Methods to improve the rate performance of solid-state batteries
By applying insulating and conductive adhesive to the bottom of the solid-state battery core, the electronic pathways and thermal conductivity are enhanced, solving the problems of poor rate performance and heat accumulation in solid-state batteries, and achieving efficient battery performance improvement and production adaptation.
Patent Information
- Application Number
- CN202311582002.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-24
AI Technical Summary
Existing solid-state batteries have poor rate performance, and heat accumulation leads to reduced battery life. Current technologies increase the number of tabs or have complex and costly tab designs, making it difficult to balance conductivity, thermal conductivity, and production efficiency.
Insulating and conductive adhesives are applied to the bottom of the core, and the negative electrode extends beyond the separator to avoid short circuits, enhance electronic pathways and thermal conductivity, and adapt to existing production lines.
It improves the rate performance and thermal conductivity of the battery, extends battery life, reduces production costs, and is suitable for industrial production.
Smart Images

Figure CN117613413B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery technology, specifically relating to a method for improving the rate performance of solid-state batteries. Background Technology
[0002] Solid-state batteries are a crucial technological direction for addressing the safety and improving the energy density of lithium-ion batteries. However, solid-state battery technology is highly complex, and currently, most mainstream manufacturers are entering the solid-state battery field using semi-solid-state technologies. Solid-state batteries are still in the incubation stage from laboratory to industrialization, or from pilot-scale production to industrialization, and large-scale mass production is still a long way off. One significant factor hindering solid-state battery development is the significantly lower ionic conductivity of solid-state electrolytes compared to liquid electrolytes, resulting in a substantial increase in internal resistance. This leads to poorer rate performance and cycle life, negatively impacting battery development. Furthermore, solid-state batteries generate heat during discharge due to impedance. Heat conduction within the core occurs in two directions: one is gradual conduction to the outer layer of the core and then to the steel casing, and the other is direct conduction through the metal tabs to the bottom of the steel casing. The steel casing then dissipates the heat through heat conduction or convection with the external environment. Larger discharge currents generate more heat. However, due to slow heat conduction, heat accumulates inside the core. As the temperature rises, the impedance of the metal increases, creating a vicious cycle of heat generation – heat accumulation – increased impedance – more heat generation. Therefore, improving the rate performance of solid-state batteries is an important research direction.
[0003] Currently, the industry uses increasing the number of tabs to improve the conductivity and thermal conductivity of solid-state batteries. However, this can cause severe heat accumulation inside the cell. Increasing the number of tabs can lead to different stress levels between the areas with welded tabs and those without. As the solid-state battery undergoes charge and discharge cycles, the electrode sheets expand and contract. Areas with varying stress are prone to lithium plating, and may even experience electrode breakage, resulting in a decrease in battery capacity and ultimately a reduction in the charge and discharge cycle life of the solid-state battery.
[0004] Existing processes generally employ two technical solutions. Solution 1: Welding multiple tabs onto the positive and negative electrode sheets increases the conductivity and thermal conductivity of the core. This allows heat generated during high-rate discharge to be quickly conducted away through wider and thicker tabs, reducing heat accumulation within the core and achieving the goal of meeting high-rate charge / discharge performance and extending battery life. The disadvantage of Solution 1 is that, because increasing the number of tabs on the electrode sheets to enhance conductivity and thermal conductivity for high-rate performance increases the stress within the core, affecting current distribution, and requiring isolation treatment or no coating of positive electrode active material in the positive electrode area corresponding to the negative electrode tabs, it prevents lithium from leaching from the positive electrode and forming lithium dendrites at the negative electrode tabs. This not only reduces battery capacity but also significantly impacts battery life.
[0005] Option 2: Employing full-tab technology for both positive and negative electrodes. This involves leaving blank areas on the sides of the positive and negative electrodes uncoated, which are then directly used as tabs and welded to the busbar after being flattened or folded. The resulting battery has greater electron and heat conduction capabilities, essentially representing an unlimited increase in the number of tabs welded in Option 1. The disadvantages of Option 2 are: The need to leave blank areas on the sides of the electrodes during coating leads to low production efficiency. Furthermore, the different stretching of the coated and uncoated areas during electrode rolling presents a significant challenge for this technology. Additionally, the need to flatten or fold the reserved sides during winding before welding to the busbar is difficult, and the welding process is hard to control, easily leading to batch welding defects. Moreover, the need to reserve space for the protruding areas from the folded sides of the positive and negative electrodes, as well as space for the busbar, limits space utilization. Overall, this technical solution is technically challenging, has a low yield rate, and is limited in space utilization. It also requires significant changes and upgrades to existing solid-state battery production processes and equipment, resulting in substantial investment.
[0006] CN202223187545.7 discloses a high-power, high-energy-density cylindrical battery. By improving the structure of the cylindrical battery and optimizing the dimensions of the positive and negative tabs in specific locations, the width and thickness of the tabs located inside the core are set to be greater than those located on the outer periphery of the core. This facilitates the rapid conduction of heat from the inner layer of the core through the wider and thicker tabs, thereby reducing heat accumulation inside the core. Furthermore, reducing the size of the tabs on the outer layer of the core reduces the proportion of inactive material, thus increasing the energy density and conductivity of the cylindrical battery. However, this process requires the introduction of more tabs or design of the size and layout of the introduced tabs, making the process relatively complex. Although the conductivity is improved, it remains relatively low, and the improvement in battery temperature rise is not significant. Summary of the Invention
[0007] To address the problems of existing technologies, this invention provides a method for improving the rate performance of batteries by coating the bottom of the battery core with conductive adhesive without altering the original solid-state battery manufacturing process. This method also considers heat transfer, exhibits strong compatibility with current solid-state battery production, and significantly improves the rate performance and thermal conductivity of the battery with almost no increase in manufacturing costs. This invention is applicable to improving the rate performance of existing liquid batteries, and is particularly suitable for solid-state batteries with significant internal polarization.
[0008] This invention provides a method for improving the rate performance of solid-state batteries. The method includes seven steps in total: preparing positive and negative electrode slurries → coating positive and negative electrodes → rolling and cutting electrode sheets → welding electrode tabs → core preparation → assembly → post-processing.
[0009] In the cutting process, the negative electrode sheet is controlled to be 2.8–3.3 mm wider than the positive electrode sheet;
[0010] The electrode tab welding process is as follows: welding the positive electrode tab onto the positive electrode sheet and applying adhesive tape; welding the negative electrode tab onto the negative electrode sheet and applying adhesive tape.
[0011] The core preparation process is as follows: the positive electrode sheet after welding the positive electrode tab, the negative electrode sheet after welding the negative electrode tab, and the separator are wound into a cylindrical core; wherein, the bottom of the core is the negative end face, the negative electrode sheet on the negative end face extends beyond the separator by 0.8 to 1.3 mm, then a layer of insulating glue is first applied to the negative end face, after drying, the end face is polished, and then a layer of conductive glue is applied.
[0012] The assembly process is as follows: the prepared core is directly inserted into the steel shell without the lower gasket, and spot welding is performed. Then, the upper gasket and groove are installed and the cap is welded. After that, baking, adding solid electrolyte, and sealing are performed in sequence.
[0013] Preferably, in the above method for improving the rate performance of solid-state batteries, the negative electrode sheet is controlled to be 3mm wider than the positive electrode sheet in the cutting process.
[0014] Preferably, in the above method for improving the rate performance of solid-state batteries, in the core preparation process, the negative electrode sheet on the negative end face extends 1 mm beyond the separator.
[0015] In the aforementioned method for improving the rate performance of solid-state batteries, the insulating adhesive used in the core preparation process is made of epoxy resin.
[0016] In the aforementioned method for improving the rate performance of solid-state batteries, the thickness of the insulating adhesive is controlled to be 0.3–0.7 mm in the core preparation process.
[0017] In the above-mentioned method for improving the rate performance of solid-state batteries, in the core preparation process, after applying insulating adhesive, the drying temperature is 80-90°C and the drying time is 1-2 hours.
[0018] In the aforementioned method for improving the rate performance of solid-state batteries, the conductive adhesive used in the core preparation process is made of conductive carbon adhesive.
[0019] In the above-mentioned method for improving the rate performance of solid-state batteries, the thickness of the conductive adhesive is controlled to be 0.1-0.2 mm in the core preparation process.
[0020] In the above-mentioned method for improving the rate performance of solid-state batteries, the baking temperature in the assembly process is 80-90°C, and the baking time is 10-12 hours.
[0021] This invention also provides a solid-state battery prepared using the aforementioned method. This solid-state battery requires only a pair of positive and negative electrodes welded together. An insulating layer is first applied to the negative electrode face to prevent short circuits, followed by a conductive layer to increase the electron path area between the negative electrode and the steel casing, allowing electrons to flow rapidly between them. Simultaneously, the negative electrode extends beyond the separator, eliminating the need for a lower gasket, and its end face is closer to the steel casing, reducing heat accumulation. Therefore, this solid-state battery not only possesses superior rate performance but also excellent thermal conductivity, extending battery life.
[0022] The beneficial effects of this invention are:
[0023] To match existing production lines and processes and ensure battery reliability, this invention improves the core-winding process by welding only one pair of positive and negative electrode tabs. The negative electrode sheet extends 1mm beyond the separator on the negative end face of the core. A layer of conductive adhesive is applied to the negative end face of the core, increasing the electron path area between the negative electrode sheet and the steel shell, allowing electrons to flow rapidly between them. Compared to a lower pad, the conductive adhesive has better thermal conductivity, quickly transferring heat from the core to the steel shell and increasing heat dissipation. Furthermore, by extending the negative electrode sheet beyond the separator and eliminating the need for a lower pad, the entire end face is closer to the steel shell, reducing heat accumulation. Additionally, an insulating adhesive layer is applied before applying the conductive adhesive, and the negative electrode sheet is sanded to expose it before applying the conductive adhesive, preventing the conductive adhesive from seeping into the positive electrode sheet and causing a short circuit.
[0024] This invention improves battery rate performance, thermal conductivity, and battery life. The process is fully compatible with existing production lines and processes, reduces production costs, and facilitates industrial production. Attached Figure Description
[0025] Figure 1This is a schematic diagram of a core structure coated with insulating adhesive and conductive adhesive; where 1 is the core; 2 is the insulating adhesive; 3 is the conductive adhesive; 4 is the positive electrode tab; 5 is the tape; 6 is the negative electrode tab; and 10 is the negative electrode end face.
[0026] Figure 2 This is a schematic diagram of the unfolded core section; where 7 is the separator; 8 is the positive electrode sheet; and 9 is the negative electrode sheet.
[0027] Figure 3 This is a comparison chart of the load voltage and capacity of the solid-state battery of this invention and conventional designs during high-rate discharge.
[0028] Figure 4 This is a comparison chart of the temperature rise of the solid-state battery of this invention and that of conventionally designed batteries during high-rate discharge.
[0029] Figure 5 This is a comparison chart of battery temperature rise during discharge at different rates for three different conductive adhesive materials. Detailed Implementation
[0030] Specifically, a method for improving the rate performance of solid-state batteries includes the following steps: preparing positive and negative electrode slurries → coating positive and negative electrodes → rolling and cutting electrode sheets → electrode tab welding → core preparation → assembly → post-processing.
[0031] In the cutting process, the negative electrode sheet is controlled to be 2.8–3.3 mm wider than the positive electrode sheet;
[0032] The electrode tab welding process is as follows: welding the positive electrode tab onto the positive electrode sheet and applying adhesive tape; welding the negative electrode tab onto the negative electrode sheet and applying adhesive tape.
[0033] The core preparation process is as follows: the positive electrode sheet after welding the positive electrode tab, the negative electrode sheet after welding the negative electrode tab, and the separator are wound into a cylindrical core; wherein, the bottom of the core is the negative end face, the negative electrode sheet on the negative end face extends beyond the separator by 0.8 to 1.3 mm, then a layer of insulating glue is first applied to the negative end face, after drying, the end face is polished, and then a layer of conductive glue is applied.
[0034] The assembly process is as follows: the prepared core is directly inserted into the steel shell without the lower gasket, and spot welding is performed. Then, the upper gasket and groove are installed and the cap is welded. After that, baking, adding solid electrolyte, and sealing are performed in sequence.
[0035] In the method of this invention, the processes of preparing positive and negative electrode slurries, coating positive and negative electrodes, rolling and cutting electrode sheets are all routine operations in battery assembly. The slurry configuration parameters, coating parameters, and rolling parameters can be controlled according to conventional requirements in the field. However, in the cutting process, to accommodate a negative electrode sheet extending 0.8–1.3 mm beyond the separator, the sheet needs to be cut to a width of 2.8–3.3 mm wider than the positive electrode sheet. In the field of battery technology, taking a 21700 solid-state battery as an example, in conventional designs, the positive electrode width is 62 mm, the negative electrode width is 63.5 mm, and the separator width is 65.5 mm; this invention designs it to have a positive electrode width of 62 mm, a negative electrode width of 65 mm, and a separator width of 64 mm. Therefore, in the cutting process, this invention preferably controls the negative electrode sheet to be 3 mm wider than the positive electrode sheet, so that in the core preparation process, the negative electrode sheet on the negative end face extends 1 mm beyond the separator.
[0036] The electrode tab welding process of this invention is a conventional operation in the field. In this process, the positive and negative electrodes are welded to the current collector by ultrasonic welding. After welding, the area will be uneven, and the electrode tab ends may even be raised to form sharp points. In order to cover the burrs generated during welding, as well as the burrs on the electrodes themselves, and to prevent the burrs from piercing the separator and causing a short circuit inside the battery, adhesive tape is applied after welding in this invention. Figure 1 In the middle, the negative electrode tape does not extend beyond the edge of the negative electrode sheet, so the negative electrode tape is covered and not shown.
[0037] In the core preparation process of this invention, the winding is carried out on a specialized winding machine. A 3.5mm diameter circular winding needle, composed of two semicircles, is used to clamp the separators. The two separators pass through the center of the circular winding needle, which rotates once to secure the separators. Then, the negative electrode is pushed in between the upper and lower separators along the electrode guide plate. The brake pedal is applied, and the winding needle rotates once to allow the negative electrode to wrap around the positive electrode. The positive electrode is then pushed in above the upper separator along the electrode guide plate, and the brake pedal is applied again, causing the winding needle to rotate once. Once the positions of the positive and negative electrodes are confirmed to be the set positions, the brake pedal is applied again, causing the winding needle to rotate and wind the two separators, negative electrode, and positive electrode. Winding stops after reaching the set number of turns. Finally, the brake pedal is applied again, and the equipment is activated to complete the separator cutting, rotating and attaching the termination tape, and core delivery. For the positional relationship of the separator, negative electrode, and positive electrode during winding, please refer to the core diagram. Figure 1 and Figure 2 .
[0038] After obtaining the cylindrical core, at the bottom of the core near the negative electrode tab, i.e., the negative end face, where the negative electrode sheet extends approximately 1 mm beyond the separator, a layer of insulating adhesive is first applied to the negative end face. The insulating adhesive penetrates into the bottom of the core and is then dried at 80–90°C for 1–2 hours to cure. After curing, the adhesive is then sanded to expose the negative current collector. The thickness of the insulating adhesive after curing should ideally be between 0.3 and 0.7 mm (this thickness is the initial thickness when the insulating adhesive is first applied. Spin coating equipment can easily control the thickness of flowable insulating adhesive). Too thin an adhesive will hinder the penetration of conductive adhesive, while too thick an adhesive will require more material to be sanded away to allow the conductive adhesive to contact the negative current collector, and excessive thickness will also increase material consumption and costs. Furthermore, a too narrow thickness range will hinder production control and increase production costs.
[0039] In this invention, liquid insulating adhesive can be applied to the bottom of the core using a cotton swab. When applying, ensure that the insulating adhesive covers the bottom of the core so that it can prevent the conductive adhesive from penetrating. The insulating adhesive is made of epoxy resin, which is a liquid and has a certain degree of adhesion. It can flow and can be fixed to the battery after drying and curing.
[0040] Similar to applying insulating adhesive, this invention can also use a cotton swab to apply liquid conductive adhesive to the bottom of the core. For mass production, a spin coater can be used, ensuring controllable thickness and uniform application. The same process can be used for applying insulating adhesive. The thickness of the conductive adhesive should ideally be between 0.1 and 0.2 mm (this is the thickness immediately after application; spin coaters and similar equipment can easily control the thickness of the flowing conductive adhesive). Too thin a thickness will prevent the conductive adhesive from forming a smooth surface, thus hindering good contact with the steel shell; too thick a thickness will create significant impedance between the negative current collector and the steel shell, impeding electron conduction between the core and the steel shell.
[0041] When applying the conductive adhesive in this invention, the goal is to ensure that the conductive adhesive covers the bottom of the core so that the conductive adhesive can form a tight connection between the negative current collector and the steel shell.
[0042] This invention also screened conductive carbon paste, conductive copper paste, conductive silver paste, etc. From Figure 5 Based on the temperature rise data from the discharge test, conductive carbon paste and conductive copper paste are similar, while conductive silver paste is superior. However, conductive silver paste is expensive, and conductive copper paste is more costly than conductive carbon paste, with less stable quality and market supply. Considering all factors, conductive carbon paste is the preferred choice. Conductive carbon paste is a liquid with inherent adhesive properties and is flowable; after baking and curing, it can be fixed onto the battery.
[0043] In this invention, the drying of the conductive adhesive and the baking of the battery cell are overlapping steps. The baking temperature is 80-90°C and the baking time is 10-12 hours.
[0044] Conventional batteries require a bottom spacer during assembly to prevent the rigid negative electrode tab from contacting the positive electrode and to prevent the positive electrode from contacting the steel casing, thus avoiding a short circuit. This invention features a larger misalignment between the positive and negative electrodes and incorporates insulating adhesive, effectively preventing both short circuits. Furthermore, the purpose of this invention is to allow direct contact between the conductive adhesive and the steel casing, increasing electrical conductivity and heat transfer between the cell and the casing. Installing a bottom spacer would actually hinder this contact. Therefore, in the assembly process of this invention, the prepared core is directly inserted into the steel casing without a bottom spacer.
[0045] In this invention, the post-processing steps are conventional operations in the field.
[0046] Compared to conventional technical solution 1, which increases conductivity and thermal conductivity by introducing more tabs or modifying the size and layout of the introduced tabs, this invention does not require adding more tabs. Therefore, it does not introduce more stress inside the core, thus avoiding impacting battery life. In particular, the negative electrode does not need more tabs, preventing capacity reduction. Compared to conventional technical solution 2, which reserves blank areas on the side of the electrode as tabs to increase conductivity and thermal conductivity, this invention does not require changing the original battery design. It can utilize existing production processes and assembly equipment without additional technical or equipment investment. It boasts high production yield and efficiency, and its space utilization is close to that of existing technical solutions. As can be seen from the examples, with the same cell, the addition of conductive adhesive results in higher battery load voltage, higher capacity, and lower temperature rise under the same discharge rate conditions.
[0047] Based on the above research, this invention also provides a solid-state battery, especially a solid-state battery with high internal polarization within the cell. This solid-state battery only requires welding a pair of positive and negative electrodes. An insulating layer is first applied to the negative electrode face to prevent short circuits, followed by a conductive layer to increase the electron path area between the negative electrode and the steel casing, allowing electrons to flow rapidly between the electrode and the casing. Simultaneously, the negative electrode extends beyond the separator, eliminating the need for a lower gasket, and its end face is closer to the steel casing, reducing heat accumulation. Therefore, this solid-state battery not only possesses superior rate performance but also excellent thermal conductivity, extending battery life.
[0048] The present invention will be further described in detail below through embodiments, but the scope of protection of the present invention is not limited to the embodiments described herein.
[0049] Experimental Example 1
[0050] To improve the rate performance of a battery, it is crucial to address its internal electrical and thermal conductivity. This involves releasing the battery's energy through the rapid flow of electrons while simultaneously transferring the heat generated by this flow to prevent heat buildup. To achieve this, this invention explores the application of conductive adhesives, which possess excellent electrical and thermal conductivity, in solid-state batteries.
[0051] Option 1: In the early stages of research, considering that in conventional lithium-ion battery designs, the negative electrode is wider than the positive electrode (in a conventional 21700 solid-state battery design, the positive electrode is 62mm wide, the negative electrode is 63.5mm wide, and the separator is 65.5mm wide), it's possible that the conductive adhesive only contacts the negative electrode current collector and not the positive electrode current collector. Therefore, the inventors directly applied the conductive adhesive to the bottom of the core near the negative electrode tab, without drying (the flowing state allows for a tighter connection between the negative electrode current collector and the steel casing), eliminating the need for a lower gasket, and assembling the battery. The aim was to achieve the goal of connecting the negative electrode current collector and the steel casing with the conductive adhesive, increasing the conductivity and thermal conductivity of the core, thereby improving the battery's rate performance. However, almost all the batteries produced in practice short-circuited.
[0052] Solution 2: To solve the aforementioned short-circuit problem, the inventors designed an increase in the misalignment distance between the positive and negative electrode plates. Additionally, they considered reducing the distance between the negative current collector and the steel casing to further increase the conductivity and thermal conductivity of the winding core. This solution maintains the positive electrode plate position, while the negative electrode plate is positioned at the bottom of the winding core (the negative end face), extending 1mm beyond the separator. After winding, conductive adhesive is applied to the bottom of the winding core, but not dried (the flowing state allows for a tighter connection between the negative current collector and the steel casing). The lower spacer is then removed, and the battery is assembled. However, the actual manufactured batteries experienced partial short circuits and a high defect rate. Analysis of the disassembled batteries revealed that some of the conductive adhesive had seeped into the winding core along the gaps and contacted the positive electrode plate, causing a short circuit due to the connection between the positive and negative electrodes.
[0053] Option 3: In further research, the inventors maintained the above core design, i.e., the positive electrode was wrapped by the separator, and the negative electrode sheet extended 1mm beyond the separator. However, they abandoned the use of conductive adhesive, which could flow and easily cause short circuits due to contact between the positive and negative electrodes (i.e., they did not use conductive adhesive), and removed the lower gasket. After the core was prepared, it was directly assembled into a battery, and the battery performance was tested. However, the median discharge voltage was inconsistent. Through battery disassembly and analysis, it was found that because there was no pressure guarantee between the core and the steel shell, the tightness of the physical contact between the negative electrode current collector at the bottom of the core and the steel shell was highly random, resulting in different battery impedances and poor consistency of the median discharge voltage.
[0054] This invention addresses the problem of short circuits caused by direct application of conductive adhesive to the bottom of the core near the negative electrode tab, which can easily lead to contact between the positive and negative electrodes. The inventors first apply an insulating adhesive layer to the bottom of the core to form a barrier layer. After applying the insulating adhesive, it is dried and cured at 85°C. Then, a layer of conductive adhesive is applied to its surface. This conductive adhesive does not need to be dried initially (its fluid state allows for a tighter connection between the negative electrode current collector and the steel casing). The core is then directly installed into the battery casing and spot-welded. The curing of the conductive adhesive overlaps with the cell baking process, which involves baking at 85°C for 12 hours until the conductive adhesive becomes solid. After battery assembly, battery performance is tested and found to be good.
[0055] Table 1 Comparison of open-circuit voltage and median discharge voltage for each scheme
[0056]
[0057] Example 1
[0058] Step 1: Prepare the positive electrode slurry and negative electrode slurry. Mix the positive electrode active material and negative electrode active material separately with conductive agent, binder, solvent, etc., to prepare positive electrode slurry and negative electrode slurry with suitable viscosity.
[0059] Step 2: Coating the positive and negative electrodes. Add the positive and negative electrode slurries to the coating machine's feed tanks respectively. Set the parameters for coating thickness, coating length, blank length, coating speed, baking temperature, and baking air frequency according to the process requirements. After coating the front and back sides sequentially, roll up the coating and place it in a vacuum oven for baking.
[0060] Step 3: Rolling and Cutting Electrodes. The parameters of the rolling mill are set according to the compaction density designed for the battery cell. The baked electrodes from the previous steps are rolled through the rollers; the positive electrode is rolled once, and the negative electrode twice; then they are cut into pieces for later use.
[0061] Step 4: Electrode tab welding. After welding the positive and negative electrodes to the positive and negative electrode plates respectively, apply adhesive tape.
[0062] Step 5: Core Preparation. The prepared positive and negative electrode sheets, along with the separately provided separator, are wound into a cylindrical core. The bottom of the core is the negative electrode end, with the negative electrode extending approximately 1 mm beyond the separator. To prevent short circuits caused by contact between the positive and negative electrodes, a layer of insulating adhesive is first applied, dried at 85°C for 2 hours, and then the end faces are polished. The thickness of the insulating adhesive is 0.3–0.7 mm. Next, a layer of conductive carbon adhesive is applied, with a thickness of 0.1–0.2 mm.
[0063] Step 6: Assembly. The prepared core is inserted into the steel shell without the lower gasket, and spot welded. Then, the upper gasket and groove are installed, and the cap is welded. After that, it is baked at 85°C for 12 hours, solid electrolyte is added, and then it is sealed.
[0064] Step 7: Post-processing. Clean and oil the sealed batteries, cover them with a protective film, label them, and then sequentially complete the electrolyte membrane curing, pre-charging, high-temperature aging, formation, and capacity testing to obtain solid-state batteries.
[0065] Depend on Figure 3 and Figure 4It can be seen that, with the same battery cell, the solid-state battery of this invention, after adding the technical solution of coating conductive adhesive, has a higher load voltage, higher capacity, and lower temperature rise under the same discharge rate conditions compared with the conventional design CN202223187545.7.
Claims
1. A method for improving the rate performance of solid-state batteries, comprising: preparing positive electrode slurry and negative electrode slurry → coating positive electrode and negative electrode → rolling and cutting electrode sheets → electrode tab welding → core preparation → assembly → post-processing steps, characterized in that: In the cutting process, the negative electrode sheet is controlled to be 2.8–3.3 mm wider than the positive electrode sheet; The electrode tab welding process is as follows: welding the positive electrode tab onto the positive electrode sheet and applying adhesive tape; welding the negative electrode tab onto the negative electrode sheet and applying adhesive tape. The core preparation process is as follows: the positive electrode sheet after welding the positive electrode tab, the negative electrode sheet after welding the negative electrode tab, and the separator are wound into a cylindrical core; wherein, the bottom of the core is the negative end face, the negative electrode sheet on the negative end face extends beyond the separator by 0.8 to 1.3 mm, then a layer of insulating glue is first applied to the negative end face, after drying, the end face is polished, and then a layer of conductive glue is applied. The assembly process is as follows: the prepared core is directly inserted into the steel shell without the lower gasket, and spot welding is performed. Then, the upper gasket and groove are installed and the cap is welded. After that, baking, adding solid electrolyte, and sealing are performed in sequence.
2. The method for improving the rate performance of solid-state batteries according to claim 1, characterized in that: In the cutting process, the negative electrode sheet is controlled to be 3mm wider than the positive electrode sheet.
3. The method for improving the rate performance of solid-state batteries according to claim 1, characterized in that: In the core preparation process, the negative electrode sheet on the negative end face extends 1 mm beyond the separator.
4. The method for improving the rate performance of solid-state batteries according to claim 1, characterized in that: In the core preparation process, the insulating adhesive is made of epoxy resin.
5. The method for improving the rate performance of solid-state batteries according to claim 1, characterized in that: In the core preparation process, the thickness of the insulating adhesive is controlled to be 0.3–0.7 mm.
6. The method for improving the rate performance of solid-state batteries according to claim 1, characterized in that: In the core preparation process, after applying insulating adhesive, the drying temperature is 80-90℃ and the drying time is 1-2 hours.
7. The method for improving the rate performance of solid-state batteries according to claim 1, characterized in that: In the core preparation process, the conductive adhesive is made of conductive carbon adhesive.
8. The method for improving the rate performance of solid-state batteries according to claim 1, characterized in that: In the core preparation process, the thickness of the conductive adhesive is controlled to be 0.1–0.2 mm.
9. The method for improving the rate performance of solid-state batteries according to any one of claims 1 to 8, characterized in that: In the assembly process, the baking temperature is 80-90℃ and the baking time is 10-12 hours.
10. A solid-state battery prepared by any one of claims 1 to 9.
Citation Information
Patent Citations
High-power high-specific-energy cylindrical battery
CN218632369U
Lithium-ion secondary battery with steel shell as cathode and manufacturing method thereof
CN101604765A
Cylindrical lithium ion secondary battery
CN212648278U