A kind of ilisimol microneedle and preparation method thereof
By combining dopamine with copper ion coordination and polyvinylpyrrolidone, ilismolid microneedles were prepared, which solved the problems of poor water solubility and low bioavailability of ilismolimus, and achieved efficient drug encapsulation and copper ion loading. A stable and precise microneedle formulation for melanoma treatment is provided.
Patent Information
- Application Number
- CN202311746996.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-12-19
AI Technical Summary
Irislimus has poor water solubility, low bioavailability and poor selectivity, making it difficult to achieve targeted enrichment of tumor cells. The preparation process of existing nano preparations is complex and highly toxic, resulting in poor melanoma treatment effects.
The drug carrier is formed by the coordination of dopamine and copper ions, combined with polyvinylpyrrolidone, to prepare ilismo microneedles. It is prepared by using hyaluronic acid and polydimethylsiloxane microneedle templates to form a high and stable copper ion load. Good nanocage wrapping structure.
It improves the water solubility and stability of ilismolimus, achieves efficient drug encapsulation rate and copper ion loading, provides a microneedle preparation that can accurately act on melanoma, and reduces preparation complexity and toxicity.
Smart Images

Figure CN117598970B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of pharmaceutical preparations, and specifically relates to an ilisimol microneedle and a preparation method thereof. Background Art
[0002] Melanoma is a malignant tumor originating from melanocytes of the skin, mucous membranes and pigment membranes. Although the incidence of melanoma is lower than the other two main manifestations of skin cancer, namely basal cell carcinoma and squamous cell carcinoma, it is also known as the "king of cancer" because of its high malignancy, rapid progression, dangerous condition, extremely poor prognosis, easy lymphatic and hematogenous metastasis, and easy metastasis to organs such as the lungs and brain. Therefore, the mortality rate of patients is high. According to statistics, only 4% of skin cancer patients suffer from melanoma, but 80% of patients who die from skin cancer are melanoma patients, making it the first fatal disease of skin cancer. At present, surgical resection is the main treatment for melanoma, but it also has shortcomings such as large skin defects, long recovery time and high recurrence rate. In addition, chemotherapy and radiotherapy are one of the most classic anti-tumor treatments, but due to the poor response duration and survival ability of patients, and the resistance of melanoma to chemotherapy drugs and radiation, it usually leads to unsatisfactory efficacy in the treatment of melanoma. Therefore, there is an urgent need to find safe and effective melanoma treatments.
[0003] Copper death is a new form of regulated cell death, and its mechanism of occurrence is significantly different from the known forms of cell death such as apoptosis, pyroptosis, necroptosis and ferroptosis. It is a copper-dependent cell death driven by mitochondrial stress and damage. Excessive copper ions trigger metabolic disorders in the tricarboxylic acid cycle pathway, leading to abnormal protein lipoylation levels and loss of iron-sulfur cluster proteins, which leads to protein toxic stress response and ultimately cell death. This non-apoptotic cell death method has become a very promising treatment method in the treatment of melanoma.
[0004] Copper death depends largely on copper ion carriers. To date, many copper ion carriers have been developed, including disulfiram, 8-hydroxyquinoline, hydroxypyrithione and elesclomol (ES). Among these copper ion carriers, elesclomol differs from other ion carriers in that it selectively transports copper ions to the mitochondria of cells, resulting in the continuous accumulation of copper Cu in the mitochondria. Therefore, ES has become an anticancer drug and has entered clinical research. However, clinical studies have shown that ES has high safety but poor efficacy. The possible reasons are as follows: On the one hand, ES is a fat-soluble drug, which is easily cleared and metabolized after oral administration and is difficult to effectively enrich at the tumor site. CN116327888 discloses a composition of elesclomol that can improve the solubility of ES, with albumin as a carrier, including glutathione, manganese dioxide and ES, but this process is complicated and requires the addition of inorganic material manganese dioxide, which increases the toxicity of the preparation. On the other hand, it is quite difficult to transport more copper to cancer cells in tumor tissues. Although ES can carry copper ions, its carrying capacity is limited, and the copper ions that enter tumor cells are extremely limited. Tang et al. (ACS Nano, 2023.17.11, 10206-10217) reported a biomimetic system (PTC) of platelet membrane-coated cuprous oxide nanoparticles (Cu2O) / photosensitizer TBP-2 for copper death-mediated tumor inhibition. However, the preparation conditions are complicated, and the quality of the platelet membrane cannot be uniform and stable.
[0005] Therefore, in the prior art, ilisimol has poor water solubility, low bioavailability, poor selectivity, and is difficult to achieve targeted enrichment of tumor cells; in addition, ilisimol has a low copper ion load and cannot trigger copper death of tumor cells. These are urgent problems to be solved in the field of melanoma treatment. Although the existing nanoformulations have improved their solubility to a certain extent, the preparation process is complicated and some inorganic materials need to be added, resulting in increased toxicity of the preparations and increased medication risks. In addition, these nanomaterials have a variety of adverse reactions after intravenous injection. Summary of the invention
[0006] In view of the shortcomings of the prior art, the inventors provide an ilisimomol microneedle and a preparation method thereof. The coordination effect of dopamine and copper ions is used to form a drug carrier, and this structure is used to carry ilisimomol to prepare microneedles. Ordinary dopamine nanostructures have poor stability and are not suitable for the long preparation cycle of microneedles; incorporating polyvinyl pyrrolidone (PVP) into dopamine nanocarriers can improve this situation and form a new type of microneedle with simple ingredients and high copper ion loading.
[0007] The present invention specifically provides an ilisimomol microneedle, wherein the needle tip of the microneedle is hyaluronic acid mixed with ilisimomol nanoparticles, the microneedle substrate is polyvinyl pyrrolidone, the ilisimomol nanoparticles are ilisimomol loaded with copper ions and then encapsulated by nanocages formed by dopamine-copper-polyvinyl pyrrolidone, and the dopamine-copper is a nanostructure formed by the coordination of the two.
[0008] The average molecular weight of the hyaluronic acid is 100000-200000 Mw, and the average molecular weight of the polyvinyl pyrrolidone is 10000 Mw.
[0009] In the ilisimol nanoparticles, ilisimol is loaded with copper ions using the following preparation method: ilisimol is dissolved in dimethyl sulfoxide DMSO, the mass volume ratio of ilisimol to DMSO is 1:100-200 mg / μL, copper chloride CuCl2 is added, the mass ratio of ilisimol to copper chloride is ilisimol: copper chloride = 1:1 in mg / mg, and the mixture is stirred at room temperature for 30 minutes to obtain an ilisimol-copper conjugate.
[0010] The preparation method of the ilisimomol nanoparticles is as follows: copper chloride, dopamine hydrochloride and polyvinyl pyrrolidone are weighed, and deionized water is added to dissolve, the mixture is stirred and reacted for 1 hour, a Tris solution with a pH of 8.5 is added, and the DMSO solution of the above-mentioned ilisimomol-copper conjugate is quickly added, the mass ratio of the ilisimomol-copper conjugate to dopamine hydrochloride is ilisimomol-copper conjugate: dopamine hydrochloride = 1:20, the mass ratio of dopamine hydrochloride, copper chloride and polyvinyl pyrrolidone is dopamine hydrochloride: copper chloride: polyvinyl pyrrolidone = 5:1:50, the mass / volume ratio of dopamine hydrochloride and Tirs buffer solution is 1:0.5 mg / ml, the reaction solution is stirred and reacted for 12-72 hours, filtered with a 0.45-micron microporous filter membrane, and the filtrate is purified by ultrafiltration centrifugation to obtain the ilisimomol nanoparticle preparation.
[0011] The microneedle is prepared by the following method: a polydimethylsiloxane (PDMS) microneedle template is used to prepare the microneedle, hyaluronic acid is dispersed in an aqueous solution of ilisimol nanoparticles, the concentration of hyaluronic acid is 140 mg / mL, the aqueous solution is added to the PDMS microneedle template, centrifuged to prepare the microneedle tip, and then polyvinyl pyrrolidone is added to the mold as a microneedle support array. After drying the water, the ilisimol microneedle is obtained.
[0012] Preferably, the microneedle is prepared by the following method: using a polydimethylsiloxane PDMS microneedle template to prepare the microneedle, dispersing hyaluronic acid in an aqueous solution of ilisimomol nanoparticles, the concentration of hyaluronic acid is 140 mg / mL, the concentration of ilisimomol nanoparticles is 0.5 mg / mL, adding the aqueous solution to the PDMS microneedle template, centrifuging at 3000 rpm for 5 minutes to prepare the microneedle tip, and then adding a polyvinyl pyrrolidone (PVP) aqueous solution to the mold as a microneedle support array, the concentration of PVP is 1.5 g / ml, and the average molecular weight is 10000 Mw. After drying the water, the ilisimomol microneedle is obtained.
[0013] Compared with the prior art, the present invention has the following advantages:
[0014] (1) An ilisimol nanoformulation for preparing microneedles was prepared, and the water solubility of ilisimol was improved;
[0015] (2) A method for preparing nanoformulation of ilisimol is provided, which has uniform and stable particle size and high drug encapsulation efficiency;
[0016] (3) The stability and copper ion loading capacity of ilisimol nanoformulation were improved;
[0017] (4) Provided is an ilisimol microneedle that can precisely target melanoma. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 : Scanning electron microscope image of the microneedle of Example 1
[0019] Figure 2 : SEM image of the microneedle of Comparative Example 10
[0020] Figure 3 : Transmission electron microscope image of the nano solution of Example 1
[0021] Figure 4 : Particle size distribution diagram of the nano solution of Example 1
[0022] Figure 5 : Curve diagram of polydispersity index of nano-solutions of Example 1 and Comparative Example 1 versus placement time
[0023] Figure 6 : Curve diagram of the particle size of the nano solution of Example 1 and Comparative Example 1 versus the placement time DETAILED DESCRIPTION
[0024] The present invention is further described below by way of examples. It should be correctly understood that the examples of the present invention are provided only for illustrating the present invention, rather than limiting the present invention, and therefore, simple modifications of the present invention under the premise of the method of the present invention are within the scope of protection claimed by the present invention.
[0025] Example 1
[0026] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 100 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0027] (2) Weigh 40 mg of dopamine hydrochloride, 8 mg of copper chloride, and 400 mg of polyvinyl pyrrolidone, add 40 ml of deionized water to dissolve, and stir to react for 1 hour;
[0028] (3) Add 20 ml of Tris solution with pH = 8.5 to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times;
[0029] (4) diluting the above nano-solution with water to 0.5 mg / ml, adding hyaluronic acid to a hyaluronic acid concentration of 140 mg / ml, and an average molecular weight of hyaluronic acid of 100,000-200,000 Mw, slowly stirring until completely dissolved, adding to a microneedle mold of polydimethylsiloxane (PDMS), centrifuging at 3,000 rpm for 5 min, and letting stand for 24 hours to evaporate the water;
[0030] (5) Adding polyvinyl pyrrolidone aqueous solution into the mold as a microneedle support array, the concentration of PVP is 1.5 g / ml, and the average molecular weight is 10,000 Mw. After standing for 48 hours and drying the water, the ilisimol microneedles are obtained.
[0031] Example 2
[0032] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 200 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0033] (2) Weigh 40 mg of dopamine hydrochloride, 8 mg of copper chloride, and 400 mg of polyvinyl pyrrolidone, add 40 ml of deionized water to dissolve, and stir to react for 1 hour;
[0034] (3) Add 20 ml of Tris solution with pH = 8.5 to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 48 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times;
[0035] (4) diluting the above nano-solution with water to 0.5 mg / ml, adding hyaluronic acid to a hyaluronic acid concentration of 140 mg / ml, and an average molecular weight of hyaluronic acid of 100,000-200,000 Mw, slowly stirring until completely dissolved, adding to a microneedle mold of polydimethylsiloxane (PDMS), centrifuging at 3,000 rpm for 5 min, and letting stand for 24 hours to evaporate the water;
[0036] (5) Adding polyvinyl pyrrolidone aqueous solution into the mold as a microneedle support array, the concentration of PVP is 1.5 g / ml, and the average molecular weight is 10,000 Mw. After standing for 48 hours and drying the water, the ilisimol microneedles are obtained.
[0037] Example 3
[0038] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 300 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0039] (2) Weigh 40 mg of dopamine hydrochloride, 8 mg of copper chloride, and 400 mg of polyvinyl pyrrolidone, add 40 ml of deionized water to dissolve, and stir to react for 1 hour;
[0040] (3) Add 20 ml of Tris solution with pH = 8.5 to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 72 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times;
[0041] (4) diluting the above nano-solution with water to 0.5 mg / ml, adding hyaluronic acid to a hyaluronic acid concentration of 140 mg / ml, and an average molecular weight of hyaluronic acid of 100,000-200,000 Mw, slowly stirring until completely dissolved, adding to a microneedle mold of polydimethylsiloxane (PDMS), centrifuging at 3,000 rpm for 5 min, and letting stand for 24 hours to evaporate the water;
[0042] (5) Adding polyvinyl pyrrolidone aqueous solution into the mold as a microneedle support array, the concentration of PVP is 1.5 g / ml, and the average molecular weight is 10,000 Mw. After standing for 48 hours and drying the water, the ilisimol microneedles are obtained.
[0043] Example 4
[0044] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 100 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0045] (2) Weigh 30 mg of dopamine hydrochloride, 6 mg of copper chloride, and 300 mg of polyvinyl pyrrolidone, add 30 ml of deionized water to dissolve, and stir to react for 1 hour;
[0046] (3) Add 15 ml of Tris solution with pH = 8.5 to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times;
[0047] (4) diluting the above nano-solution with water to 0.5 mg / ml, adding hyaluronic acid to a hyaluronic acid concentration of 140 mg / ml, and an average molecular weight of hyaluronic acid of 100,000-200,000 Mw, slowly stirring until completely dissolved, adding to a microneedle mold of polydimethylsiloxane (PDMS), centrifuging at 3,000 rpm for 5 min, and letting stand for 24 hours to evaporate the water;
[0048] (5) Adding polyvinyl pyrrolidone aqueous solution into the mold as a microneedle support array, the concentration of PVP is 1.5 g / ml, and the average molecular weight is 10,000 Mw. After standing for 48 hours and drying the water, the ilisimol microneedles are obtained.
[0049] Example 5
[0050] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 100 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0051] (2) Weigh 25 mg of dopamine hydrochloride, 5 mg of copper chloride, and 250 mg of polyvinyl pyrrolidone, add 25 ml of deionized water to dissolve, and stir to react for 1 hour;
[0052] (3) Add 12.5 ml of Tris solution with pH = 8.5 to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times;
[0053] (4) diluting the above nano-solution with water to 0.5 mg / ml, adding hyaluronic acid to a hyaluronic acid concentration of 140 mg / ml, and an average molecular weight of hyaluronic acid of 100,000-200,000 Mw, slowly stirring until completely dissolved, adding to a microneedle mold of polydimethylsiloxane (PDMS), centrifuging at 3,000 rpm for 5 min, and letting stand for 24 hours to evaporate the water;
[0054] (5) Adding polyvinyl pyrrolidone aqueous solution into the mold as a microneedle support array, the concentration of PVP is 1.5 g / ml, and the average molecular weight is 10,000 Mw. After standing for 48 hours and drying the water, the ilisimol microneedles are obtained.
[0055] Example 6
[0056] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 100 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0057] (2) Weigh 30 mg of dopamine hydrochloride, 6 mg of copper chloride, and 300 mg of polyvinyl pyrrolidone, add 30 ml of deionized water to dissolve, and stir to react for 1 hour;
[0058] (3) Add 15 ml of Tris solution (pH = 8.5) to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times.
[0059] Comparative Example 1
[0060] (1) Dissolve 10 mg of ilisimol and 1 mg of copper chloride in 100 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of ilisimol-copper conjugate;
[0061] (2) Weigh 30 mg of dopamine hydrochloride and 6 mg of copper chloride, add 30 ml of deionized water to dissolve, and stir to react for 1 hour;
[0062] (3) Add 15 ml of Tris solution (pH = 8.5) to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times.
[0063] (4) diluting the above solution with water to 0.5 mg / ml, adding hyaluronic acid to a hyaluronic acid concentration of 140 mg / ml, with an average molecular weight of 100,000-200,000 Mw, slowly stirring until completely dissolved, adding to a polydimethylsiloxane (PDMS) microneedle mold, centrifuging at 3,000 rpm for 5 min, and letting stand for 24 hours to evaporate the water;
[0064] (5) Adding polyvinyl pyrrolidone aqueous solution into the mold as a microneedle support array, the concentration of PVP is 1.5 g / ml, and the average molecular weight is 10,000 Mw. After standing for 48 hours and drying the water, the ilisimol microneedles are obtained.
[0065] Comparative Example 2
[0066] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 500 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0067] (2) Weigh 30 mg of dopamine hydrochloride, 6 mg of copper chloride, and 300 mg of polyvinyl pyrrolidone, add 15 ml of deionized water to dissolve, and stir to react for 1 hour;
[0068] (3) Add 15 ml of Tris solution (pH = 8.5) to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times.
[0069] (4) diluting the above solution with water to 0.5 mg / ml, adding hyaluronic acid to a hyaluronic acid concentration of 140 mg / ml and an average molecular weight of hyaluronic acid of 10000 Mw, slowly stirring until completely dissolved, adding to a polydimethylsiloxane (PDMS) microneedle mold, centrifuging at 3000 rpm for 5 min, and letting stand for 24 hours to evaporate the water;
[0070] (5) Adding polyvinyl pyrrolidone aqueous solution into the mold as a microneedle support array, the concentration of PVP is 1.5 g / ml, and the average molecular weight is 10,000 Mw. After standing for 48 hours and drying the water, the ilisimol microneedles are obtained.
[0071] Comparative Example 3
[0072] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 100 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0073] (2) Weigh 100 mg of dopamine hydrochloride, 6 mg of copper chloride, and 100 mg of polyvinyl pyrrolidone, add 30 ml of deionized water to dissolve, and stir to react for 1 hour;
[0074] (3) Add 15 ml of Tris solution (pH = 8.5) to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the above-mentioned DMSO solution of ilisimol-copper conjugate, stir the reaction solution for 3 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times.
[0075] Comparative Example 4
[0076] (1) 1 mg of 8-hydroxyquinoline and 1 mg of copper chloride were dissolved in 100 μL of DMSO, respectively. The two were mixed and vortexed at room temperature for 30 minutes to form a DMSO solution of ilisimol-copper conjugate;
[0077] (2) Weigh 30 mg of dopamine hydrochloride, 6 mg of copper chloride, 300 mg of polyvinyl pyrrolidone, and add 30 ml of deionized water.
[0078] Dissolve, stir and react for 1 hour;
[0079] (3) Add 15 ml of Tris solution (pH = 8.5) to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the above-mentioned DMSO solution of 8-hydroxyquinoline-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times.
[0080] Comparative Example 5
[0081] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 100 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0082] (2) Weigh 30 mg of tannic acid, 6 mg of copper chloride, and 300 mg of polyvinyl pyrrolidone, add 30 ml of deionized water to dissolve, and stir to react for 1 hour;
[0083] (3) Add 15 ml of Tris solution with pH = 8.5 to the aqueous solution of tannic acid and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times.
[0084] Comparative Example 6
[0085] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 100 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0086] (2) Weigh 25 mg of dopamine hydrochloride, 5 mg of ferric chloride hexahydrate, and 250 mg of polyvinyl pyrrolidone, add 25 ml of deionized water to dissolve, and stir to react for 1 hour;
[0087] (3) Add 12.5 ml of Tris solution (pH = 8.5) to the aqueous solution of dopamine hydrochloride and ferric chloride hexahydrate; quickly add the above-mentioned DMSO solution of ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times.
[0088] Comparative Example 7
[0089] (1) 1 mg of ilisimol and 1 mg of copper chloride were dissolved in 200 μL of methanol respectively, and the two were mixed and vortexed at room temperature for 30 minutes to form a methanol solution of ilisimol-copper conjugate;
[0090] (2) Weigh 30 mg of dopamine hydrochloride, 6 mg of copper chloride, and 300 mg of polyvinyl pyrrolidone, add 30 ml of deionized water to dissolve, and stir to react for 1 hour;
[0091] (3) Add 15 ml of Tris solution with pH = 8.5 to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the above-mentioned methanol solution of ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times.
[0092] Comparative Example 8
[0093] (1) Dissolve 10 mg of ilisimol and 1 mg of copper chloride in 100 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of ilisimol-copper conjugate;
[0094] (2) Weigh 30 mg of dopamine hydrochloride, 6 mg of copper chloride, and 300 mg of polyvinyl pyrrolidone, add 30 ml of deionized water to dissolve, and stir to react for 1 hour;
[0095] (3) Add 15 ml of Tris solution (pH = 8.5) to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times.
[0096] Comparative Example 9
[0097] (1) Dissolve 1 mg of elisemol and 1 mg of copper chloride in 100 μL of DMSO, respectively. Mix the two and vortex at room temperature for 30 minutes to form a DMSO solution of elisemol-copper conjugate.
[0098] (2) Weigh 40 mg of dopamine hydrochloride, 8 mg of copper chloride, and 400 mg of polyvinyl pyrrolidone, add 40 ml of deionized water to dissolve, and stir to react for 1 hour;
[0099] (3) Add 20 ml of Tris solution with pH = 8.5 to the aqueous solution of dopamine hydrochloride and copper chloride; quickly add the DMSO solution of the above-mentioned ilisimol-copper conjugate, stir the reaction solution for 12 hours, filter it with a 0.45 μm microporous filter membrane, centrifuge the filtrate at 4000 rpm using an ultrafiltration centrifuge tube, and purify and wash it 3 times;
[0100] (4) Dilute the above nano solution with water to 0.5 mg / ml, add polyvinyl pyrrolidone to a PVP concentration of 140 mg / ml, slowly stir until completely dissolved, add to the polydimethylsiloxane PDMS microneedle mold, centrifuge at 3000 rpm for 5 min, and let stand for 24 hours to evaporate the water;
[0101] (5) Adding polyvinyl pyrrolidone aqueous solution into the mold as a microneedle support array, the concentration of PVP is 1.5 g / ml, and the average molecular weight is 10,000 Mw. After standing for 48 hours and drying the water, the ilisimol microneedles are obtained.
[0102] Comparative Example 10
[0103] (1) Prepare hyaluronic acid at a concentration of 140 mg / ml and an average molecular weight of 100,000-200,000 Mw. Slowly stir until completely dissolved, add to the microneedle mold of polydimethylsiloxane (PDMS), centrifuge at 3,000 rpm for 5 min, and let stand for 24 hours to evaporate the water;
[0104] (2) Add polyvinyl pyrrolidone aqueous solution into the mold as a microneedle support array, the PVP concentration is 1.5 g / ml, and the average molecular weight is 10,000 Mw. Let it stand for 48 hours and dry the water to obtain the unloaded microneedles.
[0105] Verification Example
[0106] 1. The appearance of the microneedles of Example 1 and Comparative Example 10 was observed using a scanning electron microscope.
[0107] Comparative Example 10 Results Figure 2 As shown, only hyaluronic acid is used directly as the microneedle needle material. Due to its high transparency, the microneedle color is darker. Figure 1After the ilisimonate nano-solution was added to the microneedle tip of Example 1, the morphology changed significantly.
[0108] 2. The nano-solution obtained in Example 1 was negatively stained with phosphotungstic acid and the morphology was observed using a transmission electron microscope.
[0109] The results are as follows Figure 4 The particle size of the ilisimol nanoformulation prepared in the embodiment of the present invention is relatively uniform.
[0110] 3. The nano solutions obtained in Examples 1-6 and Comparative Examples 1-9 were filtered through a 0.45 μm microporous filter membrane, and the particle size and polydispersity index of the obtained liquid were monitored using a laser particle size analyzer.
[0111] Table 1. Particle size and polydispersity index of the nanosolutions of various examples
[0112]
[0113] The results are as follows Figure 3 As shown, the nanoparticle preparation prepared by the present invention has a uniform particle size distribution, a particle size of less than 200 nm, and a polydispersity index of less than 0.2.
[0114] 4. The solutions obtained in Examples 1-6 and Comparative Examples 1-9 were filtered using a 0.45 μm microporous membrane. 200 μl of the obtained liquid was added with 800 μl of DMSO to break the emulsion, and the drug content was detected using an ultraviolet spectrophotometer to calculate the drug encapsulation efficiency.
[0115] Table 2. Encapsulation efficiency of various examples
[0116]
[0117] The results are shown in Table 2. Due to the supramolecular force between the drug and dopamine, the nanoformulation prepared by the present invention can easily encapsulate the drug, and the encapsulation rate is relatively high, about 90%.
[0118] 5. Cut some of the microneedles obtained in Examples 1-6 and Comparative Examples 1, 2, and 9, and use ICP-MS to detect the amount of copper ions in the needles. The total number of needles in the microneedle mold array is 15×15.
[0119] Table 3. Copper ion content of each example
[0120]
[0121] The results in Table 3 show that the nanoformulations obtained in Examples 1-6 of the present invention have high copper ion loading, which is greatly improved compared with the comparative examples. The nano solutions formed in Comparative Examples 1 and 2 are not uniform and have poor stability, resulting in poor microneedle quality and low copper ion loading. After the needle material of the microneedle is replaced in the comparative example, a good needle shape cannot be formed, resulting in low copper ion loading.
[0122] 6. The ilisimol nano solutions obtained in Examples 1-6 and Comparative Example 1 were placed at room temperature, and the particle size and polydispersity index were measured using a particle size distribution analyzer every day for 4 days.
[0123] The results are as follows Figure 4 and 5 As shown, the particle size of Example 1 of the present invention is stable as the storage time increases, and the polydispersity index is less than 0.2, maintaining a stable state. However, the particle size of the comparative example changes greatly as the storage time increases, and the polydispersity index increases, indicating that the stability of the nano solution particle size deteriorates after the lack of PVP in the prescription.
Claims
1. An ilisimol microneedle, characterized in that: The needle tip of the microneedle is hyaluronic acid mixed with ilisimomol nanoparticles, the microneedle substrate is polyvinyl pyrrolidone, the ilisimomol nanoparticles are ilisimomol loaded with copper ions and wrapped by nanocages formed by dopamine-copper ions-polyvinyl pyrrolidone, the dopamine-copper ions are nanostructures formed by coordination between the two, the average molecular weight of the hyaluronic acid is 100000-200000 Mw, and the average molecular weight of the polyvinyl pyrrolidone is 10000 Mw; In the ilisimol nanoparticles, the ilisimol-carrying copper ions are prepared by the following method: dissolving ilisimol in dimethyl sulfoxide (DMSO), the mass volume ratio of ilisimol to DMSO (mg / μL) being 1:100-200, adding copper chloride (CuCl2), the mass ratio of ilisimol to copper chloride (mg / mg) being ilisimol:copper chloride=1:1, stirring at room temperature for 30 minutes, and obtaining an ilisimol-copper conjugate; The preparation method of the ilisimomol nanoparticles is as follows: copper chloride, dopamine hydrochloride, and polyvinyl pyrrolidone are weighed, and deionized water is added to dissolve, coordinated stirring reaction is carried out for 1 hour, a Tris solution with a pH of 8.5 is added, and the DMSO solution of the above-mentioned ilisimomol-copper conjugate is quickly added, the mass ratio of the ilisimomol-copper conjugate to dopamine hydrochloride is ilisimomol-copper conjugate: dopamine hydrochloride = 1:20, the mass ratio of dopamine hydrochloride, copper chloride, and polyvinyl pyrrolidone is dopamine hydrochloride: copper chloride: polyvinyl pyrrolidone = 5:1:50, the mass / volume ratio of dopamine hydrochloride and Tirs buffer is 1:0.5 mg / ml, the reaction solution is stirred for reaction for 12-72 hours, filtered with a 0.45-micron microporous filter membrane, and the filtrate is purified by ultrafiltration centrifugation to obtain an ilisimomol nanoparticle preparation; The microneedle is prepared by the following method: a polydimethylsiloxane (PDMS) microneedle template is used to prepare the microneedle, hyaluronic acid is dispersed in an aqueous solution of an ilisimol nanoformulation, the concentration of hyaluronic acid is 140 mg / mL, the aqueous solution is added to the PDMS microneedle template, and the microneedle tip is prepared by centrifugation, and then polyvinyl pyrrolidone is added to the mold as a microneedle support array, and the ilisimol microneedle is obtained after drying the water.