried out. Arc-starting and stable smelting are controlled through different process parameters. and the shrinkage period to achieve purification of high-temperature alloy waste powder.
The high-temperature alloy waste powder is converted into vacuum self-consumable ingots with higher purity, realizing the efficient recycling of high-temperature alloy waste powder, solving the problems of waste powder treatment and purity improvement.
Smart Images

Figure CN119076958A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of high-temperature alloy powder metallurgy, and in particular to a method for recycling waste high-temperature alloy powder. Background Art
[0002] After obtaining high-temperature alloy powder by plasma rotating electrode or compressed gas atomization, these high-temperature alloy powders need to be further screened to obtain high-temperature alloy powder with a particle size that meets the use requirements. High-temperature alloy powder whose particle size does not meet the use requirements after screening is called waste powder. Waste powder contains a certain amount of non-metallic inclusions, which are inherited from the preparation of the master alloy. Waste powder is divided into fine powder and coarse powder. Particle size ≤50μm is called fine powder, and particle size ≥150μm is called coarse powder. Compared with coarse powder, fine powder has significantly more gas content as the storage time increases. How to deal with waste high-temperature alloy powder has become a major problem for current powder preparation companies. Summary of the invention
[0003] The purpose of the present invention is to provide a method for recycling waste high-temperature alloy powder, which solves the problem of high-temperature alloy waste powder treatment. To achieve the above purpose, the present invention provides the following technical solution: a method for recycling waste high-temperature alloy powder, specifically comprising the following steps:
[0004] S1. Package preparation: Select the package of specified material and process it into specific specifications;
[0005] S2, powder loading and welding: the high temperature alloy waste powder is loaded into the package under vacuum conditions, and then welding is performed;
[0006] S3, hot isostatic pressing: placing the bag containing the high-temperature alloy waste powder in a hot isostatic pressing furnace for hot isostatic pressing;
[0007] S4, electrode processing: turning the electrode after hot isostatic pressing;
[0008] S5. Vacuum consumable melting: The electrode after turning is subjected to vacuum consumable melting, which includes arc starting period, stable melting period and shrinkage feeding period in sequence. When the pre-vacuum and leakage rate meet the requirements, power melting can be started. The arc starting period is 3-5 minutes, and then inert gas is added after entering the stable melting period to strengthen the cooling of the molten steel. Finally, the shrinkage feeding period is entered. After the melting is completed, vacuum cooling is carried out for 30 minutes before the furnace is removed.
[0009] Preferably, the sheath in S1 is made of 304 stainless steel, the inner wall diameter of the sheath is Φ68±0.05mm, the length of the sheath is 1450±1mm, the wall thickness of the sheath is 15mm, and the cylindricity of the sheath is 0.08mm.
[0010] Preferably, the vacuum degree in S2 is ≤0.5Pa, the weight ratio of fine powder to coarse powder in the high-temperature alloy waste powder is 1:1, and the welding method is vacuum electron beam welding.
[0011] Preferably, the hot isostatic pressing temperature in S3 is 10-50°C higher than the complete melting temperature of γ′, the hot isostatic pressing pressure is ≥120MPa, and the holding time is ≤2h.
[0012] Preferably, the diameter of the electrode in S4 is Φ64±1 mm, and the length of the electrode is 1400-1450 mm.
[0013] Preferably, the inner diameter of the vacuum consumable crystallizer in S5 is Φ85±0.1mm, and the effective length is 900±1mm; the arc starting period, stable melting period and feeding period of vacuum consumable melting are all controlled by current + voltage, the arc starting period current is 1.0-2.0kA, the voltage is 22.0-25.0V; the stable melting period current is 2.2-3.8kA, the voltage is 24.0-26.0V; the feeding period current gradually decreases from the stable melting period to 0.7-1.8kA, and the voltage gradually decreases from the stable melting period to 18.0-22.0V; the pre-vacuum before the arc starting period is ≤0.5Pa, and the leakage rate is ≤0.5Pa / min. The inert gas filled in the stable melting period is He gas, and the filling pressure is 300-1200Pa.
[0014] The beneficial effect of the present invention is that high-temperature alloy waste powder whose particle size does not meet the use requirements after screening can be prepared into vacuum consumable smelting electrodes through hot isostatic pressing. After vacuum consumable smelting, the electrode can obtain a vacuum consumable ingot with higher purity. The vacuum consumable ingot can be used for powder preparation again, thereby realizing efficient recycling of high-temperature alloy waste powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION
[0016] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] Example 1: Recycling of GH4169 high temperature alloy waste powder
[0018] S1. Packaging preparation
[0019] The material of the sleeve is 304 stainless steel, the inner wall diameter is Φ68mm, the length is 1450mm, the wall thickness is 15mm, and the cylindricity is 0.08mm.
[0020] S2. Powder loading and welding: The high-temperature alloy waste powder is loaded into the package under the vacuum condition of 0.4Pa, and the weight ratio of fine powder to coarse powder in the high-temperature alloy waste powder is 1:1, and then vacuum electron beam welding is used for welding. The particle size of the fine powder used is ≤20μm, and the particle size of the coarse powder used is ≥70μm.
[0021] S3. Hot isostatic pressing: Place the bag containing the high-temperature alloy waste powder in a hot isostatic pressing furnace for hot isostatic pressing. The hot isostatic pressing temperature is 1050°C, the hot isostatic pressing pressure is 120MPa, and the holding time is 1.0h.
[0022] S4. Electrode processing: The electrode after hot isostatic pressing is turned. The electrode diameter after turning is Φ64mm and the electrode length is 1400mm.
[0023] S5. Vacuum consumable melting: The electrode after turning is subjected to vacuum consumable melting, and the inner diameter of the crystallizer is Φ85mm and the effective length is 900mm. After loading the furnace, the pre-vacuum is tested to be 0.05Pa and the leakage rate is 0.12Pa / min, and melting can begin. The detailed process parameters for each period are as follows:
[0024] The arc starting period adopts current + voltage control, the current is set to 1.2kA, the voltage is set to 22.5V, and the time is set to 3min.
[0025] The stable melting period adopts current + voltage control, the current is set to 2.5kA, the voltage is set to 24.2V, and the time is set to 30min. The He gas adopts pressure control, and the pressure is 800Pa.
[0026] The feeding period was controlled by current + voltage, with the current set to 1.5 kA, the voltage set to 19.0 V, and the time set to 5 min. The starting weight of the feeding period was 6.0 kg, and the ending weight was 0.5 kg.
[0027] Example 2: Recycling of FGH4096 high temperature alloy waste powder
[0028] S1. Packaging preparation
[0029] The material of the sleeve is 304 stainless steel, the inner wall diameter is Φ68mm, the length is 1450mm, the wall thickness is 15mm, and the cylindricity is 0.08mm.
[0030] S2. Powder loading and welding: The high-temperature alloy waste powder is loaded into the package under the vacuum condition of 0.3Pa, and the weight ratio of fine powder to coarse powder in the high-temperature alloy waste powder is 1:1, and then vacuum electron beam welding is used for welding. The particle size of the fine powder used is ≤50μm, and the particle size of the coarse powder used is ≥120μm.
[0031] S3. Hot isostatic pressing: Place the bag containing the high-temperature alloy waste powder in a hot isostatic pressing furnace for hot isostatic pressing. The hot isostatic pressing temperature is 1160°C, the hot isostatic pressing pressure is 120MPa, and the holding time is 1.0h.
[0032] S4. Electrode processing: The electrode after hot isostatic pressing is turned. The electrode diameter after turning is Φ64mm and the electrode length is 1400mm.
[0033] S5. Vacuum consumable melting: The electrode after turning is subjected to vacuum consumable melting, and the inner diameter of the crystallizer is Φ85mm and the effective length is 900mm. After loading the furnace, the pre-vacuum is tested to be 0.04Pa and the leakage rate is 0.10Pa / min, and melting can begin. The detailed process parameters for each period are as follows:
[0034] The arc starting period adopts current + voltage control, the current is set to 1.5kA, the voltage is set to 23.0V, and the time is set to 3min.
[0035] The stable melting period adopts current + voltage control, the current is set to 2.2kA, the voltage is set to 24.5V, and the time is set to 30min. The He gas adopts pressure control, and the pressure is 800Pa.
[0036] The feeding period was controlled by current + voltage, with the current set to 1.6 kA, the voltage set to 18.5 V, and the time set to 5 min. The starting weight of the feeding period was 6.0 kg, and the ending weight was 0.5 kg.
[0037] Example 2: Recycling of FGH4097 high temperature alloy waste powder
[0038] S1. Packaging preparation
[0039] The material of the sleeve is 304 stainless steel, the inner wall diameter is Φ68mm, the length is 1450mm, the wall thickness is 15mm, and the cylindricity is 0.08mm.
[0040] S2. Powder loading and welding: The high-temperature alloy waste powder is loaded into the package under the vacuum condition of 0.3Pa, and the weight ratio of fine powder to coarse powder in the high-temperature alloy waste powder is 1:1, and then vacuum electron beam welding is used for welding. The particle size of the fine powder used is ≤50μm, and the particle size of the coarse powder used is ≥120μm.
[0041] S3. Hot isostatic pressing: Place the bag containing the high-temperature alloy waste powder in a hot isostatic pressing furnace for hot isostatic pressing. The hot isostatic pressing temperature is 1200°C, the hot isostatic pressing pressure is 120MPa, and the holding time is 1.0h.
[0042] S4. Electrode processing: The electrode after hot isostatic pressing is turned. The electrode diameter after turning is Φ64mm and the electrode length is 1400mm.
[0043] S5. Vacuum consumable melting: The electrode after turning is subjected to vacuum consumable melting, and the inner diameter of the crystallizer is Φ85mm and the effective length is 900mm. After loading the furnace, the pre-vacuum is tested to be 0.04Pa and the leakage rate is 0.10Pa / min, and melting can begin. The detailed process parameters for each period are as follows:
[0044] The arc starting period adopts current + voltage control, the current is set to 1.8kA, the voltage is set to 23.2V, and the time is set to 3min.
[0045] The stable melting period adopts current + voltage control, the current is set to 2.4kA, the voltage is set to 24.7V, and the time is set to 30min. The He gas adopts pressure control, and the pressure is 800Pa.
[0046] The feeding period was controlled by current + voltage, with the current set to 1.7 kA, the voltage set to 18.5 V, and the time set to 5 min. The starting weight of the feeding period was 6.0 kg, and the ending weight was 0.5 kg.
Claims
1. A method for recycling waste high-temperature alloy powder, It is characterized in that The following steps are involved: S1. Package preparation: Select the package of specified material and process it into specific specifications; S2, powder loading and welding: the high temperature alloy waste powder is loaded into the package under vacuum conditions, and then welding is performed; S3, hot isostatic pressing: placing the bag containing the high-temperature alloy waste powder in a hot isostatic pressing furnace for hot isostatic pressing; S4, electrode processing: turning the electrode after hot isostatic pressing; S5. Vacuum consumable melting: The electrode after turning is subjected to vacuum consumable melting, which includes arc starting period, stable melting period and feeding period in sequence. When the pre-vacuum and leakage rate meet the requirements, power melting can be started. The arc starting period is 3-5 minutes, and then inert gas is added after entering the stable melting period to strengthen the cooling of the molten steel, and finally enters the feeding period. After the melting is completed, vacuum cooling is carried out for 30 minutes before the furnace is removed.
2. A method for recycling waste high-temperature alloy powder according to claim 1, Features: The material of the sheath in S1 is 304 stainless steel, the inner wall diameter of the sheath is Φ68±0.05mm, the length of the sheath is 1450±1mm, the wall thickness of the sheath is 15mm, and the cylindricity of the sheath is 0.08mm.
3. A method for recycling waste high-temperature alloy powder according to claim 1, Features: The vacuum degree in S2 is ≤0.5Pa, the weight ratio of fine powder to coarse powder in the high-temperature alloy waste powder is 1:1, and the welding method is vacuum electron beam welding.
4. A method for recycling waste high-temperature alloy powder according to claim 1, Features: The hot isostatic pressing temperature in S3 is 10-50° C. higher than the complete melting temperature of γ′, the hot isostatic pressing pressure is ≥120 MPa, and the holding time is ≤2 h.
5. A method for recycling waste high-temperature alloy powder according to claim 1, Features: The diameter of the electrode in S4 is Φ64±1 mm, and the length of the electrode is 1400-1450 mm.
6. A method for recycling waste high-temperature alloy powder according to claim 1, Features: The inner diameter of the vacuum consumable crystallizer in S5 is Φ85±0.1mm, and the effective length is 900±1mm; the arc starting period, stable melting period and feeding period of the vacuum consumable melting are all controlled by current + voltage, the current in the arc starting period is 1.0-2.0kA, and the voltage is 22.0-25.0V; the current in the stable melting period is 2.2-3.8kA, and the voltage is 24.0-26.0V; the current in the feeding period gradually decreases from the stable melting period to 0.7-1.8kA, and the voltage gradually decreases from the stable melting period to 18.0-22.0V; the pre-vacuum before the arc starting period is ≤0.5Pa, and the leakage rate is ≤0.5Pa / min. The inert gas filled in the stable melting period is He gas, and the filling pressure is 300-1200Pa.
Citation Information
Cited By
Remediation method for tungsten powder high-speed steel hot isostatic pressing process defects and application thereof
CN120347210A
Remedial methods and applications for defects in the hot isostatic pressing process of tungsten-based powder high-speed steel.
CN120347210B
Device and method for high-efficiency and low-energy-consumption recovery and regeneration of high-temperature alloy powder
CN120480200A