A chip packaging method based on oxygen-free copper platinum thickening

By using oxygen-free copper-platinum thickening technology in chip packaging, the damage problem of copper wire connection to the chip is solved, the stability and service life of the chip are improved, and the process is simplified and costs are reduced.

CN117612947BActive Publication Date: 2024-11-15JIANGSU SOLID POWER SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311609843.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-27
Publication Date
2024-11-15
Estimated Expiration
2043-11-27

AI Technical Summary

Technical Problem

In the prior art, in high-power chip packaging, copper wire connection causes damage to the chip, and silver plating is high in cost, long process and low production efficiency.

Method used

Using the thickened chip packaging method of oxygen-free copper-platinum, high-temperature soldering sheets and oxygen-free copper-platinum are set on the surface of the chip pad, and vacuum flow welding technology is used to form a protective layer to prevent the copper wire connection from causing damage to the chip. .

Benefits of technology

It improves the stability and service life of the chip, simplifies the process, reduces production costs, improves production efficiency, and is suitable for various types of chip protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117612947B_ABST
    Figure CN117612947B_ABST
Patent Text Reader

Abstract

The present invention relates to a chip packaging method based on oxygen-free copper platinum thickening, comprising the following steps: plasma cleaning the chip; welding the chip on a DBC substrate to obtain a first welding assembly; placing a high-temperature welding sheet on the surface of the chip pad of the first welding assembly; placing oxygen-free copper platinum on the surface of the high-temperature welding sheet to obtain a second welding assembly, and welding the second welding assembly using a vacuum flow welding device; connecting the oxygen-free copper platinums that need to be connected on the second welding assembly using a first copper wire; connecting the oxygen-free copper platinum on the second welding assembly and the DBC substrate using a second copper wire; then encapsulating the surface of the DBC substrate with an insulating material, and completing the packaging after the insulating material is cured. By arranging oxygen-free copper platinum and a high-temperature welding sheet, the pad on the chip is thickened, which can protect the chip and prevent the copper wire connection from causing damage to the chip. The steps are simple, the process is short, and the production efficiency can be effectively improved and the production cost can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor packaging, in particular to a chip packaging method based on oxygen-free copper platinum thickening. Background Art

[0002] With the development of electronic technology, high-power chips have become the trend of industry development. In order to improve the capacity of power chips, high-power chips usually use copper wire bonding instead of aluminum wire bonding to avoid the large difference in the conductivity and thermal expansion coefficient (CTE) of aluminum wire bonding, which affects product reliability. When the wafer is manufactured, the protective layer on the surface of the chip is an aluminum layer, which is usually several μm thick. Directly using copper wires to connect will damage the chip.

[0003] In the prior art, a protective layer with a thickness of tens of μm is specially added to the surface of the chip by silver plating, thereby preventing the copper wire connection from damaging the chip. However, this treatment method is costly, has a long process, and has low production efficiency. Summary of the invention

[0004] In view of the shortcomings in the above-mentioned existing production technology, the applicant provides a chip packaging method based on oxygen-free copper platinum thickening with a reasonable structure. By setting oxygen-free copper platinum and high-temperature solder sheets, the solder pads on the chip are thickened, which can protect the chip and prevent the copper wire connection from causing damage to the chip. The method has simple steps and a short process, which can effectively improve production efficiency and reduce production costs.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A chip packaging method based on oxygen-free copper platinum thickening includes the following steps:

[0007] S1. Plasma cleaning of the chip;

[0008] S2. Soldering the chip to the DBC substrate to obtain a first welding assembly;

[0009] S3. Place a high temperature solder sheet on the chip pad surface of the first welding assembly;

[0010] S4. Place oxygen-free copper platinum on the surface of the medium and high temperature welding sheet in S3 to obtain a second welding assembly, and weld the second welding assembly using a vacuum flow welding device;

[0011] The bottom of the oxygen-free copper platinum is evenly provided with a plurality of bumps, and the oxygen-free copper platinum is used to thicken the pad on the chip;

[0012] S5. The oxygen-free copper platinum to be connected on the second welding assembly is connected using a first copper wire;

[0013] The oxygen-free copper platinum on the second welding assembly and the DBC substrate are connected by a second copper wire;

[0014] S6. Then, an insulating material is poured on the surface of the DBC substrate so that the insulating material covers the first welding component. After the insulating material is solidified, the packaging is completed.

[0015] As a further improvement of the above technical solution:

[0016] In S1., the plasma cleaning time is 2 h.

[0017] In S3., the thickness of the high temperature solder sheet is 0.1 mm.

[0018] The shapes of the high temperature solder sheet and oxygen-free copper platinum are consistent with the shapes of the corresponding solder pads on the chip.

[0019] In S4., the thickness of the oxygen-free copper platinum is 0.1 mm.

[0020] In S4., the welding temperature is 240°C-260°C.

[0021] In S5., the first copper wire and the second copper wire are both fixed by ultrasonic welding equipment.

[0022] In S6., the insulating material is silicone material.

[0023] In S6., the thickness of the insulating material is 3 mm.

[0024] The beneficial effects of the present invention are as follows:

[0025] The present invention has a compact and reasonable structure and is easy to operate. By arranging oxygen-free copper platinum, the pad on the chip is thickened, which can improve the stability and service life of the chip, thereby effectively improving the reliability of chip welding and improving the chip welding quality in the subsequent chip welding process.

[0026] The oxygen-free copper platinum in the present invention has the characteristics of low stress and high welding reliability. It is connected to the chip pad surface through a high-temperature solder sheet to protect the chip electrode. It can solve the poor reliability problem of traditional silver-plated chips under high current and high pressing conditions, and improve the stability and service life of the chip.

[0027] In the present invention, by setting steps S2. and S3., the chip surface pad can be thickened, the process is short, and it has a wide application prospect. It can be applied to various types of chip protection and improve the stability and service life of the chip.

[0028] In the present invention, oxygen-free copper platinum is provided so that the chip is capable of being connected using copper wires. The copper wire connection can effectively improve the chip capacity and make the chip applicable to high-power working conditions. Moreover, the copper wire diameter and the type of insulating material parameters can be adjusted according to actual needs to meet the needs of different fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a flow chart of the present invention.

[0030] Figure 2 This is a top view of placing oxygen-free copper platinum on a chip in the present invention.

[0031] Figure 3 This is a front view of placing oxygen-free copper platinum on a chip in the present invention.

[0032] Figure 4 This is a front view of the second welding assembly after copper wire connection in the present invention.

[0033] Among them: 1. Chip; 2. High-temperature solder sheet; 3. Oxygen-free copper platinum; 4. First copper wire; 5. Second copper wire; 6. DBC substrate. DETAILED DESCRIPTION

[0034] The specific implementation of the present invention will be described below in conjunction with the accompanying drawings.

[0035] like Figure 1 As shown, the chip packaging method based on oxygen-free copper platinum thickening of this embodiment includes the following steps:

[0036] S1. Plasma cleaning of chip 1;

[0037] S1.1. Plasma cleaning time is 2h;

[0038] S2. Soldering the chip 1 to the DBC substrate 6 to obtain a first welding assembly;

[0039] S3. Place a high temperature solder sheet 2 on the surface of the chip 1 pad of the first soldering assembly;

[0040] S3.1. The thickness of the high temperature solder sheet 2 is 0.1 mm;

[0041] S4. Figure 2-Figure 3 As shown, oxygen-free copper platinum 3 is placed on the surface of the medium-high temperature welding sheet 2 in S3 to obtain a second welding assembly, and the second welding assembly is welded using a vacuum flow welding device;

[0042] A plurality of bumps are evenly arranged at the bottom of the oxygen-free copper platinum 3, and the oxygen-free copper platinum 3 is used to thicken the pad on the chip 1;

[0043] S4.1. The shapes of the high temperature solder pad 2 and the oxygen-free copper platinum 3 are consistent with the shapes of the corresponding solder pads on the chip 1;

[0044] S4.2. The thickness of oxygen-free copper platinum 3 is 0.1 mm;

[0045] S4.3. The welding temperature is 240℃-260℃;

[0046] S4.4. The protrusions at the bottom of the oxygen-free copper platinum 3 are evenly arranged on the edges around it. In this embodiment, four protrusions are arranged;

[0047] By setting the bumps, the oxygen-free copper platinum 3 can be supported, so that after the second component is welded, the bottom end surface of the oxygen-free copper platinum 3 can be better attached to the top pad of the chip 1 through the high-temperature welding sheet 2, and the gap between the oxygen-free copper platinum 3 and the chip 1 due to the uneven surface of the oxygen-free copper platinum 3 can be prevented, which can effectively improve the connection reliability and improve the performance of the chip 1;

[0048] S5. Figure 4 As shown, the oxygen-free copper platinum 3 to be connected on the second welding assembly is connected by a first copper wire 4;

[0049] The oxygen-free copper platinum 3 on the second welding assembly and the DBC substrate 6 are connected by a second copper wire 5;

[0050] S5.1. The first copper wire 4 and the second copper wire 5 are fixed by ultrasonic welding equipment;

[0051] S6. Then, an insulating material is poured on the surface of the DBC substrate 6 so that the insulating material covers the first welding assembly. After the insulating material is solidified, the packaging is completed.

[0052] S6.1. The insulating material is silicone material, which has the advantages of high temperature resistance and corrosion resistance, and can improve the working reliability of the chip after packaging;

[0053] S6.2. The thickness of the insulating material is 3 mm.

[0054] In the present invention, a high-temperature solder sheet 2, an oxygen-free copper platinum 3 and an encapsulating insulating material are provided to form a protective layer on the surface of the chip 1, which can improve the working reliability and service life of the chip, and has a short process, low production cost and high production efficiency. At the same time, the circuit connection inside the chip 1 is realized through copper wire bonding technology, and silicone material is used as an insulating material, which can improve the working stability of the circuit.

[0055] The above description is an explanation of the present invention, not a limitation of the present invention. The scope of the present invention is defined in the claims. Any form of modification may be made within the scope of protection of the present invention.

Claims

1. A chip packaging method based on oxygen-free copper platinum thickening, characterized in that: The following steps are involved: S1. Plasma cleaning the chip (1); S2. Soldering the chip (1) to the DBC substrate (6) to obtain a first soldering assembly; S3. Place a high-temperature solder sheet (2) on the surface of the solder pad of the chip (1) of the first soldering assembly; S4. placing oxygen-free copper platinum (3) on the surface of the medium-high temperature welding sheet (2) in S3 to obtain a second welding assembly, and welding the second welding assembly using a vacuum flow welding device; The bottom of the oxygen-free copper platinum (3) is evenly provided with a plurality of bumps, and the oxygen-free copper platinum (3) is used to thicken the pad on the chip (1); The shapes of the high-temperature solder sheet (2) and the oxygen-free copper platinum (3) are consistent with the shapes of the corresponding solder pads on the chip (1); The thickness of the oxygen-free copper platinum (3) is 0.1 mm; The welding temperature is 240° C.-260° C.; S5. The oxygen-free copper platinum (3) to be connected on the second welding assembly is connected using the first copper wire (4); The oxygen-free copper platinum (3) and the DBC substrate (6) on the second welding assembly are connected by a second copper wire (5); S6. Then, an insulating material is poured onto the surface of the DBC substrate (6) so that the insulating material covers the first welding assembly. After the insulating material is solidified, the packaging is completed.

2. A chip packaging method based on oxygen-free copper platinum thickening as claimed in claim 1, characterized in that: In S1., the plasma cleaning time is 2 h.

3. A chip packaging method based on oxygen-free copper platinum thickening as claimed in claim 1, characterized in that: In S3., the thickness of the high temperature solder sheet (2) is 0.1 mm.

4. A chip packaging method based on oxygen-free copper platinum thickening as claimed in claim 1, characterized in that: In S5., the first copper wire (4) and the second copper wire (5) are both fixed by using ultrasonic welding equipment.

5. A chip packaging method based on oxygen-free copper platinum thickening as claimed in claim 1, characterized in that: In S6., the insulating material is silicone material.

6. A chip packaging method based on oxygen-free copper platinum thickening as claimed in claim 1, characterized in that: In S6., the thickness of the insulating material is 3 mm.