Solid polymer electrolyte and preparation method thereof, and application in secondary battery
By using solid polymer electrolyte with a mesh structure in lithium-ion batteries, combining the oxidation products of aromatic diamines and graphene, the problems of high impedance and low rate performance in solid electrolytes are solved, and higher energy density and Security.
Patent Information
- Application Number
- CN202311645276.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-12-01
AI Technical Summary
The solid electrolytes in existing lithium-ion batteries have problems such as high impedance and low rate performance, which is difficult to meet the needs of high capacity and high safety performance.
Using solid polymer electrolyte with a network structure, a copolymer of vinyl carbonate and polyethylene glycol diacrylate is used as a polymer matrix, combining the oxidation product of aromatic diamine and graphene to form high conductivity and mechanical strength The electrolyte is filled in the mesh structure to improve the rate performance and safety performance of the secondary battery.
It significantly improves the rate performance of the secondary battery, reduces the battery impedance, improves the cycle performance and safety performance, and avoids structural damage of the battery during the cycle.
Smart Images

Figure CN117673461B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of material preparation, and in particular to a solid polymer electrolyte and a preparation method thereof, and application of the solid polymer electrolyte in a secondary battery. Background Art
[0002] With the shortage of social energy and the promotion of low-carbon development, new energy vehicles have become one of the future development directions of the automotive industry. The core component of new energy vehicles is the power battery. As a power battery that has developed rapidly in recent years, lithium-ion batteries have the characteristics of large specific energy, no pollution, high working voltage and long cycle life, and have received widespread attention in the new energy vehicle industry. However, problems such as slow charging speed and short driving range of lithium-ion batteries for automobiles still exist. In order to solve this problem, the industry uses ternary materials as positive electrode materials. At present, the electrolyte corresponding to this type of material generally uses liquid electrolytes. The electrolyte in the ternary material system is prone to violent combustion, which poses serious safety problems.
[0003] Based on the demand for high-capacity and high-safety lithium-ion batteries, the industry has turned its attention to solid-state batteries. By using solid electrolytes instead of liquid electrolytes, the safety is improved while the energy density is increased. However, the current solid electrolytes used in lithium-ion batteries generally have high battery impedance, and battery-related performance such as internal resistance and rate performance are lower than that of liquid electrolytes.
[0004] Therefore, there is an urgent need for a new solid electrolyte or its preparation method that can further improve the rate, reduce impedance, etc. while meeting the needs of high-capacity and high-safety lithium-ion batteries. Summary of the invention
[0005] The purpose of the present invention is to provide a solid polymer electrolyte and a preparation method thereof, and application in a secondary battery. The solid polymer electrolyte has a network structure, has a large number of ion conduction channels, and has a high conductivity. When applied to a secondary battery, it can improve the rate performance of the secondary battery and reduce impedance.
[0006] To achieve the above-mentioned objectives, the present invention provides a solid polymer electrolyte on the one hand, comprising a polymer matrix having a network structure, an oxidation product of an aromatic diamine and graphene, wherein the oxidation product of the aromatic diamine and the graphene are filled in the network structure, and the polymer matrix is a copolymer of vinylene carbonate and polyethylene glycol diacrylate.
[0007] In the technical solution adopted by the present invention, the polymer matrix composed of the copolymer of vinylene carbonate and polyethylene glycol diacrylate has a mesh structure, which increases the conduction channel of the solid polymer electrolyte, and the introduction of nitrogen atoms in the oxidation product of aromatic diamine can improve the rate performance of the secondary battery. Graphene can not only improve the conductivity of the solid polymer electrolyte and reduce the battery impedance, but also fill it in the mesh structure to make the solid polymer electrolyte have a certain mechanical strength, preventing the structural damage during the battery cycle and causing the cycle performance and safety performance of the secondary battery to decrease. Therefore, the solid polymer electrolyte of the present invention includes a polymer matrix with a mesh structure, the oxidation product of aromatic diamine and graphene, which can not only improve the safety performance of the secondary battery but also further improve the rate, cycle and other performances.
[0008] As a technical solution of the present invention, the aromatic diamine includes at least one of o-phenylenediamine, m-phenylenediamine and p-phenylenediamine.
[0009] As a technical solution of the present invention, the mass ratio of the polymer matrix, the oxidation product of the aromatic diamine and the graphene is 4-6:3-5:1.
[0010] The second aspect of the present invention provides a method for preparing a solid polymer electrolyte, comprising the steps of: mixing vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide, adding an initiator and polymerizing at 45-60° C. for 2-12 hours.
[0011] In the preparation method of the solid polymer electrolyte of the present invention, vinylene carbonate (VC) is used as a polymerization monomer and polyethylene glycol diacrylate is used as a long-chain crosslinking agent, so that vinylene carbonate can form an elastic gel state after polymerization and construct a network structure. Graphene oxide is used as a raw material to be reduced to obtain graphene, which can avoid the problem that graphene is easy to agglomerate and difficult to disperse when it is directly used as a raw material. Aromatic diamine can not only assist vinylene carbonate in polymerizing to form an elastic gel state and construct a porous network structure at the microscopic level, but also reduce graphene oxide and enable it to participate in the construction of the porous network structure of the solid electrolyte.
[0012] As a technical solution of the present invention, the mass ratio of the vinylene carbonate, the aromatic diamine, the polyethylene glycol diacrylate and the graphene oxide is 0.5-2:3-5:3-5:0.5-2.
[0013] As a technical solution of the present invention, based on the sum of the masses of the vinylene carbonate, the aromatic diamine, the polyethylene glycol diacrylate and the graphene oxide being 100%, the mass of the initiator is 0.1-1.0%.
[0014] As a technical solution of the present invention, the initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.
[0015] The third aspect of the present invention provides a solid polymer electrolyte or the use of the solid polymer electrolyte prepared by the above-mentioned method for preparing the solid polymer electrolyte in a secondary battery.
[0016] A fourth aspect of the present invention provides a method for preparing a secondary battery, comprising the steps of:
[0017] (1) Preparation of battery cells
[0018] (2) Preparation of electrolyte
[0019] After vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide are mixed, an initiator is added to obtain a premix, and the premix is mixed with a liquid electrolyte to obtain an electrolyte;
[0020] (3) The battery cell is packaged in a package, injected with the electrolyte and then sealed, and after activation, a polymerization reaction is carried out at 45 to 60° C. for 2 to 12 hours, and then chemical formation is carried out.
[0021] The secondary battery of the present invention adopts a mixture of a solid polymer electrolyte and a liquid electrolyte as the electrolyte, which not only has better safety and higher energy density, but also has better cycle and rate performance of the secondary battery.
[0022] As a technical solution of the present invention, the mass ratio of the premix to the liquid electrolyte is 1 to 9:1. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 These are EIS graphs obtained through impedance testing of the semi-solid batteries of Examples 1 to 3 and Comparative Examples 1 to 4. DETAILED DESCRIPTION
[0024] The solid polymer electrolyte of the present invention comprises a polymer matrix with a mesh structure, an oxidation product of an aromatic diamine and graphene. The oxidation product of the aromatic diamine and the graphene are filled in the mesh structure, and the polymer matrix is a copolymer of vinylene carbonate and polyethylene glycol diacrylate. The aromatic diamine comprises at least one of o-phenylenediamine, m-phenylenediamine and p-phenylenediamine. The mass ratio of the polymer matrix, the oxidation product of the aromatic diamine and the graphene is 4-6:3-5:1.
[0025] The solid polymer electrolyte of the present invention can be applied to an all-solid-state secondary battery. For an all-solid-state secondary battery, an electrolyte salt and a solid polymer electrolyte can be added and mixed to form an all-solid electrolyte, and the electrolyte salt can be, but is not limited to, LiPF6, LiTFSI, LiClO4, LiAsF4, LiBF4, etc. The preparation method of the all-solid-state secondary battery may include the following steps.
[0026] (1) Preparation of solid polymer electrolyte
[0027] After vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide are mixed, an initiator is added and polymerized at 45-60° C. for 2-12 hours. The mass ratio of vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide is 0.5-2:3-5:3-5:0.5-2. The mass of the initiator is 0.1-1.0% based on the sum of the mass of vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide as 100%. The initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.
[0028] (2) Preparation of battery cells
[0029] A battery cell can be obtained by stacking and winding a positive electrode sheet, an all-solid electrolyte (a mixture of electrolyte salt and solid polymer electrolyte) and a negative electrode sheet in sequence, or by stacking a positive electrode sheet, an all-solid electrolyte (a mixture of electrolyte salt and solid polymer electrolyte) and a negative electrode sheet in sequence to obtain a single stacked body, and then stacking multiple stacked bodies to obtain a battery cell.
[0030] (3) The battery cells are packaged in a sealed package and then activated and then chemically formed.
[0031] The solid polymer electrolyte of the present invention can also be mixed with a liquid electrolyte to be used as an electrolyte in a semi-solid secondary battery.
[0032] For semi-solid secondary batteries, it refers to a mixture of solid polymer electrolyte and liquid electrolyte as a semi-solid secondary battery, and the solid polymer electrolyte is mainly in the body. The mass ratio of solid polymer electrolyte to liquid electrolyte can be 1 to 9:1. The liquid electrolyte usually includes an electrolyte salt and a non-aqueous organic solvent. The electrolyte salt can be, but is not limited to, LiPF6, LiTFSI, LiClO4, LiAsF4, LiBF4, etc. The non-aqueous organic solvent is at least one of a chain carbonate, a cyclic carbonate and a carboxylic acid ester. Further, the non-aqueous organic solvent is selected from at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propyl propionate, ethyl propionate, ethyl butyrate, difluoroethyl acetate and ethyl 2,2,2-trifluoroacetate.
[0033] The method for preparing the semi-solid secondary battery may include the following steps.
[0034] A method for preparing a secondary battery, characterized in that it comprises the steps of:
[0035] (1) Preparation of battery cells
[0036] The positive electrode sheet, the separator and the negative electrode sheet are sequentially stacked and wound to obtain a battery cell, or the positive electrode sheet, the separator and the negative electrode sheet are sequentially stacked to obtain a single stacked body, and then a plurality of stacked bodies are stacked to obtain a battery cell.
[0037] (2) Preparation of electrolyte
[0038] After vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide are mixed, an initiator is added to mix to obtain a premix, and the premix and a liquid electrolyte are mixed to obtain an electrolyte. The mass ratio of vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide is 0.5-2:3-5:3-5:0.5-2. The mass of the initiator is 0.1-1.0% based on the sum of the mass of vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide as 100%. The initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.
[0039] (3) The battery cell is packaged in a package and the electrolyte is injected and then sealed. After activation, a polymerization reaction is carried out at 45 to 60° C. for 2 to 12 hours, and then chemical formation is carried out.
[0040] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.
[0041] Example 1
[0042] This embodiment is a solid polymer electrolyte. It includes a polymer matrix with a mesh structure, an oxidation product of o-phenylenediamine and graphene in a mass ratio of 5:4:1, and the oxidation product of o-phenylenediamine and graphene are filled in the mesh structure. The polymer matrix is a copolymer of vinylene carbonate and polyethylene glycol diacrylate.
[0043] The solid polymer electrolyte is used in a semi-solid secondary battery. The preparation method of the secondary battery includes the following steps.
[0044] (1) Preparation of battery cells
[0045] A battery cell can be produced by stacking and winding the positive electrode sheet, the isolation film and the negative electrode sheet in sequence.
[0046] (2) Preparation of electrolyte
[0047] After mixing vinylene carbonate, o-phenylenediamine, polyethylene glycol diacrylate and graphene oxide in a mass ratio of 1:4:4:1, azobisisobutyronitrile (accounting for 0.5% of the sum of the masses of the first four substances) is added to obtain a premix, and the premix and a liquid electrolyte are mixed to obtain an electrolyte, and the mass ratio of the premix and the liquid electrolyte is 5:1.
[0048] (3) The battery cell is packaged in an aluminum-plastic film and sealed after injecting electrolyte. After activation, a polymerization reaction is carried out at 50° C. for 8 hours, and then chemical formation is carried out.
[0049] Example 2
[0050] This embodiment is a solid polymer electrolyte. It includes a polymer matrix with a mesh structure, an oxidation product of m-phenylenediamine and graphene in a mass ratio of 5:4:1, and the oxidation product of m-phenylenediamine and graphene are filled in the mesh structure. The polymer matrix is a copolymer of vinylene carbonate and polyethylene glycol diacrylate.
[0051] The solid polymer electrolyte is used in a semi-solid secondary battery. The preparation method of the secondary battery includes the following steps.
[0052] (1) Preparation of battery cells
[0053] A battery cell can be produced by stacking and winding the positive electrode sheet, the isolation film and the negative electrode sheet in sequence.
[0054] (2) Preparation of electrolyte
[0055] After mixing vinylene carbonate, m-phenylenediamine, polyethylene glycol diacrylate and graphene oxide in a mass ratio of 1:4:4:1, azobisisobutyronitrile (accounting for 0.5% of the sum of the masses of the first four substances) is added to obtain a premix, and the premix and a liquid electrolyte are mixed to obtain an electrolyte, and the mass ratio of the premix and the liquid electrolyte is 5:1.
[0056] (3) The battery cell is packaged in an aluminum-plastic film and sealed after injecting electrolyte. After activation, a polymerization reaction is carried out at 50° C. for 8 hours, and then chemical formation is carried out.
[0057] Example 3
[0058] This embodiment is a solid polymer electrolyte. It includes a polymer matrix with a mesh structure, an oxidation product of o-phenylenediamine and graphene in a mass ratio of 6:3:1, and the oxidation product of o-phenylenediamine and graphene are filled in the mesh structure. The polymer matrix is a copolymer of vinylene carbonate and polyethylene glycol diacrylate.
[0059] The solid polymer electrolyte is used in a semi-solid secondary battery. The preparation method of the secondary battery includes the following steps.
[0060] (1) Preparation of battery cells
[0061] A battery cell can be produced by stacking and winding the positive electrode sheet, the isolation film and the negative electrode sheet in sequence.
[0062] (2) Preparation of electrolyte
[0063] After mixing vinylene carbonate, o-phenylenediamine, polyethylene glycol diacrylate and graphene oxide in a mass ratio of 2:3:4:1, azobisisobutyronitrile (accounting for 0.3% of the sum of the masses of the first four substances) is added to obtain a premix, and the premix is mixed with a liquid electrolyte to obtain an electrolyte, and the mass ratio of the premix to the liquid electrolyte is 5:1.
[0064] (3) The battery cell is packaged in an aluminum-plastic film and sealed after injecting electrolyte. After activation, a polymerization reaction is carried out at 55° C. for 7 hours, and then chemical formation is carried out.
[0065] Comparative Example 1
[0066] This comparative example is a solid polymer electrolyte, which includes a polymer matrix with a mesh structure, and the polymer matrix is a copolymer of vinylene carbonate and polyethylene glycol diacrylate.
[0067] The solid polymer electrolyte is used in a semi-solid secondary battery. The preparation method of the secondary battery includes the following steps.
[0068] (1) Preparation of battery cells
[0069] A battery cell can be produced by stacking and winding the positive electrode sheet, the isolation film and the negative electrode sheet in sequence.
[0070] (2) Preparation of electrolyte
[0071] After vinylene carbonate and polyethylene glycol diacrylate are mixed in a mass ratio of 1:4, azobisisobutyronitrile (accounting for 0.5% of the total mass of vinylene carbonate and polyethylene glycol diacrylate) is added to obtain a premix, and the premix and a liquid electrolyte are mixed to obtain an electrolyte, and the mass ratio of the premix and the liquid electrolyte is 5:1.
[0072] (3) The battery cell is packaged in an aluminum-plastic film and sealed after injecting electrolyte. After activation, a polymerization reaction is carried out at 50° C. for 8 hours, and then chemical formation is carried out.
[0073] Comparative Example 2
[0074] This comparative example is a solid polymer electrolyte, which includes a polymer matrix with a mesh structure and graphene in a mass ratio of 5:1, wherein the graphene is filled in the mesh structure. The polymer matrix is a copolymer of vinylene carbonate and polyethylene glycol diacrylate.
[0075] The solid polymer electrolyte is used in a semi-solid secondary battery. The preparation method of the secondary battery includes the following steps.
[0076] (1) Preparation of battery cells
[0077] A battery cell can be produced by stacking and winding the positive electrode sheet, the isolation film and the negative electrode sheet in sequence.
[0078] (2) Preparation of electrolyte
[0079] After mixing vinylene carbonate, polyethylene glycol diacrylate and graphene in a mass ratio of 1:4:1, azobisisobutyronitrile (accounting for 0.5% of the sum of the masses of the first three substances) is added to obtain a premix, and the premix is mixed with a liquid electrolyte to obtain an electrolyte, and the mass ratio of the premix to the liquid electrolyte is 5:1.
[0080] (3) The battery cell is packaged in an aluminum-plastic film and sealed after injecting electrolyte. After activation, a polymerization reaction is carried out at 50° C. for 8 hours, and then chemical formation is carried out.
[0081] Comparative Example 3
[0082] This comparative example is a solid polymer electrolyte, which includes a polymer matrix with a network structure and o-phenylenediamine in a mass ratio of 5:4, wherein the o-phenylenediamine is filled in the network structure. The polymer matrix is a copolymer of vinylene carbonate and polyethylene glycol diacrylate.
[0083] The solid polymer electrolyte is used in a semi-solid secondary battery. The preparation method of the secondary battery includes the following steps.
[0084] (1) Preparation of battery cells
[0085] A battery cell can be produced by stacking and winding the positive electrode sheet, the isolation film and the negative electrode sheet in sequence.
[0086] (2) Preparation of electrolyte
[0087] After vinylene carbonate, o-phenylenediamine and polyethylene glycol diacrylate are mixed in a mass ratio of 1:4:4, azobisisobutyronitrile (accounting for 0.5% of the sum of the masses of the first three substances) is added to obtain a premix, and the premix and a liquid electrolyte are mixed to obtain an electrolyte, and the mass ratio of the premix and the liquid electrolyte is 5:1.
[0088] (3) The battery cell is packaged in an aluminum-plastic film and sealed after injecting electrolyte. After activation, a polymerization reaction is carried out at 50° C. for 8 hours, and then chemical formation is carried out.
[0089] Comparative Example 4
[0090] This embodiment is a solid polymer electrolyte, which includes a polymer matrix with a mesh structure, o-phenylenediamine and graphene in a mass ratio of 5:4:1, wherein the o-phenylenediamine and graphene are filled in the mesh structure. The polymer matrix is a copolymer of vinylene carbonate and polyethylene glycol diacrylate.
[0091] The solid polymer electrolyte is used in a semi-solid secondary battery. The preparation method of the secondary battery includes the following steps.
[0092] (1) Preparation of battery cells
[0093] A battery cell can be produced by stacking and winding the positive electrode sheet, the isolation film and the negative electrode sheet in sequence.
[0094] (2) Preparation of electrolyte
[0095] After mixing vinylene carbonate, o-phenylenediamine, polyethylene glycol diacrylate and graphene in a mass ratio of 1:4:4:1, azobisisobutyronitrile (accounting for 0.5% of the sum of the masses of the first four substances) is added to obtain a premix, and the premix is mixed with a liquid electrolyte to obtain an electrolyte, and the mass ratio of the premix and the liquid electrolyte is 5:1.
[0096] (3) The battery cell is packaged in an aluminum-plastic film and sealed after injecting electrolyte. After activation, a polymerization reaction is carried out at 50° C. for 8 hours, and then chemical formation is carried out.
[0097] The semi-solid secondary batteries prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to electrochemical performance tests. The test conditions were as follows. The test results are shown in Table 1.
[0098] (1) Normal temperature cycle performance test
[0099] Place the semi-solid secondary battery in an environment of 25°C, charge it to 4.2V at a constant current of 1C, then charge it to 0.05C at a constant voltage, and then discharge it to 2.5V at a constant current of 1C. Repeat this cycle, record the discharge capacity of the first cycle and the discharge capacity of the last cycle, and calculate the capacity retention rate of the room temperature cycle according to the following formula.
[0100] Capacity retention rate = discharge capacity of the last cycle / discharge capacity of the first cycle × 100%
[0101] (2) High temperature cycle performance test
[0102] The semi-solid secondary battery was placed in an environment of 45°C, charged at a constant current of 1C to 4.2V, then charged at a constant voltage to a current of 0.05C, and then discharged at a constant current of 1C to 2.5V. The cycle was repeated, and the discharge capacity of the first cycle and the discharge capacity of the last cycle were recorded. The capacity retention rate of the high temperature cycle was calculated according to the following formula.
[0103] Capacity retention rate = discharge capacity of the last cycle / discharge capacity of the first cycle × 100%
[0104] (3) Rate performance test
[0105] The semi-solid secondary battery was charged to 4.2V at a constant current of 0.5C, then charged to a current of 0.05C at a constant voltage, and then discharged to 2.5V at a constant current, and the discharge capacity was recorded as C0. The battery was then charged to 4.2V using the above method, and then discharged at a current of 3C, and the discharge capacity was recorded as C1.
[0106] Capacity retention rate = C1 / C0*100%
[0107] (4) Impedance test
[0108] The semi-solid secondary battery that has just been formed is discharged to a SOC of 50%, and the battery is placed on an electrochemical workstation for EIS testing. The results are as follows: Figure 1 shown.
[0109] Table 1 Cycle and rate test results of Examples 1 to 3 and Comparative Examples 1 to 4
[0110]
[0111] From the results in Table 1, it can be seen that the semi-solid secondary batteries of Examples 1 to 3 have better cycle and rate performance. This is because the introduction of nitrogen atoms in the oxidation products of aromatic diamines can improve the rate performance of the secondary battery, and the filling of graphene in the network structure can make the solid polymer electrolyte have a certain mechanical strength, preventing structural damage during the battery cycle, thereby improving the cycle performance.
[0112] Comparative Documents 1 to 3 lack the oxidation product of aromatic diamine or graphene, so the overall performance of the semi-solid secondary battery is poor. Comparative Example 4 directly uses graphene, which is easy to agglomerate during the preparation process, resulting in poor performance.
[0113] Combination Figure 1 From the results, it can be seen that the impedance values of the semi-solid secondary batteries of Examples 1 to 3 are relatively low. Comparative Examples 1 and 3 do not contain graphene, so the impedance values are relatively high. In Comparative Example 4, graphene agglomerates are difficult to exert their conductive effect in the network structure, so the improvement on impedance is limited.
[0114] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A solid polymer electrolyte, characterized in that The invention comprises a polymer matrix with a network structure, an oxidation product of an aromatic diamine and graphene, wherein the oxidation product of the aromatic diamine and the graphene are filled in the network structure, the polymer matrix is a copolymer of vinylene carbonate and polyethylene glycol diacrylate, and the solid polymer electrolyte is prepared by mixing vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide, adding an initiator and polymerizing at 45 to 60°C for 2 to 12 hours.
2. The solid polymer electrolyte according to claim 1, characterized in that The aromatic diamine includes at least one of o-phenylenediamine, m-phenylenediamine and p-phenylenediamine.
3. The solid polymer electrolyte according to claim 1, characterized in that The mass ratio of the polymer matrix, the oxidation product of the aromatic diamine and the graphene is 4-6:3-5:
1.
4. A method for preparing a solid polymer electrolyte, characterized in that: The method comprises the following steps: mixing vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide, adding an initiator and polymerizing at 45-60° C. for 2-12 hours.
5. The method for preparing a solid polymer electrolyte according to claim 4, characterized in that: The mass ratio of the vinylene carbonate, the aromatic diamine, the polyethylene glycol diacrylate and the graphene oxide is 0.5-2:3-5:3-5:0.5-2.
6. The method for preparing a solid polymer electrolyte according to claim 4, characterized in that: Based on the sum of the masses of the vinylene carbonate, the aromatic diamine, the polyethylene glycol diacrylate and the graphene oxide being 100%, the mass of the initiator is 0.1 to 1.0%.
7. The method for preparing a solid polymer electrolyte according to claim 4, characterized in that: The initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.
8. Use of the solid polymer electrolyte prepared by the solid polymer electrolyte according to any one of claims 1 to 3 or the method for preparing a solid polymer electrolyte according to any one of claims 4 to 7 in a secondary battery.
9. A method for preparing a secondary battery, characterized in that: Includes steps: (1) Preparation of battery cells (2) Preparation of electrolyte After vinylene carbonate, aromatic diamine, polyethylene glycol diacrylate and graphene oxide are mixed, an initiator is added to obtain a premix, and the premix is mixed with a liquid electrolyte to obtain an electrolyte; (3) The battery cell is packaged in a package, injected with the electrolyte and then sealed, and after activation, a polymerization reaction is carried out at 45 to 60° C. for 2 to 12 hours, and then chemical formation is carried out.
10. The method for preparing a secondary battery according to claim 9, characterized in that: The mass ratio of the premix to the liquid electrolyte is 1 to 9:1.