Method for manufacturing agar or agarose beads using natural or vegetable oils

By using a stepwise cooling method and heat exchangers to control the temperature gradient in industrial-scale production, the cooling control problem in the production of agar or agarose beads with natural or vegetable oils as the continuous phase is solved, achieving controlled bead size and porosity, suitable for chromatographic resins.

CN117642433BActive Publication Date: 2026-11-10BIO WORKS TECH AB
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202280047718.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-07-15
Filing Date
2022-07-15
Publication Date
2026-11-10
Estimated Expiration
2042-07-15

AI Technical Summary

Technical Problem

Existing technologies make it difficult to control the cooling process when using natural or vegetable oils as a continuous phase to produce agar or agarose beads on an industrial scale. This results in uncontrolled bead shape, size, and porosity properties, as well as the presence of oil inclusions.

Method used

A stepwise cooling method is adopted, in which the aqueous phase and oil phase are combined in the reactor and an emulsifier is added to form an emulsion. The heat exchanger is used for rapid and controlled cooling to control the temperature gradient and ensure that the gelation process of the beads is controlled.

Benefits of technology

It enables the production of agar or agarose beads with controlled size distribution and porosity in industrial-scale production, reducing oil content and making them suitable for use as chromatography resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117642433B_ABST
    Figure CN117642433B_ABST
Patent Text Reader

Abstract

A method for manufacturing agar or agarose beads suitable for use as chromatography resin, the method comprising the steps of: i) providing an aqueous phase comprising an aqueous solution of agar or agarose at a temperature above the gelling temperature of the aqueous solution; ii) providing an oil phase comprising a natural or vegetable oil at a temperature above the gelling temperature of the aqueous solution provided in step i); iii) combining the aqueous phase provided in step i) with the oil phase provided in step ii) in a reactor and adding an emulsifier; iv) emulsifying the mixture obtained in step iii), preferably by stirring the mixture, thereby creating an emulsion; v) performing a stepwise cooling comprising a first cooling step of cooling the emulsion obtained in step iv) to a temperature 0.1-30°C above the gelling temperature of the aqueous solution provided in step i), followed by a second cooling step of emptying the emulsion from the reactor and passing the emulsion through a heat exchanger, thereby allowing the emulsion to be cooled to a temperature below the gelling temperature of the aqueous solution provided in step i); and vi) recovering agar or agarose beads from the emulsion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to a method for producing agar or agarose beads suitable for use as chromatographic resins by emulsifying a mixture using natural or vegetable oils. Background Technology

[0002] Agarose beads for separation purposes have been commercially available for fifty years. Typically, a hot agarose solution is emulsified in a solvent immiscible with hot water to form a water-in-oil (W / O) emulsion, which is then cooled below the gelation temperature of agarose to form beads, thus obtaining agarose beads. These beads are then collected in subsequent separation steps. This method has been described, for example, in PORATH J et al., Journal of Chromatography, vol. 60, January 1, 1971, US2018071484, and WO1989011493.

[0003] A key parameter of agarose beads used as chromatography resins is their porosity. Porosity is controlled through various parameters during production; however, the cooling of the emulsion solution is the most critical. To obtain the desired porosity range in the beads, controlling the cooling and temperature gradient during the cooling process of the emulsion mixture is essential.

[0004] Traditionally, water-immiscible solvents used as the continuous phase in emulsions are typically selected from organic solvents, such as toluene. Toluene is advantageous when producing beads with controlled porosity and size because its low viscosity provides good control over cooling. This method is disclosed, for example, in WO2020221762. However, growing environmental concerns in recent years have driven industry to develop production methods that avoid the use of organic solvents and to partially or completely replace these methods with natural or plant-based substitutes. Furthermore, the use of organic solvents such as toluene raises other issues, such as the risk of explosion and concerns about occupational health and safety.

[0005] Agar consists of agarose and agar gum, typically in a ratio of 90:10 to 70:30. Both agarose and agar gum are polysaccharides with alternating dehydrated galactose and galactose subunits, meaning their polysaccharide backbones are identical. Agar gum is significantly sulfated and therefore negatively charged. Furthermore, it is methylated, meaning it contains methoxy groups. Agarose, on the other hand, is inherently uncharged and lacks sulfate groups. Agar, particularly desulfated agar and agarose, was initially proposed as a raw material for preparing crosslinked separation gels. See, for example, US 3959251 (Porath et al.). However, in recent years, more focus has been placed on agarose rather than agar, likely due to the high sulfate content of agar (present in agar gum) and the challenge of removing sulfate groups without negatively impacting the quality of the agar substrate.

[0006] It has been previously shown that vegetable oils can replace organic solvents as the continuous phase in water-in-oil emulsions when producing agarose beads, as in NICOLAS IONNIDIS et al., Journal of Colloid and Interface Science 367 (2012) and CHEN et al., Journal of Separation Science, vol 40, 22 / 17. However, these results were all produced on a laboratory scale and are therefore very small in volume.

[0007] Because vegetable oils have significantly higher viscosity than organic solvents, controlling the cooling of emulsions containing vegetable oil as a continuous phase is more challenging. When emulsifying on a smaller scale, this is less of a problem due to the smaller volume of the process, making jacketed cooling of the reactor a suitable option for cooling emulsions containing a high-viscosity continuous phase. However, this is not the choice for industrial-scale production because jacketed cooling combined with high-viscosity vegetable oils results in slow and uncontrolled cooling, leading to impaired shape, size, and porosity properties in the beads. Slow cooling results in relatively high porosity. Rapid cooling results in smaller pores.

[0008] It would be advantageous to produce agar or agarose beads using industrially feasible methods that do not employ organic solvents such as toluene. Furthermore, it would be advantageous to produce agar or agarose beads with controlled size and / or porosity distributions. Summary of the Invention

[0009] One object of the present invention is to reduce or eliminate one or more of the above-mentioned disadvantages by providing an improved method for producing agar or agarose beads.

[0010] Another object of the present invention is to provide a method for preparing agar or agarose beads using a water-in-oil (W / O) emulsion containing natural or vegetable oil as the continuous phase (oil phase). Thus, a method is achieved that eliminates or reduces the use of low-viscosity organic solvents.

[0011] Another object of the present invention is to provide a method for manufacturing agar or agarose beads, which includes a cooling step suitable for use in industrial-scale production.

[0012] Another object of the present invention is to provide a method for manufacturing agar or agarose beads, wherein the method produces agar or agarose beads having a controlled size distribution and shape.

[0013] Another object of the present invention is to provide a method for manufacturing agar or agarose beads, wherein the method produces agar or agarose beads having controlled porosity.

[0014] Another object of the present invention is to provide a method for manufacturing agar or agarose beads, wherein the method reduces or eliminates oil inclusions in the beads.

[0015] Another object of the present invention is to provide agar or agarose beads suitable for use as chromatography resins.

[0016] In a general embodiment of the present invention, a method for manufacturing agar or agarose beads is provided, the method comprising the following steps:

[0017] i) Provide an aqueous phase containing the aqueous solution at a temperature higher than the gelation temperature of the aqueous solution of agar or agarose;

[0018] ii) Provide an oil phase containing natural or vegetable oil at a temperature higher than the gelation temperature of the aqueous solution provided in step i);

[0019] iii) Combine the aqueous phase provided in step i) and the oil phase provided in step ii) in the reactor and add an emulsifier;

[0020] iv) Emulsify the mixture obtained in step iii), preferably by stirring the mixture, to produce an emulsion;

[0021] v) A gradual cooling process is performed, comprising a first cooling step of cooling the emulsion obtained in step iv) to a temperature 0.1-30°C higher than the gelation temperature of the aqueous solution provided in step i), followed by a second cooling step of draining the emulsion from the reactor and passing it through a heat exchanger, thereby cooling the emulsion to a temperature lower than the gelation temperature of the aqueous solution provided in step i); and

[0022] vi) Recover agar or agarose beads from the emulsion.

[0023] The method of this invention achieves more controlled particle size distribution and porosity. Unbound by theory, it is believed that by subjecting the emulsion to gradual cooling, thereby initially bringing it to a temperature close to but still above the gelation temperature of an agar or agarose aqueous solution, a reduced viscosity difference is achieved between the onset of cooling and the gelation point (i.e., the temperature at which “viscous” beads transform into gelled (i.e., solid) beads). This reduced temperature and viscosity difference between the initial temperature at which the beads are still in their viscous form and the temperature below the gelation temperature (i.e., when the beads will be in their gelled (i.e., solidified) form) makes it easier to control the temperature gradient. This, in turn, allows for better control of temperature-dependent parameters, such as size distribution and porosity, which are highly influenced by the cooling rate. Controlling cooling is crucial when the emulsion contains a continuous phase exhibiting high viscosity, making temperature control during cooling more challenging compared to conventional organic solvents.

[0024] Rapid cooling with a controlled temperature gradient is achieved by subjecting the emulsion to final cooling via a heat exchanger. This allows for control of the temperature distribution during gelation and, consequently, the size distribution and porosity of the resulting beads. Furthermore, by enabling rapid and controlled cooling, this method can be used in industrial-scale production, even when employing a high-viscosity continuous phase in a water-in-oil (W / O) emulsion.

[0025] The aqueous phase containing agar or agarose may be natural agar, natural agarose, or a derivative of agar or agarose, as described, for example, in WO2008136742 and US6602990, the entire contents of which are incorporated herein by reference.

[0026] The gelation temperature of agar or agarose solutions is typically above 40°C. However, this value varies slightly depending on the amount and purity of the agar present in the solution. Those skilled in the art will understand and appreciate such variations. In one embodiment of the invention, the aqueous phase comprising the agar or agarose solution is provided at a temperature above 40°C, preferably between 40-99°C, more preferably between 40.1-99.9°C, and even more preferably between 41-95°C.

[0027] In one embodiment of the invention, the oil phase is provided at a temperature above 40°C, preferably at a temperature of 40-99°C, more preferably at a temperature of 40.1-99.9°C, and even more preferably at a temperature of 41°C-95°C.

[0028] In one embodiment, the emulsifier is added to the combined solution after the aqueous and oil phases have been combined. Preferably, the emulsifier is added after the aqueous phase is added to the oil phase.

[0029] In one embodiment, step iv) of emulsifying the mixture can be performed by any conventional emulsification method known to those skilled in the art.

[0030] The first cooling step for cooling the emulsion obtained in step iv) cools the emulsion to a temperature 0.1-30°C higher than the gelation temperature of the aqueous solution provided in step i). In one embodiment, the first cooling step cools the emulsion to a temperature 0.5-15°C higher than the gelation temperature of the aqueous solution provided in step i), preferably 0.5-10°C higher, and even more preferably 0.5-5°C higher. In one embodiment, the first cooling step cools the emulsion to a temperature of 40.5-49°C, preferably 41-45°C.

[0031] By cooling in a stepwise manner according to the present invention, an oil phase that is more viscous than an organic solvent can be utilized, because the cooling will be carried out in a rapid, controlled and convenient manner.

[0032] Agar or agarose beads can be recovered from the formed emulsion using any conventional method known to those skilled in the art. In one embodiment, the beads are settled in the presence of excess water and optionally a surfactant to separate them from the aqueous phase, thereby recovering the beads.

[0033] In one embodiment of the invention, step iii) is carried out by adding the aqueous solution from step i) to the oil phase provided in step ii) in a reactor, preferably by pouring the aqueous solution from step i) into a reactor containing the oil phase from step ii). The inventors have surprisingly discovered that the method of addition significantly affects the formation of beads in the emulsion. Conventionally, when emulsifying with a low-viscosity solvent such as toluene, toluene is added to the aqueous phase. However, if this method of addition is used for more viscous oils such as vegetable oils, the subsequently formed beads will exhibit oil inclusions that impair quality. The inventors have solved this problem by instead adding the aqueous phase to the oil phase. Preferably, the addition of the aqueous phase to the oil phase is carried out in a controlled manner, for example by pouring or dripping, to ensure a more uniform distribution and avoid flocculation. Furthermore, the temperature of the aqueous phase at the time of addition to the oil phase has shown an influence on the final properties of the beads. Preferably, the aqueous phase is added at a temperature above 70°C, preferably above 80°C, more preferably above 90°C, and even more preferably above 95°C.

[0034] In one embodiment of the invention, steps iii) and iv) are performed simultaneously. In another embodiment of the invention, step iv) begins after the aqueous phase has been added to the oil phase.

[0035] In one embodiment of the invention, the first cooling step is performed by cooling the emulsion in the reactor to a temperature 0.1-20°C higher than 40°C, preferably to a temperature 1-10°C higher than 40°C, and even more preferably to a temperature 1-5°C higher than 40°C. As mentioned above, cooling the emulsion to a temperature close to the gelation temperature of an aqueous solution of agar or agarose (i.e., the aqueous phase) reduces the viscosity difference between the onset of cooling and the gelation temperature of the beads. This, in turn, produces a more controlled temperature gradient and controlled parameters, such as the porosity and size distribution of the beads.

[0036] In one embodiment of the invention, the second cooling step involves cooling the emulsion to a temperature below 30°C, preferably below 25°C. Beads are obtained by cooling to a temperature below the gelation temperature of the aqueous solution of agar or agarose (i.e., the aqueous phase).

[0037] Natural oils can be obtained from different parts of oil-bearing plants, such as oils from seeds, fruits, leaves, flowers, stems, bark, or roots. In one embodiment of the invention, the vegetable oil is selected from rapeseed oil, corn oil, sunflower oil, peanut oil, or other vegetable-based oils. Preferably, the vegetable oil is rapeseed oil. Rapeseed oil has been shown to exhibit optimal viscosity characteristics to ensure controlled cooling of the emulsion.

[0038] In one embodiment of the invention, the stirring in step iv) is performed by an overhead mixer, preferably at 1000-2000 rpm, and even more preferably at 1250-1750 rpm. Traditionally, high-shear mixers are used when manufacturing agar or agarose beads. However, when using oils with a higher viscosity than conventional organic-water immiscible solvents, high-shear mixing results in the oil being contained within the beads. Without being bound by theory, it is believed that the increased viscosity during mixing leads to increased mechanical impact on the beads compared to the same method in a low-viscosity oil phase. However, it has been shown that by using a conventional high-speed mixer, the high-viscosity oil phase allows for a good particle size distribution in the beads. The mixer speed (revolutions per minute or rpm) has been shown to have an effect on the bead size distribution. Increased speed results in stronger shear forces and a lower bead Dv50 value. Dv50 represents 50% by weight of the product below a specific micrometer size. High speeds can also force the continuous phase (oil phase) within the formed emulsion beads, resulting in emulsion formation within the emulsion, which will impair the properties of the resulting beads. Too low a speed will not produce an emulsion.

[0039] In one embodiment of the invention, the second cooling step includes passing the emulsion through a series of heat exchangers. By using a series of heat exchangers, different cooling settings can be provided, thereby controlling the cooling gradient differently.

[0040] In one embodiment of the invention, the second cooling step includes passing the emulsion through a 100-700 kW heat exchanger, preferably a 600-700 kW heat exchanger. Preferably, the water temperature passing through the heat exchanger is 5-20°C, and even more preferably 7-15°C.

[0041] In one embodiment of the invention, the volume ratio between the aqueous phase and the oil phase is 1:9 to 1:1, preferably 1:4 to 1:1, and more preferably 2:5 to 5:8. A higher volume of aqueous phase relative to the oil phase results in a higher Dv50 value.

[0042] In one embodiment of the invention, the emulsifier is a nonionic surfactant, preferably, anhydrous sorbitol ester. In one embodiment, the emulsifier is selected from the SPAN family, preferably, from Span... TM 80. Span TM 85 or mixtures thereof. The type of emulsifier affects bead size and bead geometry. Poorly chosen emulsifiers can lead to bead flocculation and oil inclusions. Emulsifiers reduce the interfacial tension between the oil and aqueous phases, facilitating the separation of smaller droplets and stabilizing them. Poor interactions often result in deformability. To obtain spherical agar or agarose beads when using a high-viscosity oil phase, emulsifiers selected from sorbitol esters (i.e., SPAN) have shown to produce minimal deformed beads while maintaining good size distribution.

[0043] Emulsifiers are characterized by their HLB value. The HLB value is an indicator of an emulsifier's solubilizing properties and indicates the type of emulsion (O / W or W / O) for which the emulsifier is best suited. In water-in-oil (W / O) emulsions, a low HLB value is preferred because it implies higher solubility in the continuous phase (oil phase), which helps to achieve a larger proportion of beads within a controlled size range compared to emulsifiers with higher HLB values.

[0044] In one embodiment of the present invention, the mixture obtained in step iii) contains an emulsifier in an amount of 10-20 g / L oil phase, preferably 12.5-17.5 g / L oil phase.

[0045] In one embodiment of the present invention, step iv) is performed at 60-95°C.

[0046] In one embodiment of the invention, the aqueous solution of agar or agarose contains 1-9% by weight of agar or agarose, preferably 3-8% by weight, and even more preferably about 7% by weight. The agar or agarose content of the aqueous solution determines the viscosity of the aqueous phase in the emulsion. Viscosity is crucial for determining the quality of phase mixing and the size of the beads in the resulting emulsion. Increased agar content generally contributes to larger, denser beads with lower porosity values. Furthermore, a high agar content appears to reduce the amount of oil inclusions. Lower agar content requires less energy input to shear and thus emulsify the mixture.

[0047] In one embodiment of the present invention, the volume ratio between the aqueous phase and the oil phase is 2:8.

[0048] In one embodiment of the invention, the aqueous phase may further contain at least one salt. The salt increases the gelation temperature while reducing viscosity. In one embodiment of the invention, the aqueous phase may further contain an acid. A lower pH reduces the viscosity of the aqueous phase and affects gel strength. In one embodiment of the invention, the oil phase further contains an antifoaming agent.

[0049] In a second general embodiment of the invention, agar or agarose beads obtained by the method according to any of the foregoing embodiments are provided. The beads exhibit K... d The porosity measured by thyroglobulin was 0.20–0.35, and more than 50% of the beads exhibited a size of 30–75 μm.

[0050] In one embodiment of the invention, more than 55% of the beads exhibit a size of 30-75 μm.

[0051] In gel filtration, the distribution of a particular compound between the internal and external mobile phases is a function of its molecular size, which is determined by the distribution coefficient (K). d () indicates. Larger molecules, such as those with K, are typically excluded from gel beads. d The value will be 0. Some molecules smaller than the pore size of the gel beads enter the pores of the gel matrix, therefore their K value will be 0. d The value is 1. For medium-sized molecules, their K... d The value is between 0 and 1. K d This type of value variation allows for the separation of molecules within a narrow range of molecular sizes. Attached Figure Description

[0052] The invention will now be described by way of example with reference to the accompanying drawings, in which:

[0053] Figure 1The image shows a 10X microscopic image of agarose beads produced by emulsifying the agar solution in rapeseed oil by adding the agar solution to the oil phase at different rates. Figure 1 It is divided into a left half and a right half, which are separated by a dotted line.

[0054] Figure 2 The image shows a 10X microscopic image of agarose beads produced by emulsifying an agar solution in rapeseed oil using different addition techniques. Figure 2 It is divided into a left half and a right half, which are separated by a dotted line.

[0055] Figure 3 The image shows 10X microscopic images of agarose beads produced by emulsifying an agar solution in rapeseed oil and toluene, respectively. Figure 3 It is divided into a left half and a right half, which are separated by a dotted line. Detailed Implementation

[0056] As used herein, “% by weight” means the percentage by weight of the ingredient mentioned in relation to the total weight of the compound or composition mentioned.

[0057] As used in this article, “about” should be interpreted as being as precise as the method used to measure the value mentioned.

[0058] This invention relates to a method for manufacturing agar or agarose beads suitable for use as chromatographic resins. The method utilizes a water-in-oil (W / O) emulsion comprising a natural or vegetable oil as the oil phase (continuous phase). When the resulting emulsion is cooled by stepwise cooling according to the invention, gelled (solidified) beads are formed. The stepwise cooling according to the invention enables the method to be used in industrial-scale processes because the cooling is carried out in a rapid, convenient, and controlled manner.

[0059] As mentioned earlier, several problems arise when replacing low-viscosity organic solvents such as toluene with high-viscosity vegetable oils due to the different properties of the oil phases. With increasing viscosity, temperature control for cooling becomes more challenging. Without a controlled temperature gradient, it becomes more difficult to control parameters such as the size distribution and pore size of the resulting beads. The increased viscosity also presents problems in how to combine the different phases together.

[0060] Methods that combine oil and water phases

[0061] As mentioned earlier, if the continuous phase has a high viscosity (oil phase), how the dispersed phase (aqueous phase) is added to the system becomes very important. If a low-viscosity continuous phase, such as toluene, is used, no difference in the final product is observed during the addition of the continuous phase to the agar solution, and vice versa. In this case, the addition rate does not appear to affect the results. However, in the case of a high-viscosity continuous phase (rapeseed oil), if the agar is added too quickly (see...),... Figure 1 Or, if instead, the oil is added to the agar (“reverse” emulsification) (see...) Figure 2 If ), then the final product will contain oil inclusions.

[0062] Figure 1 A 10X microscopic image of agarose beads produced by emulsifying an agar solution in rapeseed oil is shown. A 4:1 mixture of rapeseed oil and agar solution (7%) and 15 g / L Span was used. TM A standard emulsion consisting of 85% oil phase was stirred at 90°C using an overhead stirrer (1500 rpm) to produce beads. Gradual cooling was then performed, with a first cooling step to cool the emulsion to 40°C in the reactor, followed by a second cooling step through a 115 kW heat exchanger. Figure 1 The left half shows the beads produced by slowly adding agar solution to the oil phase. Figure 1 The right half shows the beads produced when an agar solution is rapidly added to oil. (Example) Figure 1 As shown, rapid addition leads to oil inclusions in the beads (see...). Figure 1 (the right half)

[0063] Figure 2 A 10X microscopic image of agarose beads produced by emulsifying an agar solution in rapeseed oil is shown. A 4:1 mixture of rapeseed oil and agar solution (7%) and 15 g / L Span was used. TM A standard emulsion consisting of 85% oil phase was stirred at 90°C using an overhead stirrer (1500 rpm) to produce beads. Gradual cooling was then performed, with a first cooling step to cool the emulsion to 40°C in the reactor, followed by a second cooling step through a 115 kW heat exchanger. Figure 2 The left half shows the beads produced when oil is added to an agar solution. Figure 2 The right half shows the beads produced when an agar solution is added to oil. (Example) Figure 2 As shown, if oil is added to the agar solution, oil inclusions will appear in the beads (see...). Figure 2 (The left half). This phenomenon is not observed when the agar solution is added to the oil.

[0064] Agar should preferably be added at a warm temperature (approximately 95°C) to avoid localized gelation.

[0065] Mixer type and RPM (revolutions per minute)

[0066] Traditionally, high-shear mixers are used when manufacturing agar or agarose beads to efficiently produce small droplets within the desired size range. However, this method cannot be used in emulsions with a high-viscosity continuous phase, as this would result in oil inclusions. Unbound by theory, it is believed that the increased viscosity during mixing leads to increased mechanical impaction on the beads compared to the same method in a low-viscosity oil phase. However, it has been shown that using conventional high-speed mixers allows for good particle distribution of the beads even in high-viscosity oil phases.

[0067] As in Figure 3 As can be seen, the mixing rate has a significant impact on the distribution of beads. Figure 3 10X microscopic images of agarose beads produced by emulsifying an agar solution in rapeseed oil and toluene, respectively, are shown. A 4:1 mixture of rapeseed oil and agar solution (7%) and 15 g / L Span were used. TM A standard emulsion consisting of 85% oil phase was agitated at 8000 rpm using a high-shear mixer at 90°C to produce beads. Gradual cooling was then performed, with a first cooling step to cool the emulsion to 40°C in the reactor, followed by a second cooling step through a 115 kW heat exchanger. Figure 3 The left half shows the beads produced in toluene. Figure 3 The right half of the image shows pearl-like particles in rapeseed oil. It can be seen that the quality of the particles is compromised when a high-shear mixer is used with rapeseed oil (see [link]). Figure 3 (The right half). Produced using lower rpm. Figure 1 and Figure 2 The beads shown exhibit less oil inclusions and a better overall distribution.

[0068] The ratio between the dispersed phase (aqueous phase) and the continuous phase (oil phase)

[0069] As mentioned earlier, the ratio between the dispersed phase (aqueous phase) and the continuous phase significantly affects the particle size distribution and pore size of the beads. Table 1 shows the results of an experimental series based on eight different experiments, in which four different parameters and their effects on the percentage of Dv50 and 30-75 μm beads were investigated. The parameter with the greatest influence so far in this series of experiments is the ratio between the dispersed phase and the continuous phase (AgOil).

[0070] Dv50 indicates that 50% of the product by weight is below a specific micrometer size.

[0071] Table 1

[0072]

[0073] emulsifier

[0074] In water-in-oil emulsions, low HLB values ​​are preferred because they imply higher solubility in the continuous (non-polar) phase, which contributes to a larger proportion of bead clusters in the 30-75 μm range compared to emulsifiers from the same chemical family but with higher HLB values. Two different emulsifiers from the SPAN family with different HLB values ​​were investigated. The results are shown in Table 2. Table 2 describes the effects of using SPAN emulsifiers... TM 80 and Span TM Differences in particle distribution of 85 emulsified beads. A solution of rapeseed oil and agar (5.3%) in a 4:1 ratio and 15 g / L Span was used. TM A standard emulsion consisting of 85% oil phase was stirred at 90°C using an overhead stirrer (1500 rpm) to produce beads. Gradual cooling was then performed, with a first cooling step to cool the emulsion to 55°C in the reactor, followed by a second cooling step through a 115 kW heat exchanger.

[0075] As shown in Table 2, lower HLB values ​​result in more beads within a specific size range and also a narrower overall size distribution.

[0076] Table 2

[0077]

[0078] First cooling step

[0079] As mentioned earlier, the use of stepwise cooling, where the first cooling step cools the emulsion to a temperature close to the gelation temperature of the agar or agarose solution, results in greater size control. Table 3 shows the effect of the first cooling step on bead size. This table describes the differences in particle distribution of beads cooled from different temperatures (i.e., temperature variations in the first cooling step). A 4:1 ratio of rapeseed oil to agar solution (7%) and 15 g / L Span were used. TM A standard emulsion consisting of 85% oil phase was stirred at 90°C using a top-mounted stirrer (1500 rpm) to produce beads. The beads were first cooled to a specified temperature in a reactor (first cooling step), and then cooled through a 115 kW heat exchanger (second cooling step).

[0080] It can be seen that by increasing the starting temperature of the second cooling step (the temperature of the first cooling step is higher), fewer beads within the desired size range were achieved. The conclusion of this experiment is that the temperature of the first cooling step significantly affects the size distribution of the beads.

[0081] Table 3

[0082]

[0083] Cooling technology

[0084] Various cooling techniques were evaluated: cooling in a reactor, cooling in a cooling vessel, and cooling by means of a heat exchanger. The results are shown in Table 4. A 4:1 mixture of rapeseed oil and agar solution (4.7%) and 15 g / L Span were used. TM A standard emulsion consisting of 85% oil phase was stirred at 90°C using a top-mounted stirrer (1500 rpm) to produce beads.

[0085] While the hot emulsion mixture is stirred, cooling is achieved in the reactor by flowing cold tap water through the reactor jacket. This method prolongs the uniform cooling of the emulsion mixture. Compared to other cooling methods, this method yields emulsions with high K0 content. d The porous beads are also slightly softer (see Table 4). However, this type of cooling sometimes leads to bead flotation and the formation of permanent aggregates.

[0086] Cooling in the cooling container is achieved by pouring the hot emulsion onto a cold cooling medium. This results in immediate cooling to the final temperature. This rapid cooling causes the beads to become less porous, which is reflected in a lower K0. d However, this method requires an additional refrigerant in continuous phase and an open container, which is not necessary in other methods. Therefore, it is not optimal for industrial-scale production.

[0087] Cooling is achieved by passing the hot emulsion mixture through a cooling heat exchanger. This gives the beads comparable porosity properties to those cooled, for example, in a cooling container, i.e., the beads have a relatively low K0. d value.

[0088] As can be seen from Table 4, compared with other cooling technologies, cooling in a heat exchanger results in a larger number of beads and a narrower size distribution within the required size specifications.

[0089] Table 4

[0090]

[0091] Effect of gradual cooling on porosity

[0092] In the following embodiments, the effect of gradual cooling on the porosity of the formed beads was investigated. As described above, by gradually cooling the emulsion, first bringing it to a temperature close to but still above the gelation temperature of agar or agarose aqueous solution, and then cooling the emulsion below the gelation temperature, the cooling temperature gradient can be more easily controlled. The porosity of the formed beads is highly affected by the cooling rate.

[0093] An agar aqueous solution containing 7% agar was prepared. The aqueous solution was heated to 94°C and poured into an oil phase containing rapeseed oil and Span 85 while stirring. The combined agar aqueous solution and oil phase were stirred at 980 RPM at 94°C. The resulting emulsion consisted of a 4:1 ratio of rapeseed oil to the agar aqueous solution (7%) and 15 g / L Span 85. TM 85% oil phase composition.

[0094] A first cooling step is performed to cool the emulsion to 43°C in the reactor. The cooled emulsion is then transferred to a 660kW heat exchanger connected to cooling tap water at 12°C. The emulsion is cooled to 14–18°C and the formed agar beads are recovered.

[0095] The obtained beads are in K d The porosity measured by thyroglobulin is shown in Table 5.

[0096]

[0097] As can be seen, compared to the beads shown in Table 4 produced using a single cooling step and with similar agar concentrations, K d The thyroglobulin levels were significantly lower. Therefore, the porosity of the agar beads obtained by this method is comparable to that of commercially available agar beads formed using toluene as the oil phase.

Claims

1. A method for manufacturing agar or agarose beads suitable for use as a chromatography resin, wherein the method comprises the following steps: i) Provide an aqueous phase containing the aqueous solution at a temperature higher than the gelation temperature of the aqueous solution of agar or agarose; ii) Provide an oil phase containing vegetable oil at a temperature higher than the gelation temperature of the aqueous solution provided in step i); iii) Combine the aqueous phase provided in step i) and the oil phase provided in step ii) in a reactor and add an emulsifier, wherein the volume ratio between the aqueous phase and the oil phase is 1:9 to 1:1; iv) Emulsify the mixture obtained in step iii) by stirring the mixture to produce an emulsion; v) A gradual cooling process is performed, comprising a first cooling step of cooling the emulsion obtained in step iv) to a temperature 0.1-20°C higher than 40°C, followed by a second cooling step of draining the emulsion from the reactor and passing it through a heat exchanger, thereby cooling the emulsion to a temperature below 30°C; and vi) Recover agar or agarose beads from the emulsion.

2. The method of claim 1, wherein step iii) is carried out by adding the aqueous solution from step i) to the oil phase provided in step ii) in the reactor.

3. The method as described in claim 1 or 2, wherein steps iii) and iv) are performed simultaneously.

4. The method of claim 1 or 2, wherein the first cooling step is performed by cooling the emulsion in the reactor to a temperature 1-10°C higher than 40°C.

5. The method of claim 1 or 2, wherein the second cooling step cools the emulsion to a temperature below 25°C.

6. The method of claim 1 or 2, wherein the vegetable oil is selected from rapeseed oil, corn oil, sunflower oil or peanut oil.

7. The method of claim 1 or 2, wherein the stirring in step iv) is performed by a top-mounted mixer.

8. The method of claim 1 or 2, wherein the second cooling step comprises passing the emulsion through a series of heat exchangers.

9. The method of claim 1 or 2, wherein the second cooling step comprises passing the emulsion through a 100-700 kW heat exchanger.

10. The method of claim 1 or 2, wherein the volume ratio between the aqueous phase and the oil phase is 1:4 to 1:

1.

11. The method of claim 1 or 2, wherein the emulsifier is a nonionic surfactant.

12. The method of claim 1 or 2, wherein the mixture obtained in step iii) contains an amount of emulsifier of 10-20 g / L oil phase.

13. The method of claim 1 or 2, wherein step iv) is performed at 60-95°C.

14. The method of claim 1 or 2, wherein the aqueous solution of agar or agarose contains 1-9% by weight of agar or agarose.

Citation Information

Patent Citations

  • Catheter hubs

    US20180071484A1

  • Stabilized agar product and method for its stabilization

    US3959251A

  • Process for the production of a porous cross-linked polysaccharide gel and its use as a gel filtration media and in chromatography

    US6602990B1

  • Process for preparation of agarose particles

    WO1989011493A1

  • Method for the manufacture of agarose gels

    WO2008136742A1