Method for forming a material coating layer by using a double-layer system of enhanced freeze-free anti-spacers
By utilizing the polymer mixture coating technology of the self-separating bilayer polymer system, the problem of the impact on the size of the underlying material during the removal of the coating layer is solved, achieving efficient and uniform coating layer removal and improving patterning accuracy and processing efficiency.
Patent Information
- Application Number
- CN202280039798.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-06-02
- Filing Date
- 2022-05-26
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-05-26
AI Technical Summary
Existing technologies struggle to effectively remove capping layers in photolithography processes without affecting the dimensions of the underlying material, especially during the formation of anti-spacers. Traditional methods may introduce defects or increase costs during the freezing step.
A polymer mixture outer coating is adopted using a self-separating bilayer polymer system. The first polymer fills the space below the embossed pattern, and the second polymer accumulates above the top surface of the embossed pattern. The controllable removal of the coating is achieved by utilizing surface energy difference and acid diffusion technology.
It achieves efficient removal of the capping layer, improves cross-wafer uniformity and patterning accuracy, reduces processing costs, and avoids the defects introduced by the freezing step.
Smart Images

Figure CN117546271B_ABST
Abstract
Description
[0001] Cross-reference to related applications
[0002] This disclosure claims the benefit of U.S. Provisional Application No. 63 / 195,756, filed June 2, 2021, which is incorporated herein by reference in its entirety. Technical Field
[0003] This disclosure relates to a method of semiconductor manufacturing, and more particularly to utilizing the surface energy differences found in some fluorinated polymers or polymers having long-chain alkyl functional groups, which promotes the segregation of the surface or top layer in a bilayer polymer system to facilitate the removal of capping material coated on the structure. Background Technology
[0004] The background description provided herein is intended to present the general context of this disclosure. The work of the present inventors, to the extent described in this background section, and aspects of this description that might not have been considered prior art at the time of submission, neither expressly nor implicitly acknowledges that it is prior art to this disclosure.
[0005] In materials processing methods (such as photolithography), creating a patterned layer typically involves applying a thin layer of radiation-sensitive material (such as photoresist) to the upper surface of a substrate. This radiation-sensitive material is then converted into a patterned mask in a lower layer that can be used to etch or transfer patterns onto the substrate. Patterning the radiation-sensitive material generally involves exposing it to the radiation-sensitive material from a radiation source through a mask (and associated optics) using, for example, a photolithography exposure system. This exposure creates a latent pattern within the radiation-sensitive material, which can then be developed. Development refers to dissolving and removing a portion of the radiation-sensitive material to create an embossed pattern (morphological pattern). Depending on the photoresist hue and / or the type of developing solvent used, the removed material portion can be either an irradiated or unirradiated area of the radiation-sensitive material. The embossed pattern can then be used as a mask layer defining the pattern.
[0006] The preparation and development of various films used for patterning may include heat treatment or baking. For example, newly applied films may undergo post-application baking (PAB) to evaporate solvents and / or increase structural stiffness or etch resistance. Additionally, post-exposure baking (PEB) may be performed to set a given pattern to prevent further dissolution. Processing tools used for coating and developing substrates typically include one or more baking modules. Some photolithography processes involve coating a substrate with a thin film of bottom anti-reflective coating (BARC), followed by coating with a resist, and then exposing the substrate to a light pattern as a process step to form a microchip. The resulting relief pattern can then be used as a mask or template for additional processing, such as transferring the pattern to an underlying layer.
[0007] The relief pattern may be covered by deposited material that fills the trenches for the final spacer formation. The deposited material can be further modified to adjust the dimensions of the final spacers. However, to develop the modified deposited material, it may be necessary to remove the overburden to access the modified portion. However, some soft materials cannot withstand etching or chemical mechanical polishing processes. Therefore, a method is desired to remove the overburden without affecting the underlying material or introducing changes to the dimensions of the modified material. Summary of the Invention
[0008] This disclosure relates to a method for patterning a substrate, the method comprising forming an embossed pattern including relief structures on the substrate by forming a first layer of photoresist on the substrate, the first layer of photoresist comprising a first solubility modifier and a second solubility modifier, the photoresist being sensitive to the first solubility modifier and the second solubility modifier, the embossed pattern being formed by activating the first solubility modifier by patterning with photochemical radiation and developing the first layer of photoresist; depositing a polymer mixture on these embossed structures, the polymer mixture filling openings defined by the embossed pattern and covering these embossed structures, the region above the top surface of these embossed structures being a capping layer region, the polymer mixture comprising a first polymer and a second polymer, the polymer mixture being configured to self-separate relative to gravity such that the polymer mixture... Forming a first film and a second film, the first film containing the first polymer being formed beneath the second film containing the second polymer, the formation of the first film and the second film such that the second film fills the capping layer region, the first film being sensitive to the second solubility modifier and having a sensitivity threshold less than the sensitivity threshold of the photoresist, the second film being soluble in a first developer; activating the second solubility modifier and causing the second solubility modifier to diffuse from these relief structures to the first film by a predetermined diffusion length, the second solubility modifier being sufficiently activated to reach the sensitivity threshold of the first film but not the sensitivity threshold of the photoresist, the diffusion region formed in the first film becoming soluble in the first developer while the photoresist remains insoluble in the first developer; and developing the substrate to remove the soluble diffusion regions of the second film and the first film.
[0009] This disclosure also relates to a method for patterning a substrate, the method comprising forming an embossed pattern including embossed structures on the substrate by forming a first layer of photoresist on the substrate, the first layer of photoresist comprising a first solubility modifier and a second solubility modifier, the photoresist being sensitive to the first solubility modifier and the second solubility modifier, the embossed pattern being formed by pattern activation of the first solubility modifier by photochemical radiation and development of the first layer of photoresist; depositing a resin coating layer on these embossed structures, the resin coating layer filling openings defined by the embossed pattern and covering these embossed structures, the region above the top surface of these embossed structures being a coating layer region, the resin coating layer having a resin mixture comprising the first resin and the second resin, the resin coating layer being configured to self-separate relative to gravity such that the resin... An outer coating is formed to form a first film and a second film, the first film containing the first resin being formed beneath the second film containing the second resin, the first film and the second film being formed such that the second film fills the coating region, the first film being sensitive to the second solubility modifier and having a sensitivity threshold less than the sensitivity threshold of the photoresist, the second film being soluble in a first developer; the second solubility modifier is activated and diffused from these relief structures to the first film by a predetermined diffusion length, the second solubility modifier being sufficiently activated to reach the sensitivity threshold of the first film but not the sensitivity threshold of the photoresist, the diffusion region formed in the first film becoming soluble in the first developer while the photoresist remains insoluble in the first developer; and the substrate is developed to remove the soluble diffusion regions of the second film and the first film.
[0010] This disclosure also relates to a method for patterning a substrate, the method comprising receiving a substrate having features defining openings to be partially filled; depositing a polymer mixture on the substrate, the polymer mixture filling the openings defined by the features and covering the features, a region above the top surface of the features being a capping region, the polymer mixture comprising a first polymer and a second polymer, the polymer mixture being configured to self-separate relative to gravity such that a first film and a second film are formed from the polymer mixture, the first film comprising the first polymer being formed beneath the second film comprising the second polymer, the first film and the second film being formed such that the first film partially fills the defined openings while the second film fills the remaining portion of the defined openings and fills the capping region, the second film being sensitive to a specific solvent while the first film is insoluble in the specific solvent; and developing the substrate with the specific solvent to remove the second film, the first film remaining in the defined openings.
[0011] Note that the Summary of this invention does not specify every embodiment and / or additional novel aspect of the invention disclosed herein or claimed. Rather, the Summary provides only a preliminary discussion of different embodiments and corresponding points of novelty. For additional details and / or possible perspectives on the invention and embodiments, the reader is directed to the Detailed Description of this disclosure and the corresponding drawings, which are discussed further below. Attached Figure Description
[0012] Various embodiments of this disclosure will be described in detail by way of example with reference to the following accompanying drawings, wherein similar reference numerals denote similar elements, and wherein:
[0013] Figure 1A The embodiments of this disclosure illustrate a cross-sectional substrate segment including an embossed pattern.
[0014] Figure 1B The embodiment of this disclosure shows a cross-sectional substrate segment of material deposited on an embossed pattern.
[0015] Figure 1C The embodiments of this disclosure demonstrate a modified cross-sectional substrate segment of the outer coating.
[0016] Figure 1D The cross-sectional substrate segment showing the development result is shown in the embodiment of this disclosure.
[0017] Figure 1E The embodiment of this disclosure illustrates a cross-sectional substrate segment with developing factors.
[0018] Figure 2A The embodiments of this disclosure illustrate a cross-sectional substrate segment including an embossed pattern.
[0019] Figure 2B The embodiment of this disclosure shows a cross-sectional substrate segment of material deposited on an embossed pattern.
[0020] Figure 2C The embodiment of this disclosure illustrates a cross-sectional substrate segment with acid diffusion.
[0021] Figure 2D The cross-sectional substrate segment showing the development result is shown in the embodiment of this disclosure.
[0022] Figure 3A The embodiment of this disclosure illustrates a cross-sectional substrate segment with a single polymer overlay.
[0023] Figure 3B An embodiment of the present disclosure illustrates a cross-sectional substrate segment with a recessed single polymer overlay.
[0024] Figure 4A The embodiments of this disclosure illustrate a cross-sectional substrate segment of a polymer bilayer film system.
[0025] Figure 4B The embodiment of this disclosure illustrates a cross-sectional substrate segment of a recessed polymer bilayer film system.
[0026] Figure 5 The image shows a transparent substrate segment of a deposited polymer bilayer film system according to embodiments of this disclosure.
[0027] Figure 6 This is a flowchart of a method for patterning a substrate according to an embodiment of the present disclosure. Detailed Implementation
[0028] The following disclosure provides numerous different embodiments or instances for implementing various features of the provided subject matter. Specific examples of components and arrangements are described below to simplify this disclosure. Of course, these are merely examples and are not intended to be limiting. For example, the following description of forming a first feature on or over a second feature may include embodiments where the first and second features are in direct contact, and may also include embodiments where an additional feature may be formed between the first and second features such that the first and second features are not in direct contact. Additionally, reference numerals and / or letters may be repeated in various instances throughout this disclosure. This repetition is for simplicity and clarity and does not in itself indicate a relationship between the various embodiments and / or configurations discussed. Furthermore, for ease of description, spatially related terms such as “top,” “bottom,” “beneath,” “below,” “lower,” “above,” and “upper” may be used herein to describe the relationship of one element or feature as shown in the figures to other elements(s)(s). In addition to the orientations depicted in the figures, spatially related terms are also intended to cover different orientations of the device in use or operation. The device can be oriented in other ways (rotated 90 degrees or in other orientations), and thus the spatially relevant descriptors used in this paper can also be interpreted.
[0029] For clarity, the order of discussion of the different steps described herein has been presented. In general, these steps can be performed in any suitable order. Furthermore, although each of the different features, techniques, configurations, etc., described herein may be discussed in different places within this disclosure, it is intended that each of the concepts can be performed independently of or in combination with each other. Therefore, the invention can be embodied and viewed in many different ways.
[0030] Continuous miniaturization requires increased patterning resolution. One approach is to use spacer techniques to define sub-resolution line features via atomic layer deposition (ALD). However, a challenge is that using spacer techniques can be complex if opposite-tone features are desired, involving overcoating another material, chemical mechanical planarization (CMP), and reactive ion etching (RIE) to excavate the spacer material, leaving narrow trenches, which can be expensive.
[0031] Anti-spacers are a self-aligned technique that uses the diffusion length of a reactive material to define the critical dimension (CD), thereby creating narrow trenches. Using reactive materials spatially controlled via mask exposure, narrow trench contacts can be formed without creating narrow trenches. Instead of spatial control, reactive materials can be uniformly controlled across the entire wafer by decomposing the thermogenic acid generator (TAG) through a baking process. The CD can be adjusted by changing the molecular weight of the reactive material, its molecular structure, and by the baking temperature and time. Furthermore, the CD can be controlled by the composition of the material into which the reactive material diffuses. The polarity of the components within the resin (the material into which the reactive material diffuses) can affect the acid diffusivity and the activation energy of the reactive material-sensitive components of the material, serving as an additional means of controlling the process. These techniques enable the acquisition of narrow trench contact features at dimensions exceeding the capabilities of advanced lithography. However, the process may include a freezing step. The freezing step can be a process to neutralize the solubility change potential of the layer containing the acid generator. However, freezing can introduce defects or errors and may reduce throughput.
[0032] The previously described anti-spacer process uses a thermal freezing process, in which the deprotected photoresist core is suppressed from dissolving in an aqueous developer used to remove the deprotected (or decrosslinked or otherwise amended solubility) outer coating and expose the anti-spacer features. Integrating thermal freezing functionality into photoresist may be challenging due to the stringent requirements of high-volume manufacturing and the reaction environment of the polymer resin.
[0033] To this end, U.S. Patent Application No. 63 / 135,217, "Freeze-less Anti-spacer Formation by Contrast Selectivity," describes a technique for forming sub-resolution anti-spacer features without the need for thermal freezing, i.e., a "freeze-free" anti-spacer method, which is incorporated herein by reference in its entirety. It describes a method for forming sub-resolution anti-spacer features below the deprotection threshold of the photoresist core required to achieve solubility in an aqueous developer. The inherent solubility contrast of the coating layer is paired with the photoresist core, allowing the solubility of the coating layer to be altered to form the anti-spacer, while the photoresist remains relatively insoluble or sufficiently insoluble in the developer solution. This process provides a method to avoid the thermal freezing step required to prevent the photoresist core from dissolving. Therefore, no additional TAG is required in the core formulation.
[0034] The process described in the combined disclosure offers improved patterning benefits; however, this process involves removing a cover layer from the resin outer coating. The cover layer is the amount of filler material above the top surface of the mandrel or the top surface of the embossed pattern (see below). The cover layer can be removed to access or expose the anti-spacer features for pattern transfer or further patterning.
[0035] The technique described herein enhances this anti-spacer formation method by using a polymer mixture overlay that self-separates into a bilayer polymer system. A first polymer fills the space below the top surface of the embossed pattern, while a second polymer assembles above the top surface of the embossed pattern. After the anti-spacer feature is formed by acid diffusion, the second polymer can be easily removed with a developer without affecting the first polymer or the embossed pattern.
[0036] This article describes a technique for promoting the segregation of the surface layer (or upper film) in a bilayer polymer system by utilizing surface energy differences found in some fluorinated polymers or polymers with long-chain alkyl functional groups. Therefore, the capping layer of the filler material used for anti-spacer formation can be easily removed to approximate the characteristics produced by the deprotected region defined by the diffusion length.
[0037] to this end, Figure 1AThis disclosure illustrates a cross-sectional substrate segment of a substrate 105 including an embossed pattern 110, according to embodiments thereof. In embodiments, the embossed pattern 110 may be formed on the surface of the substrate 105. For example, a photolithography process may be used, in which a photoresist material layer may be imaged and developed into the embossed pattern 110. The embossed pattern 110 may, for example, produce a mandrel 110a after development. Depending on the desired final features, multiple mandrels 110a may also be formed into the embossed pattern 110. Notably, the mandrel 110a may include a width and a height, wherein the height of the mandrel 110a may be defined by a distance measured from the surface of the substrate 105 to the top of the mandrel 110a.
[0038] Figure 1B This is a cross-sectional substrate segment illustrating the deposition of material on an embossed pattern 110 according to an embodiment of this disclosure. In the embodiment, the outer coating 115a can be deposited on the embossed pattern 110 via, for example, a spin coating process. Other non-limiting examples of coating processes may include, among others, dip coating, flow coating, spray coating, etc. The deposited material can be, for example, a resin or polymer 115. Notably, excessive deposition of resin / polymer 115 may result in a certain amount of resin / polymer 115 coating over the top of the mandrel 110a. This excess can be defined as a capping layer. It may be necessary to remove this capping layer to expose the top of the mandrel 110a for further processing. For example, a CMP process can be used to physically remove the capping layer of the outer coating 115a and planarize the outer coating 115a. However, processes like CMP may not be able to remove the outer coating 115a material between the mandrels 110a without reducing the overall height of the embossed pattern 110.
[0039] Figure 1C This embodiment of the disclosure illustrates a modified cross-sectional substrate segment of the outer cover 115a. In this embodiment, the material of the embossed pattern 110 may include an acid, which can diffuse from the embossed pattern 110 into the surrounding outer cover 115a and form a soluble region 120. That is, the acid can modify the resin / polymer 115 and cause a change in solubility. Notably, the diffusion length may not completely change the solubility of the cover layer above the top surface of the mandrel 110a, depending on the formulation of the polymer mixture. Therefore, additional process steps, such as CMP as described above, may be performed to remove the insoluble cover layer before approaching the narrow opening (trench) of the anti-spacer. Even if the outer cover 115a has partial solubility in a predetermined developer, this may still inhibit complete spacer formation. If the solubility of the outer cover 115a increases, the trench and CD uniformity across the entire wafer (substrate 105) may exhibit more variation than expected. This may also depend on the morphology of the substrate 105 and the target size to be approached.
[0040] Figure 1D This is a cross-sectional substrate segment illustrating the development result according to an embodiment of this disclosure. In this embodiment, the developer can remove the soluble region 120 after exposing the soluble region 120 of the outer coating 115a. Figure 1D As shown, the narrow opening or anti-spacer can be defined by the diffusion length of the acid that causes a change in the solubility of resin / polymer 115.
[0041] Figure 1E This is a cross-sectional substrate segment illustrating development factors according to an embodiment of the present disclosure. In the embodiment, the capping layer height and the time for clearing the anti-spacer trenches can limit the development time. Thus, excessive development time will widen the anti-spacer trenches, and therefore a low dissolution rate can provide a larger process window. As shown, the height of the mandrel 110a is not flush with the height of the remaining outer capping layer 115a. Notably, in the anti-spacer process flow, a double outer capping layer can help improve cross-wafer uniformity compared to a single polymer capping layer.
[0042] This article describes a method for patterning a substrate and forming anti-spacer features, wherein the step of removing the capping layer is facilitated by a polymer mixture outer capping layer that self-separates into a bilayer polymer system.
[0043] to this end, Figure 2A This embodiment of the disclosure illustrates a cross-sectional substrate segment of a substrate 105 including an embossed pattern 110. In this embodiment, similar to the previously described, a photoresist layer can be deposited, imaged, and developed into the embossed pattern 110.
[0044] Figure 2BThis is a cross-sectional substrate segment illustrating the deposition of material on an embossed pattern 110 according to an embodiment of this disclosure. In the embodiment, the outer coating 115a can be deposited on the embossed pattern 110 via, for example, a spin coating process. Other non-limiting examples of coating processes may include, among others, dip coating, flow coating, spray coating, etc. Here, the deposited material can be, for example, a resin or polymer mixture. The polymer mixture may include, for example, resin / polymer 115 and a highly soluble resin / polymer 125, as the first resin / polymer and the second resin / polymer in the mixture, respectively. Non-limiting examples of highly soluble resin / polymer 125 may include, among others, HFIP-M, MA-MIB-HFA, MA-BTHB-OH, MA-3,5-HFA-CHOH, MA-BTHB-NB, MA-EATf, and MA-DM-EATf. Non-limiting examples of resin / polymer 115 may include any type of methacrylate or phenolic polymer that has reverse solubility in the mandrel 110a material. The outer coating 115 can fill the opening defined by the embossed pattern 110 and cover the embossed pattern 110. It is worth noting that excessive deposited polymer mixture may again produce a coating covering the top of the mandrel 110a.
[0045] In embodiments, the polymer mixture can be configured to self-segregate or self-aggregate. For example, the polymer mixture can self-segregate relative to gravity or a plane perpendicular to the surface of substrate 105. Self-segregation can occur after deposition without any activation, or an activation step can be used based on the composition of the polymer mixture. For example, a baking step can be used for thermal activation. Self-segregation can produce bilayer or two-layer films. Figure 2B A bilayer film after self-separation is shown, comprising a resin / polymer 115 film disposed below a high-solubility resin / polymer 125 film. The compositions of the films can have different properties. For example, the lower resin / polymer 115 film can be configured to provide good etch resistance. For example, the lower resin / polymer 115 film can have very low or no solubility in TMAH unless ester protecting groups are present and deprotection occurs in the presence of an acid. Conversely, the upper high-solubility resin / polymer 125 film can have very high solubility in, for example, TMAH. The lower resin / polymer 115 film can also be configured to change solubility at lower thresholds for acids or other reagents compared to photoresist materials. Depending on the materials selected and the given concentration in the formulation, in-situ polymer separation of 10-30 Å or higher can be achieved in the upper high-solubility resin / polymer 125 film.
[0046] Notably, in the embodiments, the relative amounts of the first polymer and the second polymer (e.g., resin / polymer 115 and high-solubility resin / polymer 125) can be configured such that there is sufficient second polymer material for the area to be covered by the second polymer. The second polymer film can even extend below the top surface of the mandrel 110a in the embossed pattern 110. The second polymer film, or upper polymer layer, can be configured differently from the first polymer layer. The second polymer layer can be configured to be soluble in a predetermined developer or solvent without requiring a reagent that alters the solubility. Therefore, the polymer mixture formulation facilitates easier removal of the upper film or cover layer, thereby exposing the embossed pattern 110 and a portion of the potential lower resin / polymer 115 film.
[0047] Figure 2C The embodiment of this disclosure illustrates a cross-sectional substrate segment with acid diffusion. In the embodiment, the highly soluble resin / polymer 125 separated in the upper portion can be designed to have a relatively high dissolution rate in a predetermined developer. This allows for very rapid removal of the capping layer to expose the anti-spacer region. After acid diffusion forms the soluble region 120 and subsequently deprotection, the anti-spacer region is also soluble in the predetermined developer. The acid diffusion length or distance can be precisely controlled by baking time, temperature, and other factors. Combining the highly soluble resin / polymer 125 on top of the double-layer arrangement of the outer capping layer 115a eliminates the need for a specific dissolution rate of the remaining polymer in the developer, and therefore makes it easier to match the etching selectivity and plateau type with the polymer in the first (lower) film.
[0048] Removing the covering layer allows access to the anti-spacer area, such as Figure 2CAs indicated by the middle arrow. The high-solubility resin / polymer 125 can be used to develop the anti-spacer using a specific developer dissolution rate while maintaining the desired aspect ratio of the formed lines. Another characteristic of the lower resin / polymer 115 film can be that it has different etch selectivity. Preferably, the etch selectivity of the lower resin / polymer 115 film and the mandrel 110a material is similar to optimize etch transfer to the lower layers. Furthermore, in embodiments, the high-solubility resin / polymer 125 may not require etch selectivity. To alleviate some of the challenges of lower film selectivity, a small amount of blended polymer can be used in the upper high-solubility resin / polymer 125 film. The blended polymer can be selected to be chemically different from the main polymer because the surface energy of the blended polymer allows it to segregate to the top of the film during coating (e.g., spin coating). The blended polymer can also have high developer solubility without requiring etch selectivity. Separating polymer films to form a monolayer in a top coating for 193nm immersion lithography can produce very thin films and form bulk heterojunctions for exciton separation in photovoltaic devices. For the embodiments described herein, a thicker, highly soluble resin / polymer 125 layer can migrate to the surface of the underlying resin / polymer 115 film formulation at a thickness similar to that of the capping layer.
[0049] Figure 2D This is a cross-sectional substrate segment illustrating the development results according to an embodiment of this disclosure. In this embodiment, the upper high-solubility resin / polymer 125 film has a high developer dissolution rate that exposes the area of the lower resin / polymer 115 film that has reacted with diffused acid to form developer-soluble anti-spacer region 120. The polymer retained in the lower film now does not require inherent or unexposed developer solubility, and more attention can be focused on other properties, such as etch selectivity. Another advantage of the primary polymer in the lower resin / polymer 115 film not having developer solubility is improved uniformity across the wafer. Having an upper, developer-soluble, high-solubility resin / polymer 125 (which covers slightly more of the capping layer portion than the outer capping layer 115a) in the bilayer polymer film system allows for some inherent self-correction of non-uniformity across the wafer. The soluble anti-spacer can also be removed after the upper film is removed.
[0050] Other process steps described herein are similar to those in the rate-selective process for reverse spacer formation and do not require additional steps. A first resist, including an additional acid source, can be coated and imaged. A second formulation, including a polymer bilayer system, can be coated on top of the first layer image. This formulation can be coated with a solvent that does not dissolve the first layer pattern and may include, but is not limited to, MIBC (methylisobutyl carbitol). The second formulation may optionally include a solvent that promotes the separation of the two polymers present. The lower surface energy polymer may contain fluorinated moieties or long alkyl chain functional groups to promote surface energy differences. The lower surface energy polymer may also include acidic functional groups to promote efficient dissolution in the developer. Promoting morphological separation to form a capping layer provides the improvements described herein. The primary polymer in the lower layer can be any polymer with similar chemical properties to the first layer patterned resist, preferably having functional groups that promote similar etch selectivity. The primary polymer may include a switchable component that is protected (altering solubility) at a lower activation energy than the first layer polymer. The new soluble region is soluble in solvents that do not dissolve the first layer pattern.
[0051] In this embodiment, after the deposition of the polymer bilayer film, a baking step can be performed to generate acid and diffuse it into the underlying polymer, wherein the deprotection step alters the solubility of the primary polymer. A subsequent development step can remove the high-dissolution-rate capping layer and the areas deprotected by the acid diffusion baking. After the development step, trenches and lines have been formed from the underlying film. A new pattern with smaller trenches can now be transferred to the underlying layer.
[0052] Advantageously, in the anti-spacer process, the polymer bilayer film system described herein improves cross-wafer uniformity compared to a single polymer overlay. In the polymer bilayer system, the overlay can be a different material from the sidewalls, and the lower polymer in the polymer bilayer system does not require solubility in, for example, TMAH. As will be understood, various polymers and compositions can be selected to form the polymer bilayer system. Depending on the chosen polymer and solvent system, the upper layer can have different heights. A given overlay height and the time required to clear the anti-spacer trenches can therefore define the corresponding development time. Increasing the development time can widen the anti-spacer trenches, while a lower dissolution rate can provide a larger process window.
[0053] to this end, Figure 3A The embodiment of this disclosure illustrates a cross-sectional substrate segment with a single polymer overlay. Figure 3BThis embodiment of the disclosure illustrates a cross-sectional substrate segment with a recessed single polymer overlay. In the embodiment, there are numerous fabrication stages in which it is desired to partially fill trenches or openings. Some processes may include depositing a single polymer overlay 115a, followed by an etching step to remove the overlay and recess the material. This type of etching may not have an etch stop layer, and therefore uses the etch duration to estimate the amount of recess, which may have poor control. Atomic layer etching can be used, but this may increase costs and reduce throughput.
[0054] thus, Figure 4A The embodiments of this disclosure illustrate a cross-sectional substrate segment of a polymer bilayer film system. Figure 4B The embodiment of this disclosure illustrates a cross-sectional substrate segment of a recessed polymer bilayer film system. In the embodiment, the polymer mixture can be selected to be soluble in different developers and self-separate or self-aggregate into at least two layers. The upper film (highly soluble resin / polymer 125) can fill the capping layer region and partial openings. The upper film can be removed with a specific solvent that does not dissolve the lower film (resin / polymer 115) or has at least a significantly slower dissolution rate, such that the upper film can be removed while the lower film remains.
[0055] As will be understood, there may be several applications where it is desirable to fill recessed grooves. As a non-limiting example, one application includes forming recesses using spin-coated glass. Figure 5 This is a transparent substrate segment illustrating a deposited polymer bilayer film system according to embodiments of this disclosure. Figure 5 On the left side, precise recesses are desired between the spacers. A polymer mixture can be deposited on a substrate with the feature / opening. This polymer mixture can be segregated to a precise depth within the trench and then removed by rinsing with a spin-coating solvent. One advantage of this bilayer recess is that it can be implemented on a track tool (coater-developer tool) to increase throughput. In some recess applications, the polymer bilayer film system can be a predefined alternative to bottom growth that is independent of substrate or sidewall selectivity. It should be noted that the bilayer segregation described herein is not limited to soft materials and any type of spin-coating material mixture that supports self-segregation can be used.
[0056] In summary, the bilayer outer coating film allows for high-throughput methods for forming a capping layer of controlled thickness, which can be removed to form a flat surface or precisely calibrated recesses. During anti-spacer applications, the outer coating polymer segregated to the surface exhibits high developer solubility. The development step rapidly removes the top polymer forming the capping layer, thereby exposing the underlying deprotected polymer and forming trenches. The protected, acid-labile outer coating polymer on the bottom of the bilayer does not require developer solubility, which enhances uniformity across wafer CDs and allows for improved polymer functionality.
[0057] Figure 6 This is a flowchart of a method 600 for patterning a substrate according to an embodiment of the present disclosure.
[0058] Step 605 involves depositing the first layer of photoresist onto the substrate.
[0059] Step 610 involves forming an embossed pattern from a first layer of photoresist. The first layer of photoresist contains a first solubility modifier and a second solubility modifier. The photoresist is sensitive to the first and second solubility modifiers. The embossed pattern is formed by activating the first solubility modifier through photochemical radiation and developing the first layer of photoresist.
[0060] Step 615 involves depositing a resin or polymer mixture onto these relief structures, the resin / polymer mixture filling the openings defined by the relief pattern and covering the relief structures. The area above the top surface of these relief structures is a capping layer area. The resin / polymer mixture comprises a first resin / polymer and a second resin / polymer. The resin / polymer mixture is configured to self-separate relative to gravity such that a first film and a second film are formed from the resin / polymer mixture. The first film, comprising the first resin / polymer, is formed below the second film, comprising the second resin / polymer. The formation of the first film and the second film is such that the second film fills the capping layer area. The first film is sensitive to the second solubility modifier and has a sensitivity threshold less than the sensitivity threshold of the photoresist. The second film is soluble in the first developer.
[0061] Step 620 is to activate the second solubility modifier and diffuse it from these relief structures to the first film by a predetermined diffusion length. The second solubility modifier is sufficiently activated to reach the sensitivity threshold of the first film but not the sensitivity threshold of the photoresist. The diffusion region formed in the first film becomes soluble in the first developer while the photoresist remains insoluble in the first developer.
[0062] Step 625 involves developing the substrate to remove the soluble diffusion regions of the second film and the first film.
[0063] A method for patterning a substrate includes forming an embossed pattern comprising embossed structures on the substrate by forming a first photoresist layer on the substrate, the first photoresist layer comprising a first solubility modifier and a second solubility modifier, the photoresist being sensitive to the first solubility modifier and the second solubility modifier, the embossed pattern being formed by pattern activation of the first solubility modifier using photochemical radiation and developing the first photoresist layer; depositing a polymer mixture on the embossed structures, the polymer mixture filling openings defined by the embossed pattern and covering the embossed structures, the region above the top surface of the embossed structures being a capping layer region, the polymer mixture comprising a first polymer and a second polymer, the polymer mixture being configured to self-separate relative to gravity such that a first polymer layer is formed from the polymer mixture. A first film and a second film, the first film containing the first polymer being formed beneath the second film containing the second polymer, the first film and the second film being formed such that the second film fills the capping layer region, the first film being sensitive to the second solubility modifier and having a sensitivity threshold less than the sensitivity threshold of the photoresist, the second film being soluble in a first developer; activating the second solubility modifier and causing the second solubility modifier to diffuse from these relief structures to the first film by a predetermined diffusion length, the second solubility modifier being sufficiently activated to reach the sensitivity threshold of the first film but not the sensitivity threshold of the photoresist, the diffusion region formed in the first film becoming soluble in the first developer while the photoresist remains insoluble in the first developer; and developing the substrate to remove the soluble diffusion regions of the second film and the first film.
[0064] In the examples, the polymer mixture is deposited via spin coating deposition.
[0065] In one embodiment, the polymer mixture self-separates after being deposited on the substrate.
[0066] In one embodiment, the second membrane extends below the top surface of these relief structures after self-separation.
[0067] In an embodiment, the polymer mixture self-separates in response to heat, and the method further includes performing thermal baking after depositing the polymer mixture onto these embossed structures.
[0068] In an embodiment, developing the substrate further includes developing the substrate with the first developer to remove the soluble diffusion regions of the second film and the first film.
[0069] In an embodiment, the second film is soluble in the second developer, and developing the substrate further includes developing the substrate with the second developer to remove the second film before developing the substrate with the first developer to remove the soluble diffusion region of the first film.
[0070] In one embodiment, the second film is removed after the second solubility modifier is activated.
[0071] In an embodiment, the second film is removed before activating the second solubility modifier.
[0072] In the embodiments, the materials of the second polymer include HFIP-M, MA-MIB-HFA, MA-BTHB-OH, MA-3,5-HFA-CHOH, MA-BTHB-NB, MA-EATf, and MA-DM-EATf.
[0073] A method for patterning a substrate includes forming an embossed pattern comprising embossed structures on the substrate by forming a first photoresist layer on the substrate, the first photoresist layer comprising a first solubility modifier and a second solubility modifier, the photoresist being sensitive to the first solubility modifier and the second solubility modifier, the embossed pattern being formed by pattern activation of the first solubility modifier using photochemical radiation and development of the first photoresist layer; depositing a resin coating layer on the embossed structures, the resin coating layer filling openings defined by the embossed pattern and covering the embossed structures, the region above the top surface of the embossed structures being a coating layer region, the resin coating layer having a resin mixture comprising the first resin and the second resin, the resin coating layer being configured to self-separate relative to gravity such that the resin coating layer forms A first film and a second film, the first film containing the first resin being formed beneath the second film containing the second resin, the first film and the second film being formed such that the second film fills the capping layer region, the first film being sensitive to the second solubility modifier and having a sensitivity threshold less than the sensitivity threshold of the photoresist, the second film being soluble in a first developer; activating the second solubility modifier and causing the second solubility modifier to diffuse from these relief structures to the first film by a predetermined diffusion length, the second solubility modifier being sufficiently activated to reach the sensitivity threshold of the first film but not the sensitivity threshold of the photoresist, the diffusion region formed in the first film becoming soluble in the first developer while the photoresist remains insoluble in the first developer; and developing the substrate to remove the soluble diffusion regions of the second film and the first film.
[0074] In an embodiment,
[0075] In this embodiment, the resin coating is deposited via spin coating deposition.
[0076] In one embodiment, the resin coating self-separates after being deposited on the substrate.
[0077] In one embodiment, the second membrane extends below the top surface of these relief structures after self-separation.
[0078] In one embodiment, the resin coating segregates upon heating, and the method further includes performing a heat-baking process after depositing the resin coating onto the embossed structures.
[0079] In an embodiment, developing the substrate further includes developing the substrate with the first developer to remove the soluble diffusion regions of the second film and the first film.
[0080] In an embodiment, the second film is soluble in the second developer, and developing the substrate further includes developing the substrate with the second developer to remove the second film before developing the substrate with the first developer to remove the soluble diffusion region of the first film.
[0081] In one embodiment, the second film is removed after the second solubility modifier is activated.
[0082] In an embodiment, the second film is removed before activating the second solubility modifier.
[0083] A method for patterning a substrate includes receiving a substrate having features defining openings to be partially filled; depositing a polymer mixture on the substrate, the polymer mixture filling the openings defined by the features and covering the features, a region above the top surface of the features being a capping region, the polymer mixture comprising a first polymer and a second polymer, the polymer mixture being configured to self-separate relative to gravity such that a first film and a second film are formed from the polymer mixture, the first film comprising the first polymer being formed beneath the second film comprising the second polymer, the first film and the second film being formed such that the first film partially fills the defined openings while the second film fills the remaining portion of the defined openings and fills the capping region, the second film being sensitive to a specific solvent while the first film is insoluble in the specific solvent; and developing the substrate with the specific solvent to remove the second film, the first film remaining in the defined openings.
[0084] In the foregoing description, specific details, such as the particular geometry of the processing system and the description of the various components and processes used therein, have been set forth. However, it should be understood that the techniques described herein may be practiced in other embodiments departing from these specific details, and such details are for illustrative purposes and not for limitation. Embodiments disclosed herein have been described with reference to the accompanying drawings. Similarly, specific figures, materials, and configurations have been set forth for illustrative purposes to provide a thorough understanding. However, embodiments may be practiced without such specific details. Components having substantially the same functional construction are indicated by similar reference characters, and therefore any redundant descriptions may be omitted.
[0085] Various techniques have been described as multiple discontinuous operations to aid in understanding the various embodiments. The order of description should not be construed as implying that these operations must be performed in sequence. In fact, these operations do not need to be performed in the presented order. The described operations may be performed in an order different from the order of the described embodiments. In additional embodiments, various additional operations may be performed and / or the described operations may be omitted.
[0086] As used herein, "substrate" or "target substrate" generally refers to the object being processed according to the invention. A substrate may include any material portion or structure of a device (particularly a semiconductor or other electronic device) and may be, for example, a base substrate structure (e.g., a semiconductor wafer, a photomask), or a layer on or overlaid on a base substrate structure (e.g., a thin film). Therefore, a substrate is not limited to any particular base structure, lower layer, or upper layer, whether patterned or unpatterned, but is contemplated to include any such layer or base structure, and any combination of layers and / or base structures. This description may refer to specific types of substrates, but this is for illustrative purposes only.
[0087] Those skilled in the art will also understand that many changes can be made to the operation of the techniques explained above while still achieving the same objectives of the invention. The scope of this disclosure is intended to cover such changes. Therefore, the foregoing description of embodiments of the invention is not intended to be limiting. Rather, any limitations on embodiments of the invention are set forth in the appended claims.
Claims
1. A method for patterning a substrate, the method comprising: An embossed pattern comprising an embossed structure is formed on a substrate by a first layer of photoresist on the substrate. The first layer of photoresist contains a first solubility modifier and a second solubility modifier. The photoresist is sensitive to the first solubility modifier and the second solubility modifier. The embossed pattern is formed by activating the first solubility modifier by using a pattern of photochemical radiation and developing the first layer of photoresist. A polymer mixture is deposited on these relief structures, the polymer mixture filling the openings defined by the relief pattern and covering the relief structures, the area above the top surface of the relief structures being a capping layer area, the polymer mixture comprising a first polymer and a second polymer, the polymer mixture being configured to self-separate relative to gravity such that a first film and a second film are formed from the polymer mixture, the first film comprising the first polymer being formed below the second film comprising the second polymer, the formation of the first film and the second film such that the second film fills the capping layer area, the first film being sensitive to the second solubility modifier and having a sensitivity threshold less than the sensitivity threshold of the photoresist, the second film being soluble in a first developer; The second solubility modifier is activated and diffused from these relief structures to the first film by a predetermined diffusion length. The second solubility modifier is sufficiently activated to reach the sensitivity threshold of the first film but not the sensitivity threshold of the photoresist. The diffusion region formed in the first film becomes soluble in the first developer while the photoresist remains insoluble in the first developer. The substrate is developed to remove the soluble diffusion regions of the second film and the first film.
2. The method as described in claim 1, wherein, The polymer mixture was deposited via spin coating deposition.
3. The method as described in claim 1, wherein, The polymer mixture segregates on its own after being deposited on the substrate.
4. The method of claim 3, wherein, The second membrane extends below the top surface of these relief structures after self-separation.
5. The method of claim 3, wherein, The polymer mixture segregates upon heating, and the method further includes performing a heat bake after depositing the polymer mixture onto these relief structures.
6. The method of claim 1, wherein, Developing the substrate further includes developing the substrate with the first developer to remove the soluble diffusion regions of the second film and the first film.
7. The method of claim 1, wherein, The second film is soluble in the second developer, and Developing the substrate further includes developing the substrate with the second developer to remove the second film before developing the substrate with the first developer to remove the soluble diffusion region of the first film.
8. The method of claim 7, wherein, The second film is removed after the second solubility modifier is activated.
9. The method of claim 7, wherein, The second film is removed before activating the second solubility modifier.
10. The method of claim 1, wherein, The materials of the second polymer include HFIP-M, MA-MIB-HFA, MA-BTHB-OH, MA-3,5-HFA-CHOH, MA-BTHB-NB, MA-EATf, and MA-DM-EATf.
11. A method for patterning a substrate, the method comprising: An embossed pattern comprising an embossed structure is formed on a substrate by a first layer of photoresist on the substrate. The first layer of photoresist contains a first solubility modifier and a second solubility modifier. The photoresist is sensitive to the first solubility modifier and the second solubility modifier. The embossed pattern is formed by activating the first solubility modifier by using a pattern of photochemical radiation and developing the first layer of photoresist. A resin coating is deposited on these relief structures, the resin coating filling the openings defined by the relief pattern and covering these relief structures, the area above the top surface of these relief structures being the cover layer area, the resin coating having a resin mixture comprising a first resin and a second resin, the resin coating being configured to self-separate relative to gravity such that a first film and a second film are formed from the resin coating, the first film comprising the first resin being formed below the second film comprising the second resin, the formation of the first film and the second film such that the second film fills the cover layer area, the first film being sensitive to the second solubility modifier and having a sensitivity threshold less than the sensitivity threshold of the photoresist, the second film being soluble in a first developer; The second solubility modifier is activated and diffused from these relief structures to the first film by a predetermined diffusion length. The second solubility modifier is sufficiently activated to reach the sensitivity threshold of the first film but not the sensitivity threshold of the photoresist. The diffusion region formed in the first film becomes soluble in the first developer while the photoresist remains insoluble in the first developer. The substrate is developed to remove the soluble diffusion regions of the second film and the first film.
12. The method of claim 11, wherein, The resin coating is deposited via spin coating deposition.
13. The method of claim 11, wherein, The resin coating segregates on itself after being deposited on the substrate.
14. The method of claim 13, wherein, The second membrane extends below the top surface of these relief structures after self-separation.
15. The method of claim 13, wherein, The resin coating segregates upon heating, and the method further includes performing a heat-baking process after depositing the resin coating onto these relief structures.
16. The method of claim 11, wherein, Developing the substrate further includes developing the substrate with the first developer to remove the soluble diffusion regions of the second film and the first film.
17. The method of claim 11, wherein, The second film is soluble in the second developer, and Developing the substrate further includes developing the substrate with the second developer to remove the second film before developing the substrate with the first developer to remove the soluble diffusion region of the first film.
18. The method of claim 17, wherein, The second film is removed after the second solubility modifier is activated.
19. The method of claim 17, wherein, The second film is removed before activating the second solubility modifier.
20. A method for patterning a substrate, the method comprising: A substrate having a defined opening to be partially filled is received; A polymer mixture is deposited on the substrate, the polymer mixture filling and covering the openings defined by these features, the region above the top surface of these features being a capping layer region, the polymer mixture comprising a first polymer and a second polymer, the polymer mixture being configured to self-separate relative to gravity such that a first film and a second film are formed from the polymer mixture, the first film comprising the first polymer being formed below the second film comprising the second polymer, the first film and the second film being formed such that the first film partially fills the defined openings while the second film fills the remaining portion of the defined openings and fills the capping layer region; as well as The substrate is developed using a first solvent to remove the second film, which remains within the defined openings. The second membrane is sensitive to the first solvent, while the first membrane is insoluble in the first solvent.
Citation Information
Patent Citations
Methods of forming a masking pattern for integrated circuits
US20100130016A1
Photoresist composition and method of forming photoresist pattern
US20200105522A1