A high-temperature resistant mesh double-sided adhesive tape for use between a support membrane and a foam layer and its preparation method.
By designing a combination of mesh and non-mesh adhesive layers, the problem of double-sided tape warping under high temperature conditions was solved, achieving temperature resistance and anti-warping properties for flexible OLED displays. This ensures that the tape does not detach from the support film and foam at high temperatures, protecting the OLED devices.
Patent Information
- Application Number
- CN202311628876.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-30
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-11-30
AI Technical Summary
Existing double-sided tapes are prone to warping under high temperatures, which can damage flexible OLED devices. They are also prone to detachment during disassembly, failing to meet the temperature resistance and warping resistance requirements of flexible OLED displays.
The high-temperature resistant double-sided tape is composed of a mesh release film layer, a mesh adhesive layer, a polyester film layer, a non-mesh adhesive layer, and a plain release film layer. The mesh adhesive layer and the non-mesh adhesive layer are respectively combined with specific proportions of acrylate polymer, rosin and phenol polymer, rosin ester and curing agent, which improves the cohesion and anti-warping properties of the adhesive layer.
Maintaining good adhesion and anti-warping properties in high-temperature environments prevents damage to OLED devices and meets the requirements for use and disassembly of flexible OLED displays.
Smart Images

Figure CN117487471B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials, specifically to a high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer, and its preparation method. Background Technology
[0002] Flexible OLEDs, as an important development direction in the semiconductor display field, are attracting increasing market attention. Because of their flexibility, flexible OLED devices are susceptible to scratches, contamination, and breakage during transportation and assembly. Therefore, to improve the cushioning and protection of flexible OLEDs, some flexible display modules incorporate a support film and foam on the back of the flexible display panel. Double-sided adhesive tape is required to bond the support film and foam together.
[0003] Foam substrates are mostly made of foamed plastic particles, and their surfaces often have an uneven microstructure. Therefore, during the foam bonding process, residual gas inevitably remains between the foam and the adhesive tape. When environmental factors such as air pressure and temperature change, the pressure difference between the residual gas and the external environment creates a force that causes the adhesive tape to bulge. Furthermore, during actual use after assembly, the surface temperature of OLED displays often reaches 70°C or higher due to the heat generated by electronic components and external heat sources. When an OLED display needs repair, the disassembly process can reach temperatures exceeding 80°C. This necessitates that the double-sided adhesive tape used between the support film and the foam possess high temperature resistance and anti-warping properties to prevent damage to the OLED devices during disassembly. Summary of the Invention
[0004] The purpose of this invention is to provide a high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer, and a method for preparing the same, in order to solve the problems mentioned in the background art.
[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution:
[0006] A high-temperature resistant double-sided mesh adhesive tape for use between a support film and a foam layer comprises a mesh release film layer, a mesh adhesive layer, a polyester film layer, a non-mesh adhesive layer, and a plain release film layer, stacked sequentially. The mesh adhesive layer is adhered to the support film, and the non-mesh adhesive layer is adhered to the foam layer. The mesh adhesive layer comprises an acrylate polymer, a polymer of rosin and phenol, rosin ester, and a curing agent in a mass ratio of (33-40):(2-4):(2-4):(0.5-1), wherein the rosin ester is Arakawa GB-75 and Arakawa GA-AT in a mass ratio of (3-4):1, and the curing agent is an aromatic polyisocyanate curing agent.
[0007] Furthermore, the glass transition temperature (Tg) of the mesh adhesive layer is -10 to 12°C. At room temperature (23°C), the loss modulus G″ is 60-140 kPa, the storage modulus G′ is 150-200 kPa, and the loss factor tanδ is 0.4-0.5. At high temperature (85°C), the loss modulus G″ is 15-35 kPa, the storage modulus G′ is 25-55 kPa, and the loss factor tanδ is 0.6-0.7.
[0008] Furthermore, when the mesh adhesive layer is used to bond the substrate to the SUS board and the support film, the 180° peel force at room temperature (23°C) is >1600gf / in for SUS and >1200gf / in for the support film; at high temperature (85°C), the peel force at room temperature is >1200gf / in for SUS and >800gf / in for the support film; and the holding force at 85°C for 72 hours results in a sliding distance ≤0.1mm.
[0009] Furthermore, the non-mesh adhesive layer comprises an acrylate polymer and a curing agent in a mass ratio of (18-25):(0.1-0.5), wherein the curing agent is an epoxy curing agent.
[0010] Furthermore, the glass transition temperature (Tg) of the non-mesh adhesive layer is -13 to 5℃. At room temperature (23℃), the loss modulus G″ is 80-120 kPa, the storage modulus G′ is 220-270 kPa, and the loss factor tanδ is 0.4-0.5. At high temperature (85℃), the loss modulus G″ is 20-30 kPa, the storage modulus G′ is 90-100 kPa, and the loss factor tanδ is 0.5-0.6.
[0011] Furthermore, when the non-mesh adhesive layer is used to bond SUS board and foam as substrates, the 180° peel force at room temperature (23°C) is >1200gf / in for SUS and >700gf / in for foam, and at high temperature (85°C) it is >800gf / in for SUS and >450gf / in for foam. The holding force at 85°C for 72 hours results in a sliding distance ≤0.1mm.
[0012] Furthermore, the raw materials for preparing the acrylate polymer of the mesh adhesive layer include, by mass parts: 48-60 parts of ethyl acrylate, 1-5 parts of hydroxyethyl acrylate, 25-35 parts of isobutyl methacrylate, 2-5 parts of methacrylic acid, 1-4 parts of isobornyl methacrylate, 1-3 parts of initiator, and 150-190 parts of solvent. The solid content of the acrylate polymer in the mesh adhesive layer is 33-40%. The initiator is a free radical initiator, and the solvent is ethyl acetate and acetone in a mass ratio of (6-4):1.
[0013] Furthermore, the method for preparing the acrylate polymer of the mesh adhesive layer includes the following steps:
[0014] S1. Weigh out ethyl acrylate, hydroxyethyl acrylate, isobutyl methacrylate, methacrylic acid, isobornyl methacrylate and solvent according to the formula. Mix all monomers and part of the solvent evenly and pour into a reactor with a condenser. Heat to 60-70℃ under nitrogen protection.
[0015] S2. Dissolve half of the total mass of the initiator in a solvent and add it dropwise evenly to the reactor, and keep the reaction at the temperature for 1-3 hours;
[0016] S3. Dissolve 1 / 4 of the total mass of the initiator in a solvent and add it dropwise evenly to the reactor, and heat it to 75-80℃, and keep it at this temperature for 1-2 hours; dissolve the remaining initiator in a solvent and add it dropwise evenly to the reactor, keep the temperature at 75-80℃, and keep it at this temperature for 2-3 hours.
[0017] S4. After adding the remaining solvent to dilute and stirring evenly, cool to room temperature and discharge to obtain the acrylate polymer in the mesh adhesive layer.
[0018] Furthermore, the raw materials for preparing the acrylate polymer in the non-mesh adhesive layer include, by weight, 55-70 parts of ethyl acrylate, 25-35 parts of methyl methacrylate, 3-6 parts of hydroxyethyl methacrylate, 1-2 parts of initiator, and 300-400 parts of solvent, and the solid content of the acrylate polymer in the non-mesh adhesive layer is 20-25%.
[0019] Furthermore, in the raw materials for preparing the acrylate polymer of the non-mesh adhesive layer: the initiator is a free radical initiator, and the solvent is ethyl acetate and / or butyl acetate.
[0020] Furthermore, the method for preparing the acrylate polymer of the non-mesh adhesive layer includes the following steps:
[0021] S1. Weigh out ethyl acrylate, methyl methacrylate, hydroxyethyl methacrylate and solvent according to the formula. Mix all monomers and part of the solvent evenly and pour into a reactor with a condenser. Heat to 60-70℃ under nitrogen protection.
[0022] S2. Dissolve half of the total mass of the initiator in a solvent and add it dropwise evenly to the reactor, and keep the reaction at the temperature for 1-3 hours;
[0023] S3. Dissolve 1 / 4 of the total mass of the initiator in a solvent and add it dropwise evenly to the reactor, and heat it to 75-80℃, and keep it at this temperature for 1-2 hours; dissolve the remaining initiator in a solvent and add it dropwise evenly to the reactor, keep the temperature at 75-80℃, and keep it at this temperature for 2-3 hours.
[0024] S4. After adding the remaining solvent to dilute and stirring evenly, cool to room temperature and discharge to obtain the acrylate polymer in the non-mesh adhesive layer.
[0025] Furthermore, the thickness of the high-temperature resistant mesh double-sided adhesive tape is 34-46 μm, wherein the thickness of the mesh adhesive layer is 20-24 μm, the thickness of the polyester film layer is 6-12 μm, and the thickness of the non-mesh adhesive layer is 8-12 μm;
[0026] Furthermore, the thickness of the grid release film layer is 100-150μm, and the thickness of the plain release film layer is 20-100μm.
[0027] This invention also discloses a method for preparing a high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer, comprising the following steps:
[0028] S1. Mix the acrylate polymer of the mesh adhesive layer, the polymer of rosin and phenol, rosin ester, curing agent and solvent according to the mass ratio, stir and ultrasonically disperse to obtain adhesive mixture A; mix the acrylate polymer and curing agent of the non-mesh adhesive layer according to the mass ratio, stir and ultrasonically disperse to obtain adhesive mixture B.
[0029] S2. Apply adhesive mixture A to the release surface of the mesh release film, and after drying and curing in 6 temperature zones, obtain the mesh adhesive layer. After bonding it to the printed surface of the black printed PET substrate, obtain the semi-finished product.
[0030] S3. Apply adhesive mixture B to the release surface of the plain release film, and after drying and curing in 6 temperature zones, a non-mesh adhesive layer is obtained. After bonding it with the semi-finished product, a high-temperature resistant mesh double-sided tape is obtained.
[0031] Furthermore, the coating method is blade coating, and the drying temperatures for the six temperature zones are 55℃, 65℃, 80℃, 100℃, 110℃ and 90℃, respectively.
[0032] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0033] This invention introduces carboxyl and hydroxyl functional groups into the acrylate polymer of the mesh adhesive layer, and combines it with a mixed rosin ester containing carboxyl functional groups, as well as a polymer of rosin and phenol. By rationally determining the mass ratio of GB-75 to GA-AT in the mixed rosin ester, the acrylate polymer can crosslink with both the curing agent and the polymer of mixed rosin ester, rosin, and phenol during the curing process. This significantly improves the tightness of the molecular chain arrangement, thereby enhancing the cohesiveness and anti-warping properties of the mesh adhesive layer and preventing the migration and precipitation of low molecular weight rosin esters. This ensures that the mesh adhesive layer maintains good adhesion to the support film under high temperature and high humidity conditions. Through the rational selection and proportioning of the polymerization raw materials and curing agents of the acrylate polymer in the non-mesh adhesive layer, the influence of the crosslinking density of the non-mesh adhesive layer on the cohesiveness and anti-warping properties is effectively balanced, ensuring that the non-mesh adhesive layer still exhibits good adhesion and anti-warping properties to the foam under high temperature and high humidity conditions. Attached Figure Description
[0034] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the embodiments of the invention to explain the invention and do not constitute a limitation thereof.
[0035] Figure 1 This is a schematic diagram of a high-temperature resistant mesh double-sided adhesive tape structure used between a support film and a foam layer according to the present invention.
[0036] In the diagram, 1: mesh release film layer, 2: mesh adhesive layer, 3: polyester film layer, 4: non-mesh adhesive layer, and 5: plain release film layer. Detailed Implementation
[0037] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0038] The types and purchase channels of the rosin ester, rosin and phenol polymers and curing agents used in the embodiments of the present invention are as follows:
[0039] Rosin ester, GB-75, Arakawa Chemical;
[0040] Rosin ester, GA-AT, Arakawa Chemical;
[0041] Polymer of rosin and phenol, CAS 68083-03-4, Arakawa Chemicals;
[0042] Curing agent A for the mesh adhesive layer, L75, Bayer, Germany;
[0043] Curing agent B for non-mesh adhesive layer, Y-202, Anzo Chemical.
[0044] Example 1:
[0045] S1. Preparation of acrylate polymer A for the mesh adhesive layer:
[0046] By mass, 58 parts of ethyl acrylate, 34 parts of isobutyl methacrylate, 2 parts of hydroxyethyl acrylate, 3 parts of methacrylic acid, 3 parts of isobornyl methacrylate, 110 parts of ethyl acetate, and 25 parts of acetone were mixed and poured into a reactor equipped with a stirrer, condenser, and thermometer. The mixture was heated to 68±1℃ under nitrogen protection. 0.8 parts of azobisisobutyronitrile (AIBN) were dissolved in 7 parts of ethyl acetate and added to the reactor to initiate the reaction. The temperature was maintained at 68±1℃ for 2 hours. Then, 0.4 parts of AIBN dissolved in 4 parts of ethyl acetate were added, and the temperature was raised to 80±1℃ for 1 hour. Finally, 0.4 parts of AIBN dissolved in 4 parts of ethyl acetate were added to the reactor, and the temperature was maintained at 80±1℃ for 2 hours. The remaining 15 parts of ethyl acetate were added for dilution and stirred until homogeneous. The mixture was then cooled to room temperature and discharged to obtain acrylate polymer A with a solid content of 38%.
[0047] S2. Preparation of acrylate polymer B for non-mesh adhesive layer:
[0048] Mix 67 parts ethyl acrylate, 28 parts methyl methacrylate, 5 parts hydroxyethyl methacrylate, and 200 parts ethyl acetate, and pour the mixture into a reactor equipped with a stirrer, condenser, and thermometer. Under nitrogen protection, heat to 68±1℃. Dissolve 0.6 parts azobisisobutyronitrile (AIBN) in 6 parts ethyl acetate and add it to the reactor to initiate the reaction. Maintain the temperature at 65±1℃ for 2 hours. Then add 0.3 parts AIBN dissolved in 3 parts ethyl acetate and raise the temperature to 80±1℃, maintaining the temperature for 1 hour. Finally, add another 0.3 parts AIBN dissolved in 3 parts ethyl acetate to the reactor, maintaining the temperature at 80±1℃ for 2 hours. Dilute with the remaining 158 parts ethyl acetate and stir until homogeneous. Cool to room temperature and discharge to obtain acrylate polymer B with a solid content of 21%.
[0049] S3. A method for preparing a mesh double-sided adhesive tape, comprising the following steps:
[0050] By weight, 100 parts of acrylate polymer A, 3 parts of rosin and phenol polymer, 3 parts of rosin ester GB-75, 1 part of rosin ester GA-AT, 1 part of curing agent A, and 24 parts of ethyl acetate were mixed and stirred, and then ultrasonically dispersed to obtain glue mixture A with a solid content of 35%; 100 parts of acrylate polymer B and 0.1 parts of curing agent B were mixed and stirred, and then ultrasonically dispersed to obtain glue mixture B with a solid content of 21%.
[0051] Adhesive mixture A is applied to the release surface of a mesh release film. After drying and curing in six temperature zones, a mesh adhesive layer with a thickness of 22βm is obtained. This mesh adhesive layer is then laminated to the printed surface of an 8βm thick black printed PET substrate to obtain a semi-finished product. Adhesive mixture B is applied to the release surface of a plain weave release film. After drying and curing in six temperature zones, a non-mesh adhesive layer with a thickness of 11βm is obtained. This non-mesh adhesive layer is then laminated to the semi-finished product to obtain a mesh double-sided adhesive tape. The coating method is blade coating, with a linear speed of 5 m / min and a blade air pressure of 0.1 MPa. The temperatures of the six temperature zones are set sequentially as follows: 55℃, 65℃, 80℃, 100℃, 110℃, and 90℃, with a tension of 70 N.
[0052] Example 2:
[0053] S1. Preparation of acrylate polymer A for the mesh adhesive layer:
[0054] By mass, 60 parts of ethyl acrylate, 32 parts of isobutyl methacrylate, 1.5 parts of hydroxyethyl acrylate, 3.5 parts of methacrylic acid, 3 parts of isobornyl methacrylate, 130 parts of ethyl acetate, and 25 parts of acetone were mixed and poured into a reactor equipped with a stirrer, condenser, and thermometer. The mixture was heated to 68±1℃ under nitrogen protection. 0.8 parts of azobisisobutyronitrile (AIBN) were dissolved in 7 parts of ethyl acetate and added to the reactor to initiate the reaction. The temperature was maintained at 68±1℃ for 2 hours. Then, 0.4 parts of AIBN dissolved in 4 parts of ethyl acetate were added, and the temperature was raised to 80±1℃ for 1 hour. Finally, 0.4 parts of AIBN dissolved in 4 parts of ethyl acetate were added to the reactor, and the temperature was maintained at 80±1℃ for 2 hours. The remaining 15 parts of ethyl acetate were added for dilution and stirred until homogeneous. The mixture was then cooled to room temperature and discharged to obtain acrylate polymer A with a solid content of 35%.
[0055] S2. Preparation of acrylate polymer B for non-mesh adhesive layer:
[0056] 70 parts ethyl acrylate, 25 parts methyl methacrylate, 5 parts hydroxyethyl methacrylate, and 170 parts ethyl acetate were mixed and poured into a reactor equipped with a stirrer, condenser, and thermometer. The mixture was heated to 68±1℃ under nitrogen protection. 0.6 parts azobisisobutyronitrile (AIBN) was dissolved in 6 parts ethyl acetate and added to the reactor to initiate the reaction. The temperature was maintained at 65±1℃ for 2 hours. Then, 0.3 parts AIBN dissolved in 3 parts ethyl acetate was added, and the temperature was raised to 80±1℃ for 1 hour. Finally, 0.3 parts AIBN dissolved in 3 parts ethyl acetate was added to the reactor, and the temperature was maintained at 80±1℃ for 2 hours. The remaining 158 parts ethyl acetate were added for dilution and stirred until homogeneous. The mixture was then cooled to room temperature and discharged to obtain acrylate polymer B with a solid content of 23%.
[0057] S3. A method for preparing a mesh double-sided adhesive tape, comprising the following steps:
[0058] By weight, 100 parts of acrylate polymer A, 4 parts of rosin and phenol polymer, 3 parts of rosin ester GB-75, 1 part of rosin ester GA-AT, 1 part of curing agent A, and 18 parts of ethyl acetate were mixed and stirred, and then ultrasonically dispersed to obtain glue mixture A with a solid content of 35%; 100 parts of acrylate polymer B and 0.1 parts of curing agent B were mixed and stirred, and then ultrasonically dispersed to obtain glue mixture B with a solid content of 23%.
[0059] Adhesive mixture A is applied to the release surface of a mesh release film. After drying and curing in six temperature zones, a mesh adhesive layer with a thickness of 22βm is obtained. This mesh adhesive layer is then laminated to the printed surface of an 8βm thick black printed PET substrate to obtain a semi-finished product. Adhesive mixture B is applied to the release surface of a plain weave release film. After drying and curing in six temperature zones, a non-mesh adhesive layer with a thickness of 11βm is obtained. This non-mesh adhesive layer is then laminated to the semi-finished product to obtain a mesh double-sided adhesive tape. The coating method is blade coating, with a linear speed of 5 m / min and a blade air pressure of 0.1 MPa. The temperatures of the six temperature zones are set sequentially as follows: 55℃, 65℃, 80℃, 100℃, 110℃, and 90℃, with a tension of 70 N.
[0060] Comparative Example 1:
[0061] The same method as in Example 1 was used to prepare the mesh double-sided tape, except that petroleum resin was used instead of rosin and phenol polymer.
[0062] Comparative Example 2:
[0063] The same method as in Example 1 was used to prepare the grid double-sided tape, except that Arakawa GB-120 was used instead of GB-75 as the rosin ester.
[0064] Comparative Example 3:
[0065] The same method as in Example 1 was used to prepare the mesh double-sided tape, except that Arakawa GA-85H was used instead of GA-AT as the rosin ester.
[0066] Comparative Example 4:
[0067] The same method as in Example 1 was used to prepare the mesh double-sided tape, except that only rosin ester GB-75 was added, and the amount of rosin ester GB-75 added was 4 parts by weight.
[0068] Comparative Example 5:
[0069] The same method as in Example 1 was used to prepare the mesh double-sided tape, except that the amount of rosin ester GB-75 added was 0.5 parts by weight and the amount of rosin ester GA-AT added was 3.5 parts by weight.
[0070] experiment
[0071] 1. 180° peel force:
[0072] 1. Inspect the test board to see if its surface is clean and free of scratches or marks; use a lint-free cloth to apply an appropriate amount of anhydrous ethanol and wipe the surface of the test board from top to bottom. Once there is no dirt, wipe it again with a clean lint-free cloth until the surface is clean, and then let it stand for 5 minutes.
[0073] 2. Sample size: 25mm wide and 300mm long. Place the cut sample parallel to the steel plate, and gently press the sample with a small rubber roller to make it fit the test plate, ensuring that no air bubbles are present. Use a 2kg electric pressure roller to roll back and forth on the sample once at a speed of 300mm / min under its own weight, and leave it for 20 minutes.
[0074] 3. Peel the adhesive surface from the test plate along the free end of the sample. Clamp and fix the free end of the sample and the test plate on the upper and lower clamps respectively. The peeling surface must be aligned with the force line of the peeling test machine (180°). Peel the tape on the tensile test machine at a speed of 300 mm / min. The peeling force is the average value of the stroke of 50 mm-150 mm.
[0075] 4. Repeat the above experiment and take the average of the three test values as the final value.
[0076] II. Holding Force:
[0077] 1. Inspect the test board to check if its surface is clean and free of scratches or marks; wipe the test board clean with anhydrous ethanol and a lint-free cloth, and let it air dry at room temperature for 5 minutes.
[0078] 2. Sample size: 25mm wide and 100mm long. Use a roller to flatten the cut sample onto the test plate (25mm*20mm bonding area), and then manually roll it back and forth 3 times with a rubber pressure roller (2kg) to make it bond with the steel plate (no air bubbles are allowed between the steel plate and the sample).
[0079] 3. After the sample is prepared, let it stand for 20 minutes, then hang it in the holding force tester and add a 1KG weight;
[0080] 4. Record the time when the steel plate falls. If no steel plate falls, record the distance the spline moves down within 48 hours. The result is expressed as the time when the steel plate falls or the distance the spline moves down.
[0081] III. Leveling performance:
[0082] 1. Inspect the test board to see if its surface is clean and free of scratches or marks; wipe the test board clean with anhydrous ethanol and a lint-free cloth, and let it air dry at room temperature for 5 minutes. The test board is a glass plate and the object to be attached.
[0083] 2. Sample size: 50mm wide and 150mm long. Use a roller to flatten the cut sample onto the test plate, and then use a rubber roller (2kg) to manually roll it back and forth 3 times to make it adhere to the test plate (no air bubbles are allowed between the test plate and the sample).
[0084] 3. After the sample is prepared and left to stand for 20 minutes, fix the sample at the top, middle and bottom points respectively, observe and record the grid morphology at T0 on the back of the test plate with a microscope, and then observe and record the leveling situation every 12 hours until it is completely leveled.
[0085] 4. Repeat the above experiment and take the average of the three test values as the final value.
[0086] Performance data for the grid surfaces of each embodiment and comparative example (BP represents the supporting membrane):
[0087]
[0088] Performance data for the non-mesh surfaces of each embodiment and comparative example:
[0089]
[0090] The data in the table above shows a comparison of the key performance data obtained from Examples 1-2 and Comparative Examples 1-5. The test results indicate that the mesh side of the double-sided adhesive tape obtained in Examples 1-2 exhibits excellent high-temperature resistance, demonstrating sufficient adhesion to SUS and the support film at both room temperature and 85°C without easily detaching. The non-mesh side also exhibits good high-temperature resistance, showing sufficient adhesion to SUS and acrylic foam at both room temperature and 85°C without easily detaching. Furthermore, no adhesive residue remains on the surface of the adhered object after tape removal, meeting the bonding requirements for practical applications and disassembly / repair processes in OLED modules. As a mesh adhesive surface, it can completely level within 24 hours, achieving a high degree of adhesion to the adhered object, thus possessing both excellent temperature resistance and excellent rapid leveling properties.
[0091] Compared to Example 1, the resin types used in Comparative Examples 1, 2, and 3 are not within the scope defined in this application. In Comparative Example 1, petroleum resin was used to replace rosin and phenol in the polymer. According to the test results, the peel strength at room temperature and high temperature in Comparative Example 1 was significantly reduced, and the high temperature holding power and leveling performance were poor, failing to meet the application requirements. In Comparative Examples 2 and 3, Arakawa GB-120 and Arakawa GA-85H were used to replace Arakawa GB-75 and Arakawa GA-AT, respectively. According to the test results, the peel strength of the support film at room temperature and high temperature in Comparative Examples 2 and 3 was poor, and the high temperature holding power was easy to detach. Furthermore, there was residual adhesive on the surface of the adhered object after removal, failing to meet the application requirements.
[0092] Compared to Example 1, Comparative Example 4 only added rosin ester GB-75. The test results showed that although its peel strength and holding power at room temperature and high temperature met the performance requirements, its leveling properties were reduced, resulting in insufficient adhesion between it and the substrate, and adhesive residue remained on the substrate after removal.
[0093] Compared to Example 1, the mass ratio of rosin ester added in Comparative Example 5 was outside the defined range, being less than the defined ratio; the mass ratio of rosin ester GB-75 to rosin ester GA-AT was 1:7. According to the test results, this method resulted in good leveling properties on the adhesive surface, but it sacrificed temperature resistance. High-temperature peel strength and high-temperature holding power both decreased significantly, rendering it ineffective for practical applications.
[0094] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0095] For those skilled in the art, various modifications and improvements can be made without departing from the concept of the present invention, and these modifications and improvements are all within the scope of protection of the present invention. The scope of protection of the present invention is defined by the appended claims.
Claims
1. A high-temperature resistant double-sided mesh tape for use between a support film and a foam layer, characterized in that, It consists of a grid release film layer, a grid adhesive layer, a polyester film layer, a non-grid adhesive layer, and a plain release film layer stacked sequentially; The mesh adhesive layer is adhered to the support membrane, and the non-mesh adhesive layer is adhered to the foam layer; the mesh adhesive layer comprises an acrylate polymer, a rosin and phenol polymer, a rosin ester and a curing agent in a mass ratio of (33-40):(2-4):(2-4):(0.5-1), wherein the rosin ester is Arakawa GB-75 and Arakawa GA-AT in a mass ratio of (3-4):1, and the curing agent is an aromatic polyisocyanate curing agent; The non-mesh adhesive layer comprises an acrylate polymer and a curing agent in a mass ratio of (18-25):(0.1-0.5), wherein the curing agent is an epoxy curing agent; The raw materials for preparing the acrylate polymer of the mesh adhesive layer include, by mass parts: 48-60 parts of ethyl acrylate, 1-5 parts of hydroxyethyl acrylate, 25-35 parts of isobutyl methacrylate, 2-5 parts of methacrylic acid, 1-4 parts of isobornyl methacrylate, 1-3 parts of initiator, and 150-190 parts of solvent.
2. The high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer according to claim 1, characterized in that, The glass transition temperature of the mesh adhesive layer is -10~12℃. At room temperature (23℃), the loss modulus G″ is 60-140kPa, the storage modulus G′ is 150-200kPa, and the loss factor tanδ is 0.4-0.
5. At high temperature (85℃), the loss modulus G″ is 15-35kPa, the storage modulus G′ is 25-55kPa, and the loss factor tanδ is 0.6-0.
7.
3. The high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer according to claim 1, characterized in that, When the mesh adhesive layer is used to bond SUS board and support film, the peel force at 180° at room temperature (23°C) is >1600gf / in for SUS and >1200gf / in for support film. At high temperature (85°C), the peel force is >1200gf / in for SUS and >800gf / in for support film. The holding force at 85°C for 72 hours results in a sliding distance ≤0.1mm.
4. The high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer according to claim 1, characterized in that, The glass transition temperature of the non-mesh adhesive layer is -13~5℃. At room temperature (23℃), the loss modulus G″ is 80-120kPa, the storage modulus G′ is 220-270kPa, and the loss factor tanδ is 0.4-0.
5. At high temperature (85℃), the loss modulus G″ is 20-30kPa, the storage modulus G′ is 90-100kPa, and the loss factor tanδ is 0.5-0.
6.
5. The high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer according to claim 1, characterized in that, When the non-mesh adhesive layer is used to bond SUS board and foam as substrates, the 180° peel force at room temperature (23°C) is >1200gf / in for SUS and >700gf / in for foam; at high temperature (85°C) it is >800gf / in for SUS and >450gf / in for foam; and the holding force at 85°C for 72 hours results in a sliding distance ≤0.1mm.
6. The high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer according to claim 1, characterized in that, The solid content of the acrylate polymer in the mesh adhesive layer is 33-40%, the initiator is a free radical initiator, and the solvent is ethyl acetate and acetone in a mass ratio of (6-4):
1.
7. The high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer according to claim 1, characterized in that, The method for preparing the acrylate polymer of the mesh adhesive layer includes the following steps: S1. Weigh out ethyl acrylate, hydroxyethyl acrylate, isobutyl methacrylate, methacrylic acid, isobornyl methacrylate and solvent according to the formula. Mix all monomers and part of the solvent evenly and pour into a reactor with a condenser. Heat to 60-70℃ under nitrogen protection. S2. Dissolve half of the total mass of the initiator in a solvent and add it dropwise evenly to the reactor, and keep the reaction at the temperature for 1-3 hours; S3. Dissolve 1 / 4 of the total mass of the initiator in a solvent and add it dropwise evenly to the reactor, then heat the reactor to 75-80℃ and keep it at that temperature for 1-2 hours; dissolve the remaining initiator in a solvent and add it dropwise evenly to the reactor, keeping the temperature constant at 75-80℃ and keep it at that temperature for 2-3 hours. S4. After diluting with the remaining solvent and stirring evenly, cool to room temperature and discharge to obtain the acrylate polymer in the mesh adhesive layer.
8. The high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer according to claim 1, characterized in that, The raw materials for preparing the acrylate polymer in the non-mesh adhesive layer include, by weight: 55-70 parts of ethyl acrylate, 25-35 parts of methyl methacrylate, 3-6 parts of hydroxyethyl methacrylate, 1-2 parts of initiator, and 300-400 parts of solvent. The solid content of the acrylate polymer in the non-mesh adhesive layer is 20-25%.
9. The high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer according to claim 1, characterized in that, The thickness of the high-temperature resistant mesh double-sided adhesive tape is 34-48μm, wherein the thickness of the mesh adhesive layer is 20-24μm, the thickness of the polyester film layer is 6-12μm, and the thickness of the non-mesh adhesive layer is 8-12μm.
10. A method for preparing a high-temperature resistant mesh double-sided adhesive tape for use between a support film and a foam layer according to any one of claims 1-9, characterized in that, Includes the following steps: S1. Mix the acrylate polymer, rosin and phenol polymer, rosin ester, curing agent and solvent of the mesh adhesive layer according to the mass ratio, stir and ultrasonically disperse to obtain adhesive mixture A; mix the acrylate polymer and curing agent of the non-mesh adhesive layer according to the mass ratio, stir and ultrasonically disperse to obtain adhesive mixture B; S2. Apply adhesive mixture A to the release surface of the mesh release film, and after drying and curing in 6 temperature zones, obtain the mesh adhesive layer. After bonding it to the printed surface of the polyester film layer, obtain the semi-finished product. S3. Apply adhesive mixture B to the release surface of the plain release film, and after drying and curing in 6 temperature zones, a non-mesh adhesive layer is obtained. After bonding it with the semi-finished product, a high-temperature resistant mesh double-sided tape is obtained.
Citation Information
Patent Citations
Ultrathin single-sided grid PET double-sided adhesive tape and preparation method thereof
CN111378394A
Rapid leveling ultra-thin grid adhesive tape and preparation method thereof