Nanocellulose composite elastomer and its preparation method

By preparing a nanocellulose composite elastomer with an interwoven structure of woody nanocellulose and polymer microspheres, the problems of long preparation time and poor adsorption performance in the existing technology have been solved. This has resulted in a nanocellulose composite elastomer with low density, high porosity and large specific surface area, which is suitable for applications in multiple fields.

CN117659730BActive Publication Date: 2026-11-10INST OF WOOD INDUDTRY CHINESE ACAD OF FORESTRY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211019861.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-24
Publication Date
2026-11-10
Estimated Expiration
2042-08-24

AI Technical Summary

Technical Problem

Existing methods for preparing nanocellulose-based elastomers are time-consuming and not suitable for large-scale production. Furthermore, the adsorption properties of cellulose nanofibers deteriorate after lignin removal, limiting their application areas.

Method used

A composite elastomer with an interwoven structure of wood-based nanocellulose and polymer microspheres is prepared by mechanical dispersion and drying methods, including freeze-drying and supercritical drying, and combined with an organosilicon curing agent to form a porous nanocellulose composite elastomer.

Benefits of technology

The prepared nanocellulose composite elastomer has excellent elasticity, low density, high porosity and large specific surface area, making it suitable for large-scale production and application in fields such as adsorption separation, crude oil recovery and sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117659730B_ABST
    Figure CN117659730B_ABST
Patent Text Reader

Abstract

This invention provides a nanocellulose composite elastomer and its preparation method. The composite elastomer has multiple fiber layers connected to each other. The fiber layers are derived from lignocellulose nanoparticles and polymer microspheres, with the polymer microspheres dispersed within the composite elastomer. The lignocellulose nanoparticles have an interwoven structure formed by their interlocking and entanglement. The nanocellulose composite elastomer of this invention exhibits excellent elasticity and possesses superior properties such as low density, high porosity, and large specific surface area. The preparation method of the nanocellulose composite elastomer of this invention is simple and easy to implement, using readily available raw materials, and is time-efficient, making it suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a nanocellulose composite elastomer and its preparation method, belonging to the field of wood applications. Background Technology

[0002] With the continuous development of human society, people's demand for energy and materials is increasing. The large-scale use of traditional fossil fuels has led to serious environmental problems, making the research on renewable resources particularly important. As petrochemical resources are depleted and environmental problems become increasingly prominent, people's concepts of social development are changing. In order to achieve the goal of green and low-carbon energy transition as soon as possible, we can focus on woody forest products that can sequester carbon.

[0003] Lignocellulose mainly comprises cellulose, hemicellulose, and lignin. Cellulose nanofibers, prepared from cellulose, possess excellent properties such as high aspect ratio, large specific surface area, and good mechanical properties. Nanofiber materials weigh only 1 / 5 the weight of steel, but have five times the specific strength. Due to their numerous superior properties, nanofiber materials are widely used in packaging, food additives, polymer reinforcement, and catalytic energy storage materials. Cellulose nanofibers with diameters below 100 nm can be prepared through chemical pretreatment and mechanical exfoliation. In this preparation process, lignin is usually removed chemically as an unfavorable component that hinders fibrillation. However, removing lignin reduces the adsorption performance of cellulose nanofibers, limiting their application areas.

[0004] Nanocellulose materials are a class of renewable, high aspect ratio nanomaterials with high mechanical properties. They are widely found in plant cell walls and can also be prepared through microbial fermentation. The surface of nanocellulose has abundant chemically reactive groups that can be functionalized, and it also plays a role in stabilizing Pickering emulsions. Porous elastomers prepared using high aspect ratio as a framework possess excellent properties such as low density, high porosity, and large specific surface area, showing promising application prospects in fields such as adsorption separation, crude oil recovery, sensors, and piezoelectric materials.

[0005] The current preparation of nanocellulose-based elastomers relies heavily on ice template technology, which involves constructing anisotropic porous structures by controlling the freezing rate and ice crystal growth direction, ultimately endowing nanocellulose-based materials with a certain degree of elasticity. By setting a unidirectional temperature gradient, nanocellulose-based elastic porous materials with a honeycomb pore structure can be prepared; by setting a bidirectional temperature gradient, nanocellulose-based elastomers with a layered pore structure can be prepared. However, ice template technology is time-consuming and not suitable for the preparation of large-scale samples.

[0006] Reference 1 discloses a polydiorganosiloxane composition and its method of use in forming wood-plastic composites. The composition for preparing wood-plastic composite articles comprises: 15% to 70% by weight of (a) a lignocellulose-based filler; 29.5% to 84.5% by weight of (b) a vinyl polymer; 0.5% to 6% by weight of polydimethylsiloxane; and 0% to 4% by weight of (d) a maleicated vinyl polymer, each based on the combined weight of the starting materials (a), (b), (c), and (d) in the composition. This wood-plastic composite cannot be used to prepare an elastomer.

[0007] Reference 2 discloses a nanocellulose-dispersion concentrate and masterbatch, a method for manufacturing and using the same, and a composite material containing nanocellulose. The nanocellulose-dispersion concentrate comprises: (a) from about 5 wt% to about 90 wt% nanocellulose; and (b) a selected dispersant / drying agent from about 5 wt% to about 95 wt% for compatibility with said nanocellulose, wherein said dispersant / drying agent is selected from the group consisting of: waxes, polyolefins, olefin-maleic anhydride copolymers, olefin-acrylic acid copolymers, polyols, fatty acids, fatty alcohols, polyol-glycerides, polydimethylsiloxane, polydimethylsiloxane-alkyl esters, polyacrylamide, starch, cellulose derivatives, microparticles, and combinations thereof or reaction products, and wherein said nanocellulose-dispersion concentrate is in solid or liquid form. This nanocellulose-dispersion concentrate is also not suitable for use in an elastomer.

[0008] References:

[0009] Reference 1: CN114174437A

[0010] Reference 2: CN113557267A Summary of the Invention

[0011] The problem the invention aims to solve

[0012] In view of the technical problems existing in the prior art, the present invention first provides a nanocellulose composite elastomer with excellent properties such as low density, high porosity and large specific surface area, which has excellent elasticity.

[0013] Furthermore, the present invention provides a method for preparing nanocellulose composite elastomers, which is simple and easy to implement, uses readily available raw materials, is time-efficient, and is suitable for large-scale production.

[0014] Solution for solving the problem

[0015] This invention first provides a composite elastomer, wherein the composite elastomer has a plurality of fiber layers, the fiber layers are connected to each other, and...

[0016] The fiber layer is derived from lignocellulose nanoparticles and polymer microspheres, with the polymer microspheres dispersed within the composite elastomer; wherein...

[0017] The woody nanocellulose has an interwoven structure formed by the woody nanocellulose intertwining and entanglement.

[0018] According to the composite elastomer of the present invention, the composite elastomer has a plurality of pore structures, the average pore size of the composite elastomer is 1µm to 500µm, and the specific surface area of ​​the composite elastomer is 50-500 m². 2 / g.

[0019] According to the composite elastomer of the present invention, the content of carbon atoms is 25-35%, the content of oxygen atoms is 55-75%, and the content of silicon atoms is 1-10%, based on the total mass of the composite elastomer as 100%.

[0020] According to the composite elastomer of the present invention, the lignocellulose nanofibers comprise cellulose, hemicellulose, and lignin; wherein,

[0021] The cellulose content is 50% or more, the hemicellulose content is 10% or less, and the lignin content is 20% or less.

[0022] According to the composite elastomer of the present invention, the polymer microspheres are derived from organosilicon and organosilicon curing agent, preferably, the organosilicon includes polydimethylsiloxane.

[0023] The present invention also provides a method for preparing a composite elastomer according to the present invention, which includes the following steps:

[0024] Lignocellulose nanoparticles and polymer microspheres were dispersed in a solvent to obtain a mixed dispersion;

[0025] The mixed dispersion is dried and then cured to obtain a composite elastomer.

[0026] According to the preparation method of the present invention, the preparation method of the mixed dispersion includes the following steps:

[0027] The lignocellulose nanoparticles were dispersed in a solvent to obtain a lignocellulose nanoparticle suspension;

[0028] Organosilicon and organosilicon curing agent are dispersed in the wood-based nanocellulose dispersion, and after mechanical treatment, a mixed dispersion containing polymer microspheres is obtained.

[0029] According to the preparation method of the present invention, the solid content of lignocellulose nanoparticles in the mixed dispersion is 0.001-1 wt%; and / or the solid content of polymer microspheres in the mixed dispersion is 0.1-2 wt%.

[0030] According to the preparation method of the present invention, the drying includes freeze drying and / or supercritical drying;

[0031] Preferably, the freeze-drying includes drying for 12 h to 48 h in an environment with a vacuum degree of 0.1 μPa to 10 Pa and a temperature of -65 ℃ to -30 ℃;

[0032] The supercritical drying process involves introducing liquid carbon dioxide and performing supercritical drying for 1 h to 24 h at a temperature of 10℃ to 60℃ and a pressure of 1MPa to 30MPa.

[0033] According to the preparation method of the present invention, the curing includes heat curing; preferably, the heating temperature is 60-120°C and the heating time is 0.5-5 hours.

[0034] The effects of the invention

[0035] The nanocellulose composite elastomer of the present invention exhibits excellent elasticity and possesses superior properties such as low density, high porosity, and large specific surface area.

[0036] The preparation method of the nanocellulose composite elastomer of the present invention is simple and easy to implement, the raw materials are readily available, the preparation time is short, and it is suitable for large-scale production. Attached Figure Description

[0037] Figure 1 An electron microscope image of the composite elastomer of Embodiment 1 of the present invention is shown;

[0038] Figure 2 The X-ray photoelectron spectrum of the composite elastomer of Embodiment 2 of the present invention is shown;

[0039] Figure 3 A schematic diagram of the compressive strength of the composite elastomer of Embodiment 3 of the present invention is shown. Detailed Implementation

[0040] The present invention will now be described in detail. The descriptions of the technical features described below are based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:

[0041] In this specification, the range of values ​​referred to as "value A to value B" refers to the range including the endpoint values ​​A and B.

[0042] Unless otherwise stated, in this instruction manual, "more" in "multiple", "various", "multiple", etc., means a value of 2 or more.

[0043] In this specification, the terms “approximately,” “substantially,” “largely,” or “substantially” mean that the error is less than 5%, or less than 3%, or less than 1% compared to the relevant perfect or theoretical standard.

[0044] Unless otherwise specified, "%" in this instruction manual refers to the percentage content by mass.

[0045] In this specification, the word "may" has two meanings: to perform a certain process and not to perform a certain process.

[0046] In this instruction manual, when "room temperature" or "room temperature" is used, the temperature can be 10~40℃.

[0047] Unless otherwise specified, the term "water" used in this manual can refer to tap water, distilled water, deionized water, ion-exchange water, high-purity water, purified water, or any other water suitable for use in this field.

[0048] In this specification, "optional" or "optionally" means that the event or situation described below may or may not occur, and the description includes both the scenario in which the event occurs and the scenario in which the event does not occur.

[0049] In this specification, references to "some specific / preferred embodiments," "other specific / preferred embodiments," "implementation," etc., refer to specific elements (e.g., features, structures, properties, and / or characteristics) related to that embodiment, which are included in at least one of the embodiments described herein and may or may not be present in other embodiments. Furthermore, it should be understood that these elements may be combined in any suitable manner in various embodiments.

[0050] <First Aspect>

[0051] A first aspect of the present invention provides a composite elastomer, wherein the composite elastomer has a plurality of fiber layers, the fiber layers being interconnected, and...

[0052] The fiber layer is derived from lignocellulose nanoparticles and polymer microspheres, with the polymer microspheres dispersed within the composite elastomer; wherein...

[0053] The woody nanocellulose has an interwoven structure formed by the woody nanocellulose intertwining and entanglement.

[0054] The nanocellulose composite elastomer of the present invention exhibits excellent elasticity and possesses superior properties such as low density, high porosity, and large specific surface area.

[0055] In some specific embodiments, the composite elastomer has a multiple pore structure, and the average pore size of the composite elastomer is 1µm to 500µm, for example: 10µm, 30µm, 50µm, 80µm, 100µm, 150µm, 200µm, 250µm, 300µm, 350µm, 400µm, 450µm, etc.; the specific surface area of ​​the composite elastomer is 50-500 m². 2 / g, for example 80 m 2 / g、100 m 2 / g、120 m 2 / g, 150 m 2 / g、180 m 2 / g、200 m 2 / g、220 m 2 / g、250m 2 / g、280 m 2 / g、300 m 2 / g、320 m 2 / g、350 m 2 / g、380 m 2 / g、400 m 2 / g、420 m 2 / g、450 m 2 / g、480 m 2 / g etc. When the average pore size of the composite elastomer is 1µm~500µm and the specific surface area is 50-500m², etc. 2 At / g, its elasticity is even better.

[0056] In some specific embodiments, the lignocellulose nanofibers include cellulose nanofibers and cellulose nanocrystals. Both the cellulose nanofibers and cellulose nanocrystals are derived from wood fibers. This invention does not particularly limit the type of wood fiber; it can be any commonly used wood fiber in the art. Examples include: coniferous wood fiber, hardwood fiber, balsa wood fiber, linden fiber, poplar fiber, birch fiber, pine fiber, oak fiber, fir fiber, etc.

[0057] The wood-based nanocellulose of the present invention has an interwoven structure formed by the interlacing and entanglement of the cellulose nanofibers, which makes the composite elastomer of the present invention have excellent mechanical strength.

[0058] Furthermore, in this invention, the lignocellulose nanoparticles comprise cellulose, hemicellulose, and lignin; wherein,

[0059] The cellulose content is above 50%, for example, 50-80%, specifically 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, 72%, 75%, 78%, etc.; the hemicellulose content is below 10%, for example, 0.5-10%, specifically 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, etc.; the lignin content is below 20%, for example, 5-20%, specifically 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, etc. When the cellulose content is above 50%, the hemicellulose content is below 10%, and the lignin content is below 20%, the interfacial compatibility between the polymer microspheres and nanocellulose is improved, which is beneficial for their composite composition.

[0060] In this invention, the polymer microspheres are derived from organosilicon and organosilicon curing agents. This invention emulsifies organosilicon and organosilicon curing agents under mechanical dispersion to produce polymer microspheres. After being combined with nanocellulose, the polymer microspheres are cross-linked and cured by heating, which can increase the elasticity of the composite elastomer.

[0061] Preferably, the organosilicon comprises polydimethylsiloxane, and the curing agent used is a polydimethylsiloxane curing agent compatible with polydimethylsiloxane.

[0062] In some specific embodiments, based on the total mass of the composite elastomer (100%), the carbon atom content is 25-35%, for example: 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, etc.; the oxygen atom content is 55-75%, for example: 57%, 59%, 61%, 63%, 65%, 67%, 69%, 71%, 73%, etc.; and the silicon atom content is 1-10%, for example: 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, etc. When the carbon atom content is 25-35%, the oxygen atom content is 55-75%, and the silicon atom content is 1-10%, the composite elastomer exhibits superior elasticity.

[0063] <Second aspect>

[0064] A second aspect of the present invention provides a method for preparing a composite elastomer according to the first aspect of the present invention, comprising the following steps:

[0065] Lignocellulose nanoparticles and polymer microspheres were dispersed in a solvent to obtain a mixed dispersion;

[0066] The mixed dispersion was dried to obtain a composite elastomer.

[0067] The method for preparing the composite elastomer of the present invention is simple and easy to implement, the raw materials are readily available, and it is suitable for mass production.

[0068] <Preparation of Lignocellulose Nanoparticles>

[0069] The lignocellulose nanoparticles of the present invention can be purchased or prepared by the following preparation method.

[0070] The preparation method of lignocellulose nanoparticles may include the following steps:

[0071] The lignocellulose is ground into powder and then sieved to obtain cellulose powder;

[0072] The cellulose powder is dissolved in a solvent to form a cellulose dispersion;

[0073] The cellulose dispersion was subjected to ultrasonic treatment to obtain the ultrasonically treated product.

[0074] After the ultrasonically treated product was allowed to stand, the supernatant was taken and freeze-dried to obtain lignocellulose nanoparticles.

[0075] In some specific implementations, the sieving can be through a sieve with a mesh size of less than 100, preferably through a sieve with a mesh size of less than 80.

[0076] Furthermore, in the cellulose dispersion, the mass ratio of cellulose powder to solvent is 0.05-2:100; preferably 0.1-1:100, for example: 0.08:100, 0.12:100, 0.08:100, 0.12:100, 0.15:100, 0.18:100, 0.2:100, 0.3:100, 0.5:100, 0.7:100, 1:100, 1.5:100, etc. The present invention does not impose any particular limitation on the solvent; it can be a polar solvent commonly used in the art, such as water.

[0077] In some specific implementations, the output power of ultrasonic treatment can be 600-1200 W, and the working cycle is 1-2 seconds. The working cycle means that ultrasonic treatment is performed for a period of time and then stopped for a period of time. For example, ultrasonic treatment for 0.5 seconds and then stopping for 0.5 seconds constitutes a cycle of 1 second. Of course, ultrasonic treatment for 1 second and then stopping for 1 second can also be performed, resulting in a cycle of 2 seconds.

[0078] Furthermore, in this invention, the purpose of settling is to obtain a supernatant, which is then freeze-dried to obtain lignocellulose nanoparticles.

[0079] Furthermore, in this invention, the lignocellulose nanofibers can be lignocellulose nanofibers.

[0080] <Preparation of Mixed Dispersions>

[0081] In some specific embodiments, the method for preparing the mixed dispersion includes the following steps:

[0082] The lignocellulose nanoparticles were dispersed in a solvent to obtain a lignocellulose nanoparticle dispersion.

[0083] Organosilicon and organosilicon curing agent are dispersed in the wood nanocellulose dispersion. After mechanical treatment, a mixed dispersion containing polymer microspheres is obtained. Mechanical treatment can make the mixed dispersion more uniform.

[0084] The present invention does not impose any particular limitation on the solvent, which can be a polar solvent commonly used in the art, such as water.

[0085] Furthermore, in the mixed dispersion, the solid content of lignocellulose nanoparticles is 0.001-1 wt%, for example: 0.005 wt%, 0.01 wt%, 0.02 wt%, 0.05 wt%, 0.08 wt%, 0.1 wt%, 0.2 wt%, 0.5 wt%, 0.8 wt%, etc.; and / or, in the mixed dispersion, the solid content of polymer microspheres is 0.1-2 wt%, for example: 0.2 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, 1.8 wt%, etc.

[0086] Specifically, the present invention can utilize one or more of the following for mechanical processing: a high-speed disperser, an ultrasonic disruptor, and a high-speed emulsifier.

[0087] When using a high-speed disperser to mechanically treat the mixed dispersion, the rotation speed of the high-speed disperser is 5000~20000 rpm / min, for example: 7000 rpm / min, 9000 rpm / min, 11000 rpm / min, 13000 rpm / min, 15000 rpm / min, 17000 rpm / min, 19000 rpm / min, etc.; the mechanical treatment time is 10~50 min, for example: 10 min, 20 min, 30 min, 40 min, etc.

[0088] When using an ultrasonic disruptor to mechanically treat a mixed dispersion, the power of the ultrasonic disruptor is 800~1500 W, for example: 900W, 1000W, 1100W, 1200W, 1300W, 1400W, etc.; the working cycle is 1~2 s, for example: 1s, 1.5s, etc.; the mechanical treatment time is 0.5~3h, preferably 0.5-1h, for example: 0.8h, 1.5h, 2h, 2.5h, 2.8h, etc. The working cycle means that ultrasonic treatment is performed for a period of time and then stopped for a period of time. For example, ultrasonic treatment for 0.5s and then stopping for 0.5s constitutes a cycle of 1s. Alternatively, ultrasonic treatment for 1s and then stopping for 1s constitutes a cycle of 2s.

[0089] When using a high-speed emulsifier to mechanically process the mixed dispersion, the rotation speed of the high-speed emulsifier is 5000~20000 rpm / min, for example: 7000 rpm / min, 9000 rpm / min, 11000 rpm / min, 13000 rpm / min, 15000 rpm / min, 17000 rpm / min, 19000 rpm / min, etc.; the mechanical processing time is 5~40 min, for example: 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, etc.

[0090] dry

[0091] After mechanical processing, the mixed dispersion can be dried to obtain a dried product. Specifically, the mixed dispersion can be washed to neutrality using a polar solvent, such as water or an alcohol solvent, to facilitate subsequent drying. Furthermore, if water was used to wash the mixed dispersion before drying, an alcohol solvent can be used for further washing to displace the solvent and facilitate drying.

[0092] In some specific implementations, the drying includes one or a combination of two or more of freeze drying or supercritical drying.

[0093] For freeze drying, in this invention, the freeze drying includes drying for 12 h to 48 h, for example, 15 h, 20 h, 25 h, 30 h, 35 h, 40 h, 45 h, etc., at a vacuum degree of 0.1 μPa to 10 Pa, such as 10 μPa, 100 μPa, 200 μPa, 500 μPa, 700 μPa, 1 mPa, 5 mPa, 10 mPa, 5 mPa, 10 mPa, 5 mPa, 100 mPa, 200 mPa, 500 mPa, 800 mPa, 1 Pa, 10 Pa, etc., and at a temperature of -65 ℃ to -30 ℃, such as -62 ℃, -60 ℃, -58 ℃, -55 ℃, -52 ℃, -50 ℃, -48 ℃, etc.

[0094] For supercritical drying, in this invention, the supercritical drying includes introducing liquid carbon dioxide and conducting supercritical drying for 0.5 h to 24 h at a temperature of 10 ℃ to 60 ℃, for example: 20 ℃, 30 ℃, 40 ℃, 50 ℃, and pressurizing to 1 MPa to 30 MPa, for example: 2 MPa, 5 MPa, 8 MPa, 10 MPa, 12 MPa, 15 MPa, 18 MPa, 20 MPa, 22 MPa, 25 MPa, 28 MPa, etc., for example: 2 h, 5 h, 8 h, 10 h, 12 h, 15 h, 18 h, 20 h, 22 h, etc. The boost rate can be 0.5-5 MPa / min, for example: 1 MPa / min, 1.5 MPa / min, 2 MPa / min, 2.5 MPa / min, 3 MPa / min, 3.5 MPa / min, 4 MPa / min, 4.5 MPa / min, etc.

[0095] Furthermore, during supercritical drying, the process can be repeated 3 to 5 times to obtain the desired dried product. Additionally, after drying, pressure is released at a rate of 0.1 to 1.5 MPa / min, such as 0.2 MPa / min, 0.4 MPa / min, 0.6 MPa / min, 0.8 MPa / min, 1.0 MPa / min, 1.2 MPa / min, 1.4 MPa / min, etc.

[0096] Furthermore, the dried product is cured to obtain a composite elastomer. Preferably, curing can be carried out by heating. Specifically, the heating temperature is 60-120℃, such as 70℃, 80℃, 90℃, 100℃, 110℃, etc.; the heating time is 0.5-5 hours, such as 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, etc.

[0097] Example

[0098] The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer are followed. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0099] Example 1

[0100] (1) Grind lignocellulose into powder using a high-speed grinder and pass it through a 60-mesh sieve. Add 1g of cellulose powder to 400mL of distilled water to form a cellulose dispersion. Place the dispersion into a high-frequency ultrasonic disruptor for ultrasonic treatment. The output power is 900W, the working cycle is 1s (0.5s ultrasonic, 0.5s pause), and the ultrasonic duration is 30min. After ultrasonication, let the sample dispersion stand overnight, take the supernatant and freeze-dry it to obtain cellulose nanofiber material.

[0101] (2) Prepare 200 mL of cellulose nanofiber dispersion with a solid content of 0.5 wt% using cellulose nanofiber material.

[0102] (3) Add 1g of polydimethylsiloxane (PDMS) and 0.1g of polydimethylsiloxane curing agent (Dow Corning DC184 PDMS curing agent) to the cellulose nanofiber dispersion, and treat the mixed solution for 30 min using a high-speed disperser (speed: 10000 rpm / min) to obtain a mixed dispersion containing polymer microspheres (solid content 0.5 wt%).

[0103] (4) The mixed dispersion was placed in a freezer at -18°C for 12 h, and then the sample was transferred to a freeze dryer at -50°C and 10 mPa vacuum for 48 h to freeze dry the product.

[0104] (5) Place the dried product in a forced-air drying oven and heat it at 100 °C for 1 hour to promote PDMS curing and finally obtain the composite elastomer.

[0105] Example 2

[0106] (1) Prepare 200 mL of cellulose nanofiber dispersion with a solid content of 0.2 wt% using cellulose nanofibers (cellulose nanofibers were purchased from Wood Elf Biotechnology Co., Ltd., with a solid content of 2 wt%).

[0107] (2) Add 0.5 g of polydimethylsiloxane (PDMS) and 0.05 g of polydimethylsiloxane curing agent (Dow Corning DC184 PDMS curing agent) to the cellulose nanofiber dispersion, and then treat the mixed solution with a high-frequency ultrasonic disruptor for 1 h (output power 1000W, working cycle 1s, ultrasonic 0.5s, stop 0.5s) to obtain a mixed dispersion containing polymer microspheres (solid content 0.25%).

[0108] (3) The mixed dispersion was replaced with tert-butanol for 4 hours. The replaced sample was placed in liquid nitrogen for freezing, and then transferred to a freeze dryer with a temperature of -50℃ and a vacuum of 10 mPa for freeze drying for 36 hours to obtain the dried product.

[0109] (4) Place the dried product in an oven and treat it at 80°C for 3 hours to obtain the composite elastomer.

[0110] Example 3

[0111] (1) Prepare 100 mL of cellulose nanofiber dispersion with a solid content of 0.2 wt% using cellulose nanofibers (cellulose nanofibers were purchased from Wood Elf Biotechnology Co., Ltd., with a solid content of 2 wt%).

[0112] (2) Add 0.5 g PDMS and 0.05 g curing agent to the cellulose nanofiber dispersion. Treat the sample with a high-speed emulsifier at 12000 rpm for 20 min to obtain a mixed dispersion containing polymer microspheres (solid content 0.5 wt%).

[0113] (3) Pour the mixed dispersion into a dialysis bag and replace the solution with anhydrous ethanol. Replace the anhydrous ethanol every 3 hours for a total of three times. Dispense the replaced sample into a mold.

[0114] The replaced sample was placed in the pressure chamber of a supercritical dryer, liquid CO2 was poured in, the chamber temperature was set to 45 ℃, the pressure increase rate was 2 MPa / min, and the pressure was increased to 10 MPa for supercritical CO2 drying. After 2 h, the pressure was released. The above process was repeated 3 times, with a pressure release rate of 0.8 MPa / min, to obtain the dried product.

[0115] (4) Place the dried product into an oven and heat it to 100°C for 2 hours to obtain the composite elastomer.

[0116] Performance testing

[0117] 1. Content of lignin, cellulose, and hemicellulose in cellulose nanofibers

[0118] The contents of cellulose, hemicellulose, and lignin in cellulose nanofibers were determined according to the national standard GB / T35818-2018: Analysis Methods for Forestry Biomass Raw Materials - Determination of Polysaccharide and Lignin Content. The test results are shown in Table 1 below.

[0119] Table 1

[0120]

[0121] 2. Specific surface area and average pore size testing of composite elastomers

[0122] The specific surface area and pore size distribution of the composite elastomer were determined and calculated using a Bestar 3H-2000BET-A specific surface area analyzer. The results are shown in Table 1 below.

[0123] Table 2

[0124]

[0125] 3. Electron microscopy characterization

[0126] The composite elastomer obtained in Example 1 was characterized by scanning electron microscopy, and the results are as follows: Figure 1 As shown.

[0127] Depend on Figure 1 It can be seen that there are large pores in the composite elastomer, and polydimethylsiloxane is dispersed in the material in the form of microspheres.

[0128] 4. X-ray photoelectron spectroscopy characterization

[0129] The composite elastomer obtained in Example 2 was characterized by X-ray photoelectron spectroscopy, and the results are as follows: Figure 2 As shown. Figure 2 It can be seen that in addition to C and O elements, the composite elastomer material also shows the characteristic peak of Si element, indicating that polydimethylsiloxane was successfully composited inside the composite elastomer. The C atom content is 30.2 wt%, the O atom content is 62.37 wt%, and the Si atom content is 4.2 wt%.

[0130] 5. Compression strength test

[0131] The compressive strength of the composite elastomer obtained in Example 3 was tested using a universal testing machine. Specifically, a 15 mm square composite elastomer was placed in the center of a compression fixture, the maximum compressive strain was set to 50%, and the compression rate was 5 mm / min. The test results are as follows: Figure 3 As shown.

[0132] Depend on Figure 3It can be seen that the material still maintains good elasticity under 50% compressive strain.

[0133] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or technical improvements to the embodiments in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.

Claims

1. A composite elastomer, characterized in that, The composite elastomer has multiple fiber layers, which are connected to each other, and... The fiber layer is derived from lignocellulose nanoparticles and polymer microspheres, with the polymer microspheres dispersed within the composite elastomer; wherein... The wood-based nanocellulose has an interwoven structure formed by the wood-based nanocellulose intertwining and entanglement; The composite elastomer has a multiple pore structure, with an average pore size of 1µm to 500µm; the specific surface area of ​​the composite elastomer is 50-500 m². 2 / g; The polymer microspheres are derived from organosilicon and organosilicon curing agents; The lignocellulose nanoparticles comprise cellulose, hemicellulose, and lignin; wherein, The cellulose content is 50% or more, the hemicellulose content is 10% or less, and the lignin content is 20% or less.

2. The composite elastomer according to claim 1, characterized in that, Based on the total mass of the composite elastomer as 100%, the content of carbon atoms is 25-35%, the content of oxygen atoms is 55-75%, and the content of silicon atoms is 1-10%.

3. The composite elastomer according to claim 1 or 2, characterized in that, The organosilicon includes polydimethylsiloxane.

4. A method for preparing a composite elastomer according to any one of claims 1-3, characterized in that, Includes the following steps: Lignocellulose nanoparticles and polymer microspheres were dispersed in a solvent to obtain a mixed dispersion; The mixed dispersion is dried and then cured to obtain a composite elastomer.

5. The preparation method according to claim 4, characterized in that, The method for preparing the mixed dispersion includes the following steps: The lignocellulose nanoparticles were dispersed in a solvent to obtain a lignocellulose nanoparticle suspension; Organosilicon and organosilicon curing agent are dispersed in the wood-based nanocellulose dispersion, and after mechanical treatment, a mixed dispersion containing polymer microspheres is obtained.

6. The preparation method according to claim 5, characterized in that, In the mixed dispersion, the solid content of lignocellulose nanoparticles is 0.001-1 wt%; and / or, in the mixed dispersion, the solid content of polymer microspheres is 0.1-2 wt%.

7. The preparation method according to any one of claims 4-6, characterized in that, The drying process includes freeze drying and / or supercritical drying.

8. The preparation method according to claim 7, characterized in that, The freeze-drying process includes drying for 12 h to 48 h in an environment with a vacuum of 0.1 μPa to 10 Pa and a temperature of -65℃ to -30℃. The supercritical drying process involves introducing liquid carbon dioxide and performing supercritical drying for 1 h to 24 h at a temperature of 10℃ to 60℃ and a pressure of 1 MPa to 30 MPa.

9. The preparation method according to any one of claims 4-6, characterized in that, The curing includes heat curing.

10. The preparation method according to claim 9, characterized in that, The heating temperature is 60-120℃, and the heating time is 0.5-5 hours.

Citation Information

Patent Citations

  • Polydiorganosiloxane compositions and methods of use thereof in forming wood-plastic composites

    CN114174437A

  • Preparation method of nanocellulose and polymer composite aerogel

    CN106117592A

  • Micro-nano lignocellulose, preparation method and applications thereof

    CN110055796A

  • Hyper-elastic 3D printing nano cellulose composite material and preparation method thereof

    CN112920538A

  • Nanocellulose-dispersion concentrates and masterbatches, methods of making and using the same, and nanocellulose-containing composites