A fiber-modified reinforced soil and its preparation method

By combining the directional distribution of magnetized core polypropylene fibers in a magnetic field with EICP technology, the problems of uneven fiber distribution and low interfacial strength in fiber-reinforced soil are solved, thereby strengthening the fiber-soil interface and improving pull-out resistance, and reducing the risk of brittle failure.

CN117535057BActive Publication Date: 2026-11-10YANSHAN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311480275.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-08
Publication Date
2026-11-10
Estimated Expiration
2043-11-08

AI Technical Summary

Technical Problem

In existing fiber-reinforced soil technology, the fibers cannot be oriented in the soil, the bonding strength between polypropylene fibers and soil is low, the pull-out resistance is poor, and the lack of nucleation sites in EICP technology leads to uneven calcium carbonate precipitation, resulting in a high risk of brittle failure of the cemented hardened layer.

Method used

Magnetized core polypropylene fibers are oriented in a magnetic field, and calcium carbonate precipitate is formed on the fiber surface using EICP technology. The reaction window is controlled by combining urease inhibitors, and the reaction solution is coated on the fiber surface to induce calcium carbonate precipitation at the fiber-soil interface. Silane coupling agents are used to improve fiber dispersibility.

Benefits of technology

This method enables the directional distribution of fibers in the soil, enhances the interfacial strength between fibers and soil, improves pull-out resistance, improves the uniformity and depth of calcium carbonate precipitation, and reduces the risk of brittle failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117535057B_ABST
    Figure CN117535057B_ABST
Patent Text Reader

Abstract

This invention provides a fiber-modified reinforced soil and its preparation method. Using magnetized core polypropylene fibers, urease, urease inhibitors, calcium chloride solution, urea solution, and silane coupling agent as raw materials, this invention combines EICP technology with magnetized core polypropylene fibers. The cementing effect of calcium carbonate improves the interfacial bond strength between the polypropylene fibers and the soil. Simultaneously, calcium carbonate modifies the polypropylene fibers, increasing their surface roughness and improving their pull-out resistance, thus better enhancing the fiber-reinforced soil effect. The magnetized core polypropylene fibers allow for directional distribution within the soil under the influence of a magnetic field; the addition of urease inhibitors extends the controllable window period of calcium carbonate precipitation; and the external coating solution improves the uneven distribution of calcium carbonate at different soil depths produced by EICP technology, while also saving raw material consumption. This method results in high strength and significant economic, social, and practical benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fiber-reinforced soil technology, specifically to a fiber-modified reinforced soil and its preparation method. Background Technology

[0002] Fiber-reinforced soil involves adding a certain amount of uniform fibers to the soil, utilizing the high strength, toughness, and durability of the selected fibers to improve the soil's mechanical properties. With the rapid development of geotechnical engineering, traditional fiber-reinforced soil has begun to reveal its shortcomings. For example, the fibers may not be directionally distributed within the soil, potentially leading to fiber agglomeration and thus reducing its reinforcing effect. Some high-quality fibers, such as polypropylene fibers, have relatively smooth surfaces, resulting in lower interfacial bonding strength with the soil and poor pull-out resistance, making them unsuitable for high-strength engineering requirements. Therefore, researching and developing higher-strength fiber-reinforced soil using high-quality fibers such as polypropylene has become a hot topic in this field.

[0003] In recent years, bio-stabilization technology, as an emerging environmentally friendly soil reinforcement technology, has attracted much attention from scholars. It mainly includes Enzyme-Induced Carbonate Precipitation (EICP) and Microbial-Induced Carbonate Precipitation (MICP). Both technologies utilize urease to induce calcium carbonate deposition, filling the spaces between soil particles to cement them and improve the physical and mechanical properties of the soil. Compared to MICP, EICP does not require microbial cultivation, making it simpler, less costly, and less environmentally risky. However, EICP lacks microorganisms as nucleation sites for calcium carbonate precipitation. Currently, the challenges in applying EICP are: 1. Providing nucleation sites for calcium carbonate precipitation during EICP soil stabilization; 2. Finding suitable methods to improve the depth and uniformity of soil modification using EICP; and 3. Preventing brittle failure of the cemented hardened layer after EICP treatment.

[0004] Chinese patent CN109970381B discloses a method for microbial mineralization modification of polypropylene fibers and its application. This method improves fiber properties and enhances the performance of fiber-reinforced concrete composites by generating calcium carbonate precipitate on the surface of polypropylene fibers to form a calcite film. However, there is no controllable window period during the calcium carbonate modification process. The formed calcium carbonate precipitate adheres entirely to the fiber surface, forming a calcium carbonate crust. This crust has weak adhesion to the polypropylene fiber surface and is prone to peeling off. Furthermore, the calcium carbonate precipitation process is completed before the fibers are mixed in. If applied to soil, the dried calcium carbonate layer on the modified polypropylene fiber surface does not provide ideal bonding between the fiber and the soil. Summary of the Invention

[0005] The purpose of this invention is to meet the development trend of fiber-reinforced soil and, in view of the shortcomings of existing technologies, provide a fiber-modified reinforced soil and its preparation method. The specific technical solution is as follows:

[0006] A method for preparing fiber-modified reinforced soil includes the following steps:

[0007] (1) The core material and the sheath material are respectively placed into a two-component concentric sheath-core composite spinning machine for melt spinning to obtain magnetized sheath-core geofiber. Then, it is placed in a silane coupling agent for dispersion modification, and then washed and dried to produce modified magnetized sheath-core geofiber.

[0008] (2) Mix the urease-containing reagent and the urease inhibitor to obtain mixture A; mix the urea solution and the calcium chloride solution to obtain cemented solution B;

[0009] (3) Coat the surface of the modified magnetized core geofiber with a mixture A, and then coat it with a binder B to produce a modified magnetized core geofiber with a roughened surface.

[0010] (4) The modified magnetized core geotextile fiber with roughened surface and clay are placed in a directional magnetic field and mixed while vibrating. Then, the mixture is left to stand in the magnetic field until the calcium carbonate in the soil is precipitated, thus obtaining the fiber-modified reinforced soil.

[0011] Preferably, the fiber-modified reinforced soil comprises the following raw materials in parts by weight: 1000 parts clay, 2-4 parts modified magnetized core geofiber, 8-12 parts mixture A, and 8-12 parts cementing solution B;

[0012] Preferably, all steps are performed at room temperature.

[0013] Preferably, in step (1), the magnetized core geotextile fiber is a magnetized core polypropylene fiber. Using magnetized core polypropylene fiber in fiber-reinforced soil and mixing the reinforcement and soil under magnetic field conditions can effectively induce the fiber to be oriented in the soil and prevent the fiber from agglomerating in the soil to a certain extent, which would lead to uneven stress on the soil.

[0014] Preferably, the core layer material is magnetic powder and polypropylene chips; the skin layer material is pure polypropylene chips.

[0015] Preferably, the magnetic powder content in the core layer material is 50% to 80%.

[0016] Preferably, in step (1), the silane coupling agent is selected from any one of the dilute solutions of SCA-1603, SCA-1613 or SCA-1623 prepared with anhydrous ethanol;

[0017] Preferably, the concentration of the silane coupling agent is 0.6–1.0 wt%.

[0018] Preferably, the dispersion modification time is 20–30 min.

[0019] Preferably, in step (2), the urease-containing reagent is selected from a urease solution of 10-20 g / L or a soybean flour solution of 50-100 g / L, and the concentration of the urease inhibitor is 0.1-0.2 g / L;

[0020] Preferably, the volume ratio of urease reagent to urease inhibitor is 1:1;

[0021] Preferably, the mixing time is 20 to 30 minutes.

[0022] Preferably, the urease inhibitor is selected from 0.1–0.2 g / L of n-butylthiophosphate triamine. During the soil-reinforcement interface treatment process, the addition of the urease inhibitor, used in conjunction with urease, effectively inhibits the immediate reaction between urease and urea, prolonging the EICP process and providing a controllable window period for calcium carbonate precipitation. The addition of the urease inhibitor divides the calcium carbonate produced by the EICP reaction into two parts: the first part precipitates on the fiber surface during the inhibition phase to modify the fiber, and the second part precipitates at the soil-reinforcement interface during the later inhibition phase to strengthen the interface. This fully utilizes the calcium carbonate precipitate produced by the reaction to modify the fiber surface and fill the voids at the soil-reinforcement interface, improving the fiber's pull-out resistance in the soil and enhancing the soil-reinforcement interface strength through the cementing effect of calcium carbonate.

[0023] Preferably, in step (2), the concentrations of the urea solution and the calcium chloride solution are the same;

[0024] Preferably, the concentrations of both the urea solution and the calcium chloride solution are 0.5–1.5 mol / L;

[0025] Preferably, the volume ratio of urea solution to calcium chloride solution is 1:1.

[0026] Preferably, in step (3), the outer coating is achieved by soaking or spraying. If the reaction solution is directly sprayed or grouted into the soil, calcium carbonate precipitation can easily block the pores between soil particles, leading to uneven distribution of calcium carbonate and a gradual weakening of the cementing effect as the soil depth increases. By using the outer coating solution, calcium carbonate can be induced to concentrate and precipitate at the interface between the fiber and the soil. Furthermore, the mixing of the fiber and the soil increases the depth and uniformity of calcium carbonate precipitation, effectively improving the utilization rate of the reaction solution.

[0027] Preferably, in step (4), the short time is 0.5 to 2 hours;

[0028] Preferably, the settling time is 24 to 36 hours.

[0029] The present invention also provides fiber-modified reinforced soil prepared by the above preparation method.

[0030] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0031] 1. Combining fiber-reinforced soil technology with EICP technology, the surface roughness of polypropylene fibers is increased by modifying them using EICP technology. The calcium carbonate precipitate formed by EICP technology fills the gap between the fibers and the soil, thereby strengthening the interfacial strength of the fiber-reinforced soil. At the same time, the fibers provide nucleation sites for the precipitation of free calcium carbonate in the soil, and the high toughness of the fibers reduces the probability of brittle failure of the cemented soil.

[0032] 2. By coating the fiber surface with the reaction solution before mixing the fiber-reinforced soil, calcium carbonate can be induced to precipitate at the interface between the fiber and the soil. The calcium carbonate precipitate formed by EICP technology modifies the fiber surface, and the mixing of the fiber and soil further enhances the depth and uniformity of the calcium carbonate precipitation, effectively improving the utilization rate of the reaction solution. Furthermore, the calcium carbonate particles formed by EICP technology reach the micron level, while previous fiber surface modification methods mostly involved grafting chemical functional groups onto the fiber surface, resulting in roughening that often only reaches the nanometer level. Therefore, EICP technology can effectively increase the surface roughness of the fiber, improving its pull-out resistance in the soil.

[0033] 3. Adding a urease inhibitor during the EICP process suppresses the immediate reaction between urease and urea, prolonging the EICP process and providing a controllable window for calcium carbonate precipitation. In the combined treatment of fiber-reinforced soil and EICP, the addition of a urease inhibitor divides the calcium carbonate produced by the EICP reaction into two parts: one precipitates on the fiber surface during the inhibition phase to modify the fibers, and the other precipitates at the soil-reinforcement interface during the later inhibition phase to strengthen the interface. The addition of the urease inhibitor fully utilizes the calcium carbonate precipitate produced by the reaction to modify the fiber surface and fill the voids at the soil-reinforcement interface, improving the fiber's pull-out resistance in the soil and enhancing the strength of the soil-reinforcement interface through the cementing effect of calcium carbonate.

[0034] 4. Magnetized polypropylene fiber with a core is selected, and the fiber-reinforced soil is mixed in a magnetic field. The magnetic field induces the fiber to be oriented in the soil, preventing the fiber from entangled and agglomerated, which would cause uneven stress on the fiber-reinforced soil.

[0035] 5. Before surface roughening modification, use a silane coupling agent to disperse the fiber to prevent it from agglomerating due to intermolecular forces. Attached Figure Description

[0036] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention, wherein:

[0037] Figure 1 This is a schematic diagram of the fiber-modified reinforced soil preparation process of the present invention;

[0038] Figure 2 This is a comparison diagram of shear tests between Examples 1 and 2 and Comparative Example 1;

[0039] Figure 3 This is the SEM image of Comparative Example 1;

[0040] Figure 4 The images are SEM images of Examples 1 and 2. Detailed Implementation

[0041] The following disclosure provides many different embodiments or examples for implementing different structures of the invention. To simplify the disclosure, specific examples of components and arrangements are described below. Of course, these are merely examples and are not intended to limit the invention. Furthermore, reference numerals and / or letters may be repeated in different examples; such repetition is for simplification and clarity and does not in itself indicate a relationship between the various embodiments and / or arrangements discussed.

[0042] Example 1

[0043] A core layer material composed of magnetic powder and polypropylene chips is placed into the inner shaft injection pump of a two-component concentric core-sheath composite spinning machine, wherein the magnetic powder content is 60% of the core layer material; a sheath material composed of polypropylene chips is placed into the outer shaft injection pump of the two-component concentric core-sheath composite spinning machine. Melt spinning is then performed to obtain magnetized core-sheath polypropylene fibers.

[0044] Take 20g of the magnetized core polypropylene fiber prepared above and place it in a 1.0wt% dilute solution of silane coupling agent SCA-1613 prepared with anhydrous ethanol. Dispersion modification is carried out at room temperature for 20min. After dispersion modification, the fiber is washed and dried to prepare modified magnetized core polypropylene fiber.

[0045] Mix 100 ml of 10 g / L urease solution and 100 ml of 0.1 g / L urease inhibitor solution, and stir at room temperature for 20 min to obtain mixture A.

[0046] Mix 100 ml of 1 mol / L urea solution and 1 mol / L calcium chloride solution to obtain cementing solution B.

[0047] Weigh 100g of mixture A and spray it evenly onto the surface of the modified magnetized sheath-core polypropylene fiber.

[0048] Weigh another 100g of cementing liquid B and spray it evenly onto the surface of the modified magnetized sheath polypropylene fiber coated with the mixture A, thus completing the fiber surface roughening treatment.

[0049] Within 2 hours after the fiber surface roughening treatment is completed, the treated magnetized core polypropylene fiber and 10 kg of clay are placed in a directional magnetic field and mixed while vibrating to complete the preparation of fiber-reinforced soil.

[0050] The mixed soil is left to stand in a magnetic field for 24 hours, and the calcium carbonate in the soil is precipitated, thus obtaining the interface-reinforced fiber-reinforced soil.

[0051] Example 2

[0052] A core material composed of magnetic powder and polypropylene chips is placed into the inner shaft injection pump of a two-component concentric core-sheath composite spinning machine, wherein the magnetic powder content is 80% of the core material; a sheath material composed of polypropylene chips is placed into the outer shaft injection pump of the same machine. Melt spinning is then performed to obtain magnetized core-sheath polypropylene fibers.

[0053] Take 20g of the magnetized core polypropylene fiber prepared above and place it in a 1.0wt% dilute solution of silane coupling agent SCA-1613 prepared with anhydrous ethanol. Dispersion modification is carried out at room temperature for 20min. After dispersion modification, the fiber is washed and dried to prepare modified magnetized core polypropylene fiber.

[0054] Mix 100 ml of 80 g / L soybean flour solution and 100 ml of 0.1 g / L urease inhibitor solution, and stir at room temperature for 20 min to obtain mixture A.

[0055] Mix 100 ml of 1 mol / L urea solution and 1 mol / L calcium chloride solution to obtain cementing solution B.

[0056] Weigh 120g of mixture A, immerse the modified magnetized sheath-core polypropylene fiber in mixture A, and stir to ensure that mixture A fully coats the fiber surface.

[0057] Weigh another 120g of cementing solution B, immerse the modified magnetized sheath-core polypropylene fiber coated with mixture A into cementing solution B, stir to ensure that cementing solution B fully coats the fiber surface, thus completing the fiber surface roughening treatment.

[0058] Within 2 hours after the fiber surface roughening treatment is completed, the treated magnetized core polypropylene fiber and 10 kg of clay are placed in a directional magnetic field and mixed while vibrating to complete the preparation of fiber-reinforced soil.

[0059] The mixed soil is left to stand in a magnetic field for 24 hours, and the calcium carbonate in the soil is precipitated, thus obtaining the interface-reinforced fiber-reinforced soil.

[0060] Comparative Example 1

[0061] To demonstrate the role of fiber modification in this invention, this comparative example, compared with Examples 1 and 2, uses the same weight of untreated polypropylene fiber and clay to mix and prepare fiber-reinforced soil.

[0062] Performance testing:

[0063] For the fiber-reinforced soils obtained in the above embodiments and comparative examples, specimens were prepared and shear tests were conducted according to the "Standard for Geotechnical Testing Methods" (GB / T50123-2019). All shear specimens had the same compaction degree, with vertical pressures of 50 kPa, 100 kPa, 150 kPa, and 200 kPa, and a shear rate of 1.2 mm / min. The results are as follows: Figure 2 As shown.

[0064] The experimental results show that: Figure 2 It can be seen that the fiber-reinforced soil without fiber treatment has the lowest shear strength. In contrast, the shear strength of the fiber-reinforced soils in Examples 1 and 2 is significantly improved. The fibers added to the fiber-reinforced soil in Comparative Example 1 have not undergone fiber modification treatment, are non-magnetic, and have a smooth surface. Its SEM image is shown below. Figure 3 As shown in the figure. In Examples 1 and 2, the fibers added to the fiber-reinforced soil were magnetized sheath-core polypropylene fibers. The surface of the fibers was modified using EICP technology to increase their surface roughness, and their SEM images are shown below. Figure 4As shown. The fiber modification treatment in this invention increases the surface roughness of the fibers, thereby improving the pull-out resistance of the fibers in the soil. At the same time, the solution coating the fiber surface can continue to induce calcium carbonate precipitation at the interface between the fibers and the soil during soil mixing, thus strengthening the interfacial strength of the fiber-reinforced soil.

[0065] Other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art. The specification and examples are to be considered exemplary only, and the true scope and spirit of the invention are indicated by the claims.

[0066] It should be understood that the present invention is not limited to the precise structure described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.

Claims

1. A method for preparing fiber-modified reinforced soil, characterized in that, The fiber-modified reinforced soil comprises the following raw materials in parts by weight: 1000 parts clay, 2-4 parts modified magnetized core geofiber, 8-12 parts mixture A, and 8-12 parts cementing solution B; The preparation method includes the following steps: (1) The core material and the sheath material are respectively placed into a two-component concentric sheath-core composite spinning machine for melt spinning to obtain magnetized sheath-core geofiber. Then, it is placed in a silane coupling agent for dispersion modification, and then washed and dried to make modified magnetized sheath-core geofiber. (2) Mix the urease-containing reagent and the urease inhibitor to obtain a mixture A; mix the urea solution and the calcium chloride solution to obtain a cementing solution B; the urease-containing reagent is selected from a urease solution of 10~20g / L or a soybean flour solution of 50~100g / L, and the urease inhibitor is selected from 0.1~0.2g / L of n-butylthiophosphate triamine; (3) The modified magnetized core geofiber is coated with the mixture A and then coated with the cementing liquid B to produce a modified magnetized core geofiber with roughened surface. (4) Within 0.5 to 2 hours, the modified magnetized core geotextile fiber with surface roughening treatment and clay are placed in a directional magnetic field and mixed while vibrating. Then, the mixture is left to stand in the magnetic field until the calcium carbonate in the soil is completely precipitated, thus obtaining the fiber-modified reinforced soil. In step (1), the magnetized core geofiber is magnetized core polypropylene fiber; the core material is magnetic powder and polypropylene chips; the outer layer material is pure polypropylene chips; and the magnetic powder content in the core material is 50% to 80%.

2. The preparation method according to claim 1, characterized in that, All steps were performed at room temperature.

3. The preparation method according to claim 1, characterized in that, In step (1), the silane coupling agent is selected from any one of the dilute solutions of SCA-1603, SCA-1613 or SCA-1623 prepared with anhydrous ethanol; The concentration of the silane coupling agent is 0.6~1.0 wt%; The dispersion modification time is 20-30 minutes.

4. The preparation method according to claim 1, characterized in that, In step (2), the volume ratio of the urease-containing reagent to the urease inhibitor is 1:1; the mixing time is 20-30 min.

5. The preparation method according to claim 1, characterized in that, In step (2), the urea solution and the calcium chloride solution have the same concentration; The concentrations of both the urea solution and the calcium chloride solution are 0.5~1.5 mol / L; The volume ratio of the urea solution to the calcium chloride solution is 1:

1.

6. The preparation method according to claim 1, characterized in that, In step (3), the outer wrapping is achieved by soaking or spraying.

7. The preparation method according to claim 1, characterized in that, In step (4), the settling time is 24~36h.

8. Fiber-modified reinforced soil prepared by the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • A method for microbial mineralization modification of polypropylene fibers and its application

    CN109970381B

  • Method for mineralizing modification of polypropylene fibers and application of polypropylene fibers subjected to mineralizing modification

    CN109970381A

  • Grouting method for soil reinforcing through microbe induced mineralization by introducing of urease inhibitors

    CN111441337A