An amino acid derivative nanoarray material, its preparation method, and its application.

By co-assembling L-glutamic acid-modified Fe3O4 nanoparticles with phenylalanine derivative nanorods to form a directionally arranged nanoarray, the problem of insufficient piezoelectric performance of existing amino acid derivative piezoelectric materials is solved, achieving a high-efficiency improvement in piezoelectric performance, which is suitable for environmentally friendly materials with good biocompatibility.

CN117529210BActive Publication Date: 2026-11-10SHANGHAI JIAOTONG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311413570.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-27
Publication Date
2026-11-10
Estimated Expiration
2043-10-27

AI Technical Summary

Technical Problem

Existing amino acid derivative piezoelectric materials have insufficient piezoelectric properties, making them unsuitable for practical applications, especially due to their low output signal, which cannot reach the level of inorganic PENGs.

Method used

By co-assembling L-glutamic acid-modified Fe3O4 nanoparticles with phenylalanine derivative nanorods, a directionally arranged nanoarray is formed, and its alignment direction is controlled by a magnetic field to enhance piezoelectric properties.

Benefits of technology

The piezoelectric coefficient of the nanoarray is increased by an order of magnitude, the output voltage reaches ~2.5V, and the current reaches ~150nA, meeting the performance requirements of existing piezoelectric materials and making it suitable for environmentally friendly materials with good biocompatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117529210B_ABST
    Figure CN117529210B_ABST
Patent Text Reader

Abstract

This invention relates to an amino acid derivative nanoarray material, its preparation method, and its applications. The invention involves the preparation of a piezoelectric nanoarray of directionally aligned amino acid derivatives. By co-assembling magnetic nanoparticles with amino acid derivative nanorods, nanorods that can be directionally aligned under a magnetic field are obtained. This orientation effectively improves the piezoelectric properties of the nanomaterial, elevating them to the same order of magnitude as inorganic materials. Piezoelectric devices prepared using this material can achieve significantly improved output current and voltage values, promoting the practical application of this environmentally friendly piezoelectric material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials technology, and particularly relates to an amino acid derivative nanoarray material, its preparation method and application, especially an amino acid derivative piezoelectric nanoarray and the preparation of its corresponding piezoelectric devices. Background Technology

[0002] With the further development of multifunctional devices such as portable electronic devices, implantable electronic devices, and wireless sensors, environmental energy harvesting technology has developed rapidly in recent years. The piezoelectric nanogenerator (PENG) based on hexagonal zinc oxide (ZnO) nanowires, invented by Professor Wang Zhonglin's team, can effectively convert minute and irregular mechanical energy such as vibration, wind, walking, water waves, heartbeats, and breathing movements into electrical energy. Subsequently, several inorganic ceramic oxides, polyvinylidene fluoride (PVDF), PVDF copolymers, and composites of these materials have also been found to be effective electromechanical energy harvesters. However, the application of these materials requires high-temperature or melt-quenching techniques, resulting in long processing times. Sometimes, they also require stretching and high-pressure polarization, making the operation complex and energy-intensive. In particular, some of these materials contain toxic heavy metals that pose a serious environmental hazard, making them unsuitable for wearable electronic devices or biological applications.

[0003] To address the aforementioned shortcomings, Professor Gazit and his colleagues used small-molecule amino acid derivatives as piezoelectric materials to prepare organic small-molecule nanogenerators with good biocompatibility and high strength. These materials are not only very environmentally friendly but also improve the flexibility of required devices, making them ideal for constructing miniaturized and self-powered next-generation electronic microdevices. However, the piezoelectric coefficient of organic small molecules has remained relatively low, currently failing to exceed 40 pm V. -1 Furthermore, the output signal of this type of piezoelectric material is also low, with current mostly in the tens of nA and voltage difficult to reach above 2V, which hinders the further application of this type of material.

[0004] It is evident that existing amino acid derivative piezoelectric materials generally suffer from insufficient piezoelectric performance, hindering their practical applications. If the output of organic molecular piezoelectric devices could be increased to the level of inorganic PENGs, they would become one of the most competitive micro-power sources. Summary of the Invention

[0005] The purpose of this invention is to address the problems existing in the prior art by providing an amino acid derivative nanoarray material, its preparation method, and its application. This invention aims to solve the problem that existing amino acid derivative piezoelectric materials generally suffer from low piezoelectric signal and insufficient performance, thus hindering their effective application.

[0006] This invention uses phenylalanine derivative rods as the main raw material, and co-assembles them with L-glutamic acid-modified Fe3O4 nanoparticles. The L-glutamic acid doping effect on the phenylalanine derivative nanoparticles allows the two to bond together. After forming a composite structure, a magnet is used to orient the co-assembled structure, forming a regularly arranged nanoarray. The piezoelectric coefficient of the oriented nanoarray increases by an order of magnitude, meeting the piezoelectric performance requirements of piezoelectric materials in applications and effectively promoting the practical application of nanoarrays.

[0007] The objective of this invention can be achieved through the following methods:

[0008] This invention provides an amino acid derivative nanoarray material, which is an array of oriented nanorods formed by nanorods under a magnetic field. The nanorods are obtained by co-assembling magnetic nanoparticles and amino acid derivative nanorods.

[0009] In one embodiment of the present invention, the magnetic nanoparticles are magnetic Fe3O4 nanoparticles (L-Fe3O4) obtained by modifying Fe3O4 nanoparticles with L-glutamic acid (L-Glu). The specific preparation steps are as follows: Fe3O4 particles are uniformly dispersed in a solvent, an L-glutamic acid solution is added, the mixture is mixed, ultrasonically dispersed, reacted at a constant temperature, and washed to obtain the magnetic Fe3O4 nanoparticles (L-Fe3O4). The molar ratio of L-glutamic acid (L-Glu) to iron in the Fe3O4 particles is 1–2:1. The solvent is a mixture of ethanol and water, with a volume ratio of 5:5–9:1. The ultrasonic dispersion time is 10–30 min; the constant temperature reaction temperature is 40–60 °C, and the time is 0.5–2 h. The reaction is carried out under stirring conditions and nitrogen protection. Washing is performed using deionized water and ethanol alternately until the pH of the supernatant is 7, thus obtaining L-Fe3O4.

[0010] Magnetic nanoparticles are present at the top of one end of the amino acid derivative nanorods, while the other end is essentially absent (see...). Figure 1 c, d), this is related to the amount of L-Fe3O4 added and the assembly structure. The crystal structure of the assembly has been confirmed ( Figure 1 (The part shown in the dashed box) The AD units that can form ionic bonds with L-Fe3O4 are located on the end face of the assembly. Due to the small amount added and the mutual attraction of magnetic particles, they are mostly concentrated at one end.

[0011] The Fe3O4 nanoparticles were prepared by the following method:

[0012] T1. Prepare solution A: Mix FeCl3 solution and FeSO4 solution, then add the mixed solvent;

[0013] T2. Prepare solution B: Take NaOH solution and add it to the mixed solvent;

[0014] T3. Add solution B dropwise to solution A, let it stand after reaction to break the emulsion, then use a magnet to hold the product, wash the product, and obtain Fe3O4 nanoparticles.

[0015] In step T1, the concentration of FeCl3 solution is 0.04–0.1 mol / L, the concentration of FeSO4 solution is 0.04–0.1 mol / L, and the volume ratio of FeCl3 solution, FeSO4 solution, and mixed solvent is 30:50–60:15–50.

[0016] In step T2, the NaOH concentration is 1.6 mol / L. The volume ratio of NaOH solution to mixed solvent is 50:15–75.

[0017] In steps T1 and T2, the mixed solvent includes cyclohexane, n-butanol, and a surfactant added sequentially in a ratio of 4–6 mL: 8–15 mL: 2–5 g. The surfactant is PEG-400. Cyclohexane and n-butanol are used as the mixed solvent to form a water-oil two-phase system. The surfactant is added to increase the compatibility of the two phases, forming a microemulsion, which facilitates the formation of nano-Fe3O4 particles within the microemulsion system. The microemulsion formulation allows for control over the size of the Fe3O4 nanoparticles.

[0018] In step T3, the reaction temperature is 40–60°C, and the time is 0.5–2 hours. The settling time is 30 minutes. Demulsification is performed using acetone; the product is washed with alternating ethanol and water until the pH of the supernatant is 7.

[0019] In one embodiment of the present invention, the amino acid derivative nanorods are formed by the self-assembly of amino acid derivatives. The self-assembly solvent used is a mixture of acetonitrile and water or DMSO solvent.

[0020] In one embodiment of the present invention, the amino acid derivative is a D-phenylalanine derivative (D-PheAD), which has a C2 symmetrical molecular structure. Based on the chirality of the D-phenylalanine contained in the synthesized molecule, the molecule is recorded as D-PheAD. The structural formula of the small organic molecule of the phenylalanine derivative is shown in Formula I:

[0021]

[0022] In one embodiment of the present invention, the weight ratio of magnetic Fe3O4 nanoparticles (L-Fe3O4) to D-phenylalanine derivative (D-PheAD) molecules is 1.56–0.39:1. Preferably, the weight ratio of L-Fe3O4 nanoparticles to D-PheAD is 1.56–0.78:1. In the fabrication of the nanoarray, L-Fe3O4 and D-PheAD nanorods are co-assembled in a certain ratio. Effective magnetic field orientation requires a certain proportion of L-Fe3O4 and D-PheAD nanorods to form a co-assembly. Therefore, in this embodiment of the present invention, a co-assembly needs to be formed at the above ratio before the formation of the nanoarray.

[0023] The present invention also provides a method for preparing the amino acid derivative nanoarray material, wherein the preparation method is either method one or method two below;

[0024] In Method 1, the self-assembly solvent is acetonitrile, and the process includes the following steps:

[0025] S1. Add D-phenylalanine derivative (D-PheAD) to acetonitrile, sonicate and let stand until the assembly forms to obtain the assembly dispersion.

[0026] S2. Mix the assembly dispersion with the dispersion of magnetic Fe3O4 nanoparticles (L-Fe3O4), and sonicate to obtain a co-assembly.

[0027] S3. The co-assembled material is drop-coated onto the surface of a conductive thin film, oriented using a magnet, and the solvent is evaporated to obtain an oriented amino acid derivative nanoarray material.

[0028] Method 2 uses DMSO as the self-assembly solvent and includes the following steps:

[0029] A1. Dissolve D-phenylalanine derivative (D-PheAD) in DMSO and sonicate until completely dissolved to obtain a D-phenylalanine derivative (D-PheAD) solution.

[0030] A2. The dispersion of magnetic Fe3O4 nanoparticles (L-Fe3O4) was added dropwise to a solution of D-phenylalanine derivative (D-PheAD), followed by ultrasonic treatment to obtain a co-assembled product.

[0031] A3. The co-assembled material is drop-coated onto the surface of a conductive film, oriented using a magnet, and the solvent is evaporated to obtain an oriented amino acid derivative nanoarray material.

[0032] Both methods 1 and 2 can prepare nanoarrays. Method 1 produces shorter, rod-shaped nanofibers, while method 2 produces nanofibers with a certain degree of helical structure. Furthermore, because methods 1 and 2 use different solvent systems, their wettability varies depending on the substrate, allowing for the selection of appropriate methods based on the substrate. DMSO is a good solvent for D-PheAD molecules, and the assemblies only form after the addition of an aqueous solution containing magnetic particles.

[0033] In one embodiment of the present invention, in step S1 of method one, D-phenylalanine derivative (D-PheAD) molecules are dissolved in acetonitrile, and the content of D-phenylalanine derivative (D-PheAD) molecules in the resulting solution is 1-10 mg / mL. Water may be added after standing, the amount added not exceeding the volume of acetonitrile, i.e., the volume ratio of acetonitrile to water in the solvent is 10⁻⁰ to 5⁻⁵; the ultrasonic vibration time is 30 min.

[0034] In one embodiment of the present invention, in step S2 of method one, the dispersion of magnetic Fe3O4 nanoparticles (L-Fe3O4) is prepared by dispersing magnetic Fe3O4 nanoparticles (L-Fe3O4) in water. The content of magnetic Fe3O4 nanoparticles (L-Fe3O4) in the dispersion is 3–10 mg / mL, and the volume ratio of the assembly dispersion to the magnetic Fe3O4 nanoparticle (L-Fe3O4) dispersion is 5–20:1.

[0035] In one embodiment of the present invention, in step S2 of method one, the ultrasonic oscillation time is 20 minutes.

[0036] In one embodiment of the present invention, step S3 of method one involves orienting the conductive film by placing a magnet above or below it. The conductive film is a metal film, including copper tape and aluminum foil.

[0037] In one embodiment of the present invention, in step A1 of method two, the ratio of D-phenylalanine derivative (D-PheAD) to DMSO is 1 mg: 50-100 μL.

[0038] In one embodiment of the present invention, in step A2 of method two, the content of magnetic Fe3O4 nanoparticles (L-Fe3O4) in the magnetic Fe3O4 nanoparticle dispersion is 3-10 mg / mL, and the volume ratio of the assembly dispersion to the magnetic Fe3O4 nanoparticle (L-Fe3O4) dispersion is 0.5-2:10.

[0039] After the dispersion of magnetic Fe3O4 nanoparticles (L-Fe3O4) is added dropwise, the solubility of D-phenylalanine derivative (D-PheAD) decreases, causing D-PheAD molecules to precipitate and form self-assemblies. Ultrasonic treatment then induces the co-assembly of these assemblies with the L-Fe3O4 magnetic microparticles.

[0040] In one embodiment of the present invention, step A3 of method two involves orienting the material by placing a magnet above or below a highly hydrophilic substrate. The conductive film is a highly hydrophilic substrate, including copper tape.

[0041] Vertical orientation of magnetic particles is quite difficult; most existing technologies focus on horizontal orientation. The challenge in co-assembling the magnetic nanoparticles and amino acid derivative assemblies in this invention lies in matching the size of the Fe3O4 with that of the amino acid derivative assembly, while simultaneously requiring the selection of suitable organic molecules to modify the Fe3O4.

[0042] The present invention also provides an application of the amino acid derivative nanoarray material in the field of piezoelectricity.

[0043] The present invention also provides a piezoelectric device, which is prepared from the amino acid derivative nanoarray material.

[0044] As one embodiment of the present invention, the piezoelectric device fabrication method includes the following steps:

[0045] PDMS is coated on top of an amino acid derivative nanoarray material, and a conductive film is covered on top of the PDMS before it is set. After drying, wires are led out from the uppermost and lowermost conductive films of the nanoarray material and encapsulated to obtain the piezoelectric device.

[0046] Drying involves placing the device in an oven and pressing it down with an iron block to ensure tight contact between the PDMS layer and the layers above and below. After the PDMS has dried and set, the device is removed, and leads are made onto the copper tape on the top and bottom layers. Finally, the device is encapsulated with Kapton tape.

[0047] When the sensor element described above is subjected to pressure, a voltage can be obtained between the upper and lower electrodes in the open-circuit state, and a current can be obtained between the upper and lower electrodes in the short-circuit state. This directional nanoarray material achieves piezoelectric properties of the same order of magnitude as inorganic nanopiezoelectric materials, and the fabricated piezoelectric device obtains enhanced output voltage and current signals, which is beneficial to the practical application of this biocompatible and environmentally friendly material.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] (1) The embodiments of the present invention control the arrangement direction of the nanoarray by magnetic field, which effectively improves the piezoelectric coefficient of the material, making it reach the same order of magnitude as inorganic nanopiezoelectric materials, meeting the performance requirements of existing piezoelectric materials, and can be used as a biocompatible and environmentally friendly piezoelectric material.

[0050] (2) After magnetic field orientation, the piezoelectric coefficient of the D-PheAD nanoarray reaches an order of magnitude comparable to that of some inorganic materials. The piezoelectric device prepared from D-PheAD nanoarrays has a voltage of ~2.5V and an output current of ~150nA, which effectively improves the output electrical signal strength of the device and can meet the practical application requirements of amino acid derivative piezoelectric materials. Attached Figure Description

[0051] Other features, objects, and advantages of the present invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings:

[0052] Figure 1 This is a schematic diagram of the preparation process and structure of the amino acid derivative nanoarray provided in Example 1 of the present invention.

[0053] Where a is a schematic diagram of the preparation of the entire amino acid derivative nanoarray, b is a transmission electron microscope (TEM) image of L-Fe3O4, and c and d are TEM images of the L-Fe3O4 and D-PheAD co-assembly without magnetic field orientation.

[0054] Figure 2 This is a schematic diagram of the piezoelectric device structure of the amino acid derivative nanoarray material provided in Embodiment 2 of the present invention.

[0055] Figure 3 This is a scanning electron microscope (SEM) image of the upwardly oriented amino acid derivative nanoarray provided in Example 1 of the present invention.

[0056] Figure 4 This is a scanning electron microscope (SEM) image of the downward-oriented amino acid derivative nanoarray provided in Example 1 of the present invention.

[0057] Figure 5 This is a scanning electron microscope (SEM) image of the non-magnetic field oriented amino acid derivative nanoarray provided in Example 1 of the present invention.

[0058] Figure 6 The above are amplitude diagrams of the amino acid derivative nanoarray material provided in Example 1 of this invention, where a is the amplitude diagram of D-PheAD-L-Fe3O4 nanorods with no magnetic field orientation, magnetic field upward orientation, and magnetic field downward orientation, and b is the amplitude diagram of D-PheAD-L-Fe3O4 nanorods with no magnetic field orientation and D-PheAD assemblies with different voltages.

[0059] Figure 7 This diagram shows the electrical signal output data of piezoelectric devices prepared from amino acid derivative nanoarray materials under different magnetic fields according to embodiments of the present invention. In the diagram, a represents the output current of the device prepared from the D-PheAD-L-Fe3O4 nanorods oriented upwards; b represents the output voltage of the device prepared from the D-PheAD-L-Fe3O4 nanorods oriented upwards; c represents the output current of the device prepared from the D-PheAD-L-Fe3O4 nanorods oriented downwards; d represents the output voltage of the device prepared from the D-PheAD-L-Fe3O4 nanorods oriented downwards; e represents the output current of the device prepared from the D-PheAD-L-Fe3O4 nanorods oriented without a magnetic field; and f represents the output voltage of the device prepared from the D-PheAD-L-Fe3O4 nanorods oriented without a magnetic field.

[0060] Figure 8 This is a comparison of the orientation capabilities of Fe3O4 and L-Fe3O4 magnetic particles to D-2AD molecules under a magnetic field, as provided in Comparative Example 1 of this invention. In the image, a is a photograph of Fe3O4 and D-2AD co-assembled under magnetic field orientation, and b is a photograph of L-Glu-modified L-Fe3O4 co-assembled with D-2AD under magnetic field orientation. Detailed Implementation

[0061] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0062] The terminology used in the embodiments of this invention is for the purpose of describing particular embodiments only and is not intended to limit the invention. The singular forms “a” and “the” as used in the embodiments of this invention and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the term “and / or” as used herein refers to and includes any or all possible combinations of one or more of the associated listed items.

[0063] The following are embodiments of certain implementations of the present invention, which are not intended to limit the scope of the present invention.

[0064] The preparation of D-PheAD molecules used in the implementation and comparative examples of this invention refers to Example 1 of patent (CN115458676A).

[0065] Example 1

[0066] This invention provides a nanoarray material based on the amino acid derivative, such as... Figure 1As shown, magnetic Fe3O4 nanoparticles are combined with amino acid derivative molecules to form nanorods, which then form a nanoarray under the action of a magnetic field.

[0067] 1. The preparation method of D-PheAD nanorods, the specific steps are as follows:

[0068] Weigh 2 mg of D-PheAD molecules, add 1.4 mL of acetonitrile solvent, sonicate to dissolve completely, add 0.6 mL of water, continue sonicating for 30 min, and then let stand.

[0069] 2. The preparation method of magnetic Fe3O4 nanoparticles (L-Fe3O4) includes the following steps:

[0070] Prepare solution A: Prepare 30 mL of FeCl3 solution with a concentration of 0.04 mol / L; prepare 50 mL of FeSO4 solution with a concentration of 0.04 mol / L. Add 5 mL of cyclohexane, 10 mL of n-butanol, and 4 g of PEG-400 sequentially.

[0071] Prepare solution B: Prepare a 1.6 mol / L NaOH solution, take 50 mL. Add 5 mL of cyclohexane, 10 mL of n-butanol, and 4 g of PEG-400 sequentially.

[0072] Solution B was added dropwise to solution A, and the reaction was stopped after reacting at 50 degrees Celsius for 1 hour. The mixture was then allowed to stand for 30 minutes. The resulting mixture was demulsified with acetone, and the product was then attracted with a magnet. The mixture was washed alternately with ethanol and water until the pH of the supernatant was 7. The resulting magnetic Fe3O4 nanoparticles had a particle size of less than 20 nm.

[0073] A certain mass of L-glutamic acid was dissolved in deionized water, maintaining a mass ratio of L-glutamic acid to iron of 1:1. The Fe3O4 colloid, meeting this ratio, was uniformly dispersed in a mixture of ethanol and water (100 mL, volume ratio 6:4). The L-glutamic acid solution was added to this solution, and the mixture was ultrasonically dispersed for 10 min. The mixture was then transferred to a temperature-controlled, magnetically stirred water bath with a stirring rod and nitrogen protection. The reaction temperature was set to 45°C, and the mixture was stirred for 1 hour. After the reaction was complete, the mixture was washed alternately with deionized water and ethanol until the pH of the supernatant reached 7, yielding L-Fe3O4.

[0074] 3. Construct a directional array of D-PheAD nanorods, as detailed below:

[0075] (1) Weigh 7.8 mg of L-Fe3O4 powder, add 1 mL of water, and sonicate for 10 min. Then, use a pipette to add 200 μL of the dispersion to the prepared D-PheAD assembly. Sonicate the above mixture for 20 min.

[0076] (2) Cut a piece of copper tape, about 7 cm long, and place it on an inverted transparent plastic dish. Suspend a circular magnet with a diameter of 5 cm in the dish or above the tape. Apply 200 μL of the mixed liquid prepared in step (1) onto the copper tape. Place the entire apparatus in a constant temperature drying oven at 60 degrees Celsius. Wait for the solvent to evaporate completely to obtain the oriented nanoarray (e.g., ...). Figure 3 , Figure 4 The effective piezoelectric coefficients of the D-PheAD-L-Fe3O4 nanoarrays oriented upwards and downwards by magnetic force are 121.88 pm V. -1 and 109.74pm V -1 The piezoelectric coefficient of the unoriented sample is 12.58 pm V. -1 The piezoelectric coefficient of the standalone D-PheAD assembly (without co-assembly with L-Fe3O4) is 10.44 pm V. -1 (like Figure 5 , Figure 6 ).

[0077] Example 2

[0078] This embodiment provides a sensor element, such as... Figure 2 As shown, the specific construction method is as follows:

[0079] (1) Prepare a PDMS base agent and curing agent with a ratio of 10:1. After mixing, apply the mixture evenly to the magnetically oriented D-PheAD assembly layer prepared in Example 1, and cover the PDMS layer with a layer of copper tape. Place the three-layer device in a 70°C oven for more than 2 hours.

[0080] (2) After the PDMS from step (1) has completely dried, remove the three-layer device and lead out a wire from each of the upper and lower copper tapes. Finally, seal it with Kapton tape.

[0081] (3) The sensing element prepared in step (2) was tested for open-circuit voltage and short-circuit current under a cyclic pressure of 30N and 0.25Hz using a Keithley 6514 digital source meter. The test structure is as follows:

[0082] The open-circuit voltage (VOC) and short-circuit current (ISC) signals of L-Fe3O4-D-PheAD upward-oriented devices are as follows: Figure 7 As shown.

[0083] Example 3

[0084] The present invention provides an amino acid derivative nanoarray material, which uses magnetic Fe3O4 nanoparticles combined with amino acid derivative molecules to form nanorods, forming a nanoarray under the action of a magnetic field.

[0085] 1. The preparation method of D-PheAD nanofibers, the specific steps are as follows:

[0086] Weigh 1 mg of D-PheAD molecules, add 100 μL of DMSO solvent, and sonicate to dissolve completely.

[0087] 2. The preparation method of magnetic Fe3O4 nanoparticles (L-Fe3O4) is the same as in Example 1.

[0088] 3. Construct a directional array of D-PheAD nanorods, as detailed below:

[0089] (1) Weigh 7.8 mg of L-Fe3O4 powder, add 1 mL of water, and sonicate for 10 min. Then, use a pipette to add the dispersion dropwise to the prepared D-PheAD DMSO solution. Sonicate the above mixture for 20 min and let it stand for 30 min.

[0090] (2) Cut a piece of copper tape, about 7 cm long, and place it on an inverted transparent plastic dish. Suspend a circular magnet with a diameter of 5 cm in the dish or above the tape. Take 200 μL of the mixed liquid prepared in step (1) and drop it onto the copper tape. Place the entire apparatus in a constant temperature drying oven at 75 degrees Celsius. Wait for the solvent to evaporate completely to obtain the oriented nanoarray.

[0091] Example 4

[0092] This embodiment provides a sensor element, and the specific construction method is as follows:

[0093] (1) Prepare a PDMS base agent and curing agent with a ratio of 10:1. After mixing, apply the mixture evenly to the oriented D-PheAD assembly layer prepared in Example 3, and cover the PDMS layer with a layer of copper tape. Place the three-layer device in a 70°C oven for more than 2 hours.

[0094] (2) After the PDMS from step (1) has completely dried, remove the three-layer device and lead out a wire from each of the upper and lower copper tapes. Finally, seal it with Kapton tape.

[0095] Comparative Example 1

[0096] This comparative example provides an amino acid derivative nanomaterial, which uses magnetic Fe3O4 nanoparticles combined with amino acid derivative molecules to form nanorods. Orientation is achieved using a magnetic field. The preparation method is basically the same as in Example 1, except that amino acid-modified Fe3O4 is not used. Experimental results show that when a magnet is placed on the right side of the sample vial, after 3 minutes, the Fe3O4 without amino acid modification cannot drive the oriented movement of the assembly (e.g., ...). Figure 8 As shown in a), D-PheAD is still largely dispersed in the solution.

[0097] Comparative Example 2

[0098] This comparative example provides an amino acid derivative nanomaterial. Oleic acid-modified magnetic Fe3O4 nanoparticles (denoted as O-Fe3O4) are used to form a co-assembly with amino acid derivative molecules, which is then subjected to a magnetic field. The preparation method is basically the same as in Example 1, except that oleic acid is used to modify Fe3O4. Experimental results show that the O-Fe3O4-D-PheAD cannot form a regular nanoarray under the magnetic field. This may be because oleic acid retains a large number of unreacted carboxyl groups, which can connect to multiple D-PheAD assemblies, making it difficult to determine their orientation.

[0099] The specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the specific embodiments described above, and those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. An amino acid derivative nanoarray material, characterized in that, The amino acid derivative nanoarray material is a directional array of nanorods formed under a magnetic field. The nanorods are obtained by co-assembling magnetic nanoparticles and amino acid derivative nanorods. The magnetic nanoparticles are magnetic Fe3O4 nanoparticles obtained by modifying Fe3O4 nanoparticles with L-glutamic acid. The specific preparation steps are as follows: Fe3O4 particles are uniformly dispersed in a solvent, L-glutamic acid solution is added, the mixture is ultrasonically dispersed, reacted at a constant temperature, and washed to obtain the magnetic Fe3O4 nanoparticles. The amino acid derivative nanorods are formed through the self-assembly of amino acid derivatives; the amino acid derivative is a D-phenylalanine derivative, with the following structural formula: 。 2. The amino acid derivative nanoarray material according to claim 1, characterized in that, The Fe3O4 nanoparticles were prepared by the following method: T1. Prepare solution A: Mix FeCl3 solution and FeSO4 solution, then add cyclohexane, n-butanol and surfactant in sequence; T2. Prepare solution B: Take NaOH solution and add cyclohexane, n-butanol, and surfactant in sequence; T3. Add solution B dropwise to solution A, let it stand after reaction to break the emulsion, then use a magnet to hold the product, wash the product, and obtain Fe3O4 nanoparticles.

3. The amino acid derivative nanoarray material according to claim 1, characterized in that, The solvent used for self-assembly is acetonitrile or DMSO.

4. A method for preparing the amino acid derivative nanoarray material as described in claim 1, characterized in that, The preparation method is either Method 1 or Method 2 as follows; In Method 1, the self-assembly solvent is acetonitrile, and the process includes the following steps: S1. Add the D-phenylalanine derivative to acetonitrile, sonicate and let stand until the assembly forms to obtain the assembly dispersion. S2. Mix the assembly dispersion with the magnetic Fe3O4 nanoparticle dispersion, and sonicate to obtain a co-assembly. S3. The co-assembled material is drop-coated onto the surface of a conductive thin film, oriented using a magnet, and the solvent is evaporated to obtain an oriented amino acid derivative nanoarray material. Method 2 uses DMSO as the self-assembly solvent and includes the following steps: A1. Dissolve the D-phenylalanine derivative in DMSO and sonicate it until completely dissolved to obtain a D-phenylalanine derivative solution. A2. The dispersion of magnetic Fe3O4 nanoparticles was added dropwise to the D-phenylalanine derivative solution, followed by ultrasonic treatment to obtain the co-assembly. A3. The co-assembled material is drop-coated onto the surface of a conductive film, oriented using a magnet, and the solvent is evaporated to obtain an oriented amino acid derivative nanoarray material.

5. The preparation method according to claim 4, characterized in that, In step S3 of Method 1 and step A3 of Method 2, the orientation process specifically involves placing a magnet above or below the conductive film for orientation.

6. An application of the amino acid derivative nanoarray material as described in claim 1 in the field of piezoelectricity.

7. A piezoelectric device, characterized in that, The piezoelectric device is prepared from the amino acid derivative nanoarray material as described in claim 1.

8. The piezoelectric device according to claim 7, characterized in that, The piezoelectric device is prepared by coating PDMS on an amino acid derivative nanoarray material including a conductive film, and covering the PDMS with a conductive film while the PDMS is still unformed. After drying, wires are led out from the uppermost and lowermost conductive films and then packaged to obtain the piezoelectric device.

Citation Information

Patent Citations

  • Phenylalanine derivative-based micromolecular organic piezoelectric material and preparation method thereof

    CN115458676A

  • Fe3O4 / octreotide modified nano-liposome and preparing method thereof

    CN107029246A

  • Self-assembled amino acid derivative functionalized magnetic-carbon nanotube composite material as well as preparation method and application thereof

    CN111229189A