A fiber-coated, composite-coated spring coil and its preparation method

By forming a composite coating of uniform fiber mesh on the surface of the spring coil, the problems of fiber shedding and entanglement are solved, improving the reliability and flexibility of embolization and achieving effective blood flow blocking.

CN117679565BActive Publication Date: 2026-11-10THE FIFTH MEDICAL CENT OF CHINESE PLA GENERAL HOSPITAL
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311692119.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-11
Publication Date
2026-11-10
Estimated Expiration
2043-12-11

AI Technical Summary

Technical Problem

The existing spring coil fibers are prone to falling off or tangling during the conveying process, which affects the embolization effect.

Method used

Using polymers, poloxamer, K-carrageenan, and sodium hyaluronate as raw materials, a uniform fiber web is formed on and around the spring coil through electrostatic spraying, forming a composite coated spring coil, which improves the adhesion and flexibility of the fiber coating.

Benefits of technology

The fiber coating adheres firmly to the surface of the spring coil and is not easy to fall off, which improves the reliability and practicality of embolization. It can absorb water in the blood after delivery to promote coagulation, fully physically embolize, and block blood flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117679565B_ABST
    Figure CN117679565B_ABST
Patent Text Reader

Abstract

This application relates to the technical field of medical devices, specifically disclosing a fiber coating, a composite-coated spring coil, and a method for preparing the same. The fiber coating disclosed in this application comprises the following components in parts by weight: 42-58 parts polymer, 3-9 parts poloxamer, 0.6-2.4 parts K-carrageenan, and 0.2-0.8 parts sodium hyaluronate. This application also discloses a composite-coated spring coil containing the above-mentioned fiber coating and a method for preparing the same. Using the technical solution disclosed in this application, the fiber coating is firmly adhered to the surface of the spring coil, and the resulting composite-coated spring coil exhibits excellent uniformity and high flexibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the technical field of medical devices, specifically to a fiber-coated, composite-coated spring coil and its preparation method. Background Technology

[0002] Transcatheter arterial chemoembolization (TACE) plays a crucial role in the treatment of hepatocellular carcinoma and is currently the preferred treatment for intermediate and advanced-stage HCC. The key to TACE success lies in the design of the embolic material, which primarily blocks the tumor's blood vessels, cutting off its nutrient and oxygen supply. Coil embolization, as a simple, easily visualized, permanent embolic device with a low error rate, is considered the best material currently available for hepatocellular artery embolization. It is delivered to the target vessel via catheter, followed by 3D structural reconstruction to physically block blood flow and achieve the embolization effect.

[0003] Existing coils are mostly made of platinum-tungsten alloys, stainless steel alloys, etc., and their auxiliary accessories are mostly made of polymer fibers with a diameter between 10-40 μm. The fiber bundles are held together by the compression force of the coil layers. The disadvantage is that during delivery or when adjusting the shape of the coil in the blood vessel, the fiber bundles are easy to fall off or become entangled on the surface of the coil, thereby reducing the embolization effect. Summary of the Invention

[0004] To address the issues of fiber shedding and entanglement in spring coils, this application provides a fiber-coated, composite-coated spring coil and its preparation method.

[0005] In a first aspect, this application provides a fiber coating comprising the following components in parts by weight: 42-58 parts of polymer, 3-9 parts of poloxamer, 0.6-2.4 parts of K-carrageenan, and 0.2-0.8 parts of sodium hyaluronate.

[0006] The technical solution provided in this application involves electrostatically spraying a polymer material with poloxamer, K-carrageenan, and sodium hyaluronate to form a uniform fiber web on and around the surface of a spring coil, preventing it from easily detaching or entangled. This technical solution ensures the fiber coating firmly adheres to the spring coil surface, resulting in a composite-coated spring coil with advantages such as good uniformity and high flexibility. Furthermore, the spun-wrapped spring coil prepared using this method allows for the addition of anticancer drugs or hemostatic agents to the biodegradable polymer, significantly improving the reliability and practicality of embolization.

[0007] In this application, a biocompatible polymer material is used as the main component, which imparts a certain degree of water absorption to the fiber coating. After the coil is inserted into the blood vessel, it absorbs water from the blood and swells for a period of time, increasing blood concentration, promoting coagulation, and effectively physically embolizing and blocking blood flow. Poloxamer, as a polymer compound, has good water solubility and low toxicity; it is a polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer. The present invention involves electrostatically spraying the polymer material to form a highly porosity and uniform fiber network on and around the surface of the coil. This fiber network effectively promotes coagulation.

[0008] Preferably, the fiber coating comprises the following components in parts by weight: 50-58 parts polymer, 3-6 parts poloxamer, 1.2-2.4 parts carrageenan, and 0.2-0.5 parts sodium hyaluronate.

[0009] Preferably, the polymer is selected from one or more of polycaprolactone, polylactic acid, polyurethane, polyhydroxyalkanoate, polyvinyl alcohol, and polyethylene glycol.

[0010] Preferably, the poloxamer is selected from any one or more of poloxamer 124, poloxamer 188, poloxamer 237, poloxamer 338, and poloxamer 407.

[0011] Furthermore, the poloxamer is poloxamer 124 and poloxamer 407 in a weight ratio of (3-7):(0.4-0.8).

[0012] In one specific implementation, the weight ratio of poloxamer 124 to poloxamer 407 can be 3:0.4, 5:0.4, 7:0.4, 3:0.6, 5:0.6, 7:0.6, 3:0.8, 5:0.8, or 7:0.8.

[0013] In some specific implementations, the weight ratio of poloxamer 124 to poloxamer 407 can also be (3-5):0.4, 5:(0.4-0.6), 7:(0.4-0.6), (3-5):0.6, 5:(0.6-0.8), 7:(0.6-0.8), (3-5):0.8, (5-7):0.8, (3-7):0.8.

[0014] Experimental analysis shows that the selection of poloxamer 124 and poloxamer 407 in the above weight ratio as raw materials for poloxamer in this application further improves the adhesion and flexibility between the fiber coating and the spring coil body.

[0015] Secondly, this application provides a composite coated spring coil, comprising a spring coil body and a fiber coating as described in any one of claims 1-5, wherein the fiber coating encapsulates the spring coil body.

[0016] Preferably, the porosity of the fiber coating is 50±35%.

[0017] Thirdly, this application provides a method for preparing the above-mentioned composite coated spring ring, specifically including the following steps: According to the weight parts of the raw materials, the polymer, the poloxamer, the carrageenan, and the sodium hyaluronate are dissolved in a solvent and sealed. The solution is heated to 60-90°C and stirred until it becomes clear. After cooling, the solution is used to obtain a spinning solution. The solution is then sprayed onto the surface of the rotating spring coil body through electrospinning and dried under vacuum to form a fiber coating, thus obtaining a composite coated spring coil.

[0018] This application utilizes the above-mentioned technical solution to form a high-porosity fiber web on and around the spring coil by electrostatic spraying, thereby solving the problems of fiber shedding and entanglement in the spring coil.

[0019] Preferably, the electrospinning process parameters are: electrostatic voltage 13-18kV, rotation speed of the spring coil body 260-380rpm, receiving distance 12-18cm, injection speed 0.3-0.7ml / h, spinning diameter 1-150um, and wire diameter 24-50um.

[0020] Experimental analysis shows that, in the process of preparing the composite coated spring ring, this application achieves higher porosity and uniformity of the fiber coating loaded on the composite coated spring ring by reasonably controlling the parameters in the electrospinning process. At the same time, the fiber coating has good flexibility, so that the fiber coating formed by spinning deforms with the deformation of the spring ring without affecting the 3D structure of the spring ring.

[0021] Furthermore, the solvent is selected from any one or more of dichloromethane, chloroform, toluene, tetrahydrofuran, N,N-dimethylformamide, water, and ethyl acetate.

[0022] In summary, the technical solution of this application has the following effects: This application utilizes polymers, poloxamer, K-carrageenan, and sodium hyaluronate as raw material components to provide a fiber coating. By electrostatic spraying, a fiber web is formed on and around the surface of the spring coil body, which enables the fiber coating to adhere firmly to the surface of the spring coil and is not easy to fall off, thus solving the problem of easy shedding and tangling of spring coil fibers.

[0023] The composite coated spring coil provided in this application has good uniformity and high flexibility; at the same time, it can absorb water from the blood and expand after the spring coil is delivered into the blood vessel for a period of time. Its function is to increase the blood concentration, promote coagulation, fully perform physical embolization, and block blood flow.

[0024] The fiber coating provided in this application allows for the selection of polymer spinning with different concentrations and materials according to the needs of the patient's condition. It can also be made of a variety of polymer materials and spun into a web on the spring coil. Furthermore, since the fiber web is made of polymer materials, drugs can be added to it to control the drug loading and drug release time, thereby improving the drug's efficacy. Attached Figure Description

[0025] Figure 1 This is a full micrograph of the composite-coated spring coil in Example 2.

[0026] Figure 2 This is a magnified micrograph of the composite-coated spring coil in Example 2.

[0027] Figure 3 This is a magnified micrograph of the composite-coated spring coil in Example 12. Detailed Implementation

[0028] The present application will be further described in detail below with reference to embodiments, comparative examples and performance test results. These embodiments should not be construed as limiting the scope of protection claimed in this application. Example

[0029] Examples 1-4 Examples 1-4 each provide a composite coated spring coil.

[0030] The difference in the above embodiments is that the amount of each raw material component in the fiber coating is different, as shown in Table 1.

[0031] The specific method for preparing the composite coated spring coil in the above embodiments is as follows: S1: Preparation of spinning solution: Weigh the amount of each raw material according to the weight in Table 1. Dissolve the polymer (polyurethane or polyvinyl alcohol), poloxamer (composed of poloxamer 124 and poloxamer 407 in a weight ratio of 5:0.6), K-carrageenan (CAS No.: 11114-20-8), and sodium hyaluronate in 100g of solvent (N,N-dimethylformamide and tetrahydrofuran in a volume ratio of 1:1) and seal it. Heat to 75±5℃ and stir to dissolve until clear and free of particles. Cool and set aside to obtain the spinning solution. S2: Forming a fiber coating on the surface of a rotating spring coil (from Cook Company, model IMWCE-35-5-5) by electrospinning: In a room-temperature, windless environment, a syringe is used to draw up the above spinning solution, which is then placed on a precision injection pump and fixed at an injection rate of 0.5 ml / h. The catheter and conductive needle (connected to the positive terminal of the power supply) are connected. The stainless steel alloy spring coil is placed on a carbide rod and fixed on a rotary motor, grounded and kept coaxially rotating at a speed of 300 rpm. The distance between the conductive needle and the spring coil is maintained at 15 ± 1 cm (receiving distance). The electrostatic voltage is adjusted to 15 ± 1 kV, the spinning diameter is 10 ± 2 μm, and the wire diameter is 33 μm. After spinning, the coil is dried in a vacuum drying oven at 60°C for 60 min to form a fiber coating, resulting in a composite coated spring coil with a porosity of 62-68%.

[0032] Among them, the composite coated spring coil prepared in Example 2 is as follows: Figure 1-2 As shown, where, Figure 1 This is a full-size micrograph of a composite-coated spring coil. Figure 2 This is a magnified micrograph of a composite coated spring coil with a porosity of 67%.

[0033] Table 1. Dosage of each raw material component in the fiber coating Examples 5-9 Examples 5-9 each provide a composite coated spring coil.

[0034] The difference between the above embodiment and Embodiment 2 is that the types of poloxamer are different, as detailed below.

[0035] In Example 5: Poloxamer 124 was used as the poloxamer component.

[0036] In Example 6, the mixture consisted of poloxamer 124 and poloxamer 338 in a weight ratio of 5:0.6.

[0037] In Example 7, the mixture consists of poloxamer 124 and poloxamer 407 in a weight ratio of 3:1.

[0038] In Example 8, the mixture consisted of poloxamer 124 and poloxamer 407 in a weight ratio of 3:0.8.

[0039] In Example 9, the mixture consists of poloxamer 124 and poloxamer 407 in a weight ratio of 7:0.4.

[0040] The types of raw materials, the amounts of each raw material, and the preparation method of the composite coated spring coil are the same in the above embodiments and in Embodiment 2.

[0041] Example 10 Example 10 provides a composite coated spring coil.

[0042] The difference between this embodiment and Embodiment 2 is that step S2 in the preparation method of the composite coated spring ring is different, as shown below.

[0043] The specific method for preparing the composite coated spring coil in the embodiment is as follows: S2: Forming a fiber coating on the surface of a rotating spring coil body by electrospinning: In a room-temperature, windless hood, a syringe is used to draw up the above spinning solution, which is then placed on a precision injection pump and fixed at an injection speed of 0.3 ml / h. The conduit and conductive needle (connected to the positive terminal of the power supply) are connected. The spring coil is placed on a carbide rod and fixed on a rotary motor, grounded and kept coaxially rotating at a speed of 260 rpm. The distance between the conductive needle and the spring coil is maintained at 15 ± 1 cm (receiving distance). The electrostatic voltage is adjusted to 15 ± 1 kV, the spinning diameter is 10 ± 2 μm, and the wire diameter is 33 μm. After spinning, the coil is dried in a vacuum drying oven at 60°C for 60 min to form a fiber coating, thus obtaining a composite coated spring coil with a porosity of 62%.

[0044] The types and amounts of raw materials used in this embodiment are the same as those in Embodiment 2, as are the remaining preparation methods for the composite coated spring coil.

[0045] Example 11 Example 11 provides a composite coated spring coil.

[0046] The difference between this embodiment and Embodiment 2 is that step S2 in the preparation method of the composite coated spring ring is different, as shown below.

[0047] The specific method for preparing the composite coated spring coil in the embodiment is as follows: S2: Forming a fiber coating on the surface of a rotating spring coil body by electrospinning: In a windless hood at room temperature, use a syringe to draw up the above spinning solution, place it on a precision injection pump and fix it, with an injection speed of 0.7 ml / h, and connect the guide tube and the conductive needle (connected to the positive terminal of the power supply); put the spring coil on a carbide rod and fix it on a rotary motor, ground it and keep it coaxially rotating at a speed of 380 rpm, keep the distance between the conductive needle and the spring coil at 15±1 cm (receiving distance), adjust the electrostatic voltage to 15±1 kV, the spinning diameter is 10±2 μm, and the wire diameter is 33 μm; after spinning, dry in a vacuum drying oven at 60℃ for 60 min to form a fiber coating, thus obtaining a composite coated spring coil with a porosity of 68%.

[0048] The types and amounts of raw materials used in this embodiment are the same as those in Embodiment 2, as are the remaining preparation methods for the composite coated spring coil.

[0049] Example 12 Example 12 provides a composite coated spring coil.

[0050] The difference between this embodiment and Embodiment 2 is that step S2 in the preparation method of the composite coated spring ring is different, as shown below.

[0051] The specific method for preparing the composite coated spring coil in the embodiment is as follows: S2: Forming a fiber coating on the surface of a rotating spring coil body by electrospinning: In a room-temperature, windless hood, a syringe is used to draw up the above spinning solution, which is then placed on a precision injection pump and fixed at an injection speed of 0.5 ml / h. The conduit and conductive needle (connected to the positive terminal of the power supply) are connected. The spring coil is placed on a hard alloy rod and fixed on a rotary motor, grounded and kept coaxially rotating at a speed of 390 rpm. The distance between the conductive needle and the spring coil is maintained at 15 ± 1 cm (receiving distance). The electrostatic voltage is adjusted to 15 ± 1 kV, the spinning diameter is 10 ± 2 μm, and the wire diameter is 50 μm. After spinning, the coil is dried in a vacuum drying oven at 60°C for 60 min to form a fiber coating, thus obtaining a composite coated spring coil with a porosity of 79%.

[0052] The complete microscopic image of the composite-coated spring coil prepared in this embodiment is shown below. Figure 3 As shown, the porosity is 79%.

[0053] The types and amounts of raw materials used in this embodiment are the same as those in Embodiment 2, as are the remaining preparation methods for the composite coated spring coil.

[0054] Comparative Examples 1-2 Comparative Examples 1 and 2 each provide a composite coated spring coil.

[0055] The difference between the above comparative examples lies in the amount of each raw material component used in the fiber coating, as shown in Table 1.

[0056] The types of raw materials, the amounts of each raw material, and the preparation method of the composite coated spring coil are the same as those in the comparative example and Example 2.

[0057] Performance testing (1) Cytotoxicity test: The test was conducted in accordance with GB / T 16886.5-2017 Biological evaluation of medical devices - Part 5: In vitro cytotoxicity test. The test method was to evaluate the cytotoxicity of the fiber coating using a quantitative method. Cytotoxicity grade 0 indicates no cytotoxicity; cytotoxicity grade 1 indicates mild cytotoxicity; cytotoxicity grade 2 indicates moderate cytotoxicity; and cytotoxicity grade 3 indicates severe cytotoxicity.

[0058] (2) Adhesive strength: Refer to GBT 19976-2005 standard and use an electronic comprehensive strength tester to test the adhesive strength between the fiber coating and the spring coil body.

[0059] (3) Tensile strength: The composite coated spring coil was stretched with a tensile tester to test whether the fiber coating of the composite coated spring coil would shed or fall off under a force of 0.34N.

[0060] (4) Flexibility: Repeatedly fold the composite coated spring coil at +45° until the fiber coating shows signs of shedding or falling off, and record the number of repeated folds.

[0061] Test results are shown in Table 2.

[0062] Table 2 Performance test results of composite coated spring coils As shown in Table 2 above, the cytotoxicity of the composite-coated spring coils prepared in this application is grade 0, meeting clinical requirements. Furthermore, the adhesive strength between the fiber coating and the spring coil body is greater than 16.8 N / mm. Under a force of 0.34 N, the fiber coating of the composite-coated spring coils did not show any shedding or detachment. When repeatedly folded at +45°, the composite-coated spring coils withstood up to 23 folds. These test results demonstrate that the technical solution provided in this application, using polymers, poloxamer, K-carrageenan, and sodium hyaluronate as raw material components, provides a fiber coating. This coating, formed by electrostatic spraying on and around the surface of the spring coil body, forms a high-porosity fiber network, enabling the fiber coating to firmly adhere to the spring coil surface and preventing detachment, thus solving the problem of easy fiber shedding and entanglement in spring coils.

[0063] By comparing the test results of Examples 1-4 with those of Comparative Examples 1-2, it can be seen that when Comparative Example 2 uses other raw materials, or when the amount of raw material components in Comparative Example 1 does not conform to the technical solution of this application, the adhesion between the fiber coating and the spring coil body is weak, and defects such as shedding and falling off are likely to occur.

[0064] By comparing the test results of Example 2 with those of Comparative Examples 5-9, it can be seen that the present application selected poloxamer 124 and poloxamer 407 with a weight ratio of (3-7):(0.4-0.8) as raw materials for poloxamer, which further improved the adhesion and flexibility between the fiber coating and the spring coil body.

[0065] By comparing the test results of Example 2 with those of Comparative Examples 10-12, it can be seen that by selecting different process conditions and changing process parameters such as spinning concentration and spinning diameter, this application can obtain composite coated spring rings with different porosities, thereby improving the application scenarios of composite coated spring rings.

[0066] Although the present invention has been described in detail above with general descriptions and specific embodiments, modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, all such modifications or improvements made without departing from the spirit of the present invention fall within the scope of protection claimed by the present invention.

Claims

1. A composite coated spring coil, characterized in that, The device includes a spring coil body and a fiber coating, wherein the fiber coating encapsulates the spring coil body; the fiber coating has a porosity of 50±35% and comprises the following components in parts by weight: 42-58 parts of polymer, 3-9 parts of poloxamer, 0.6-2.4 parts of K-carrageenan, and 0.2-0.8 parts of sodium hyaluronate; The preparation method of the composite coated spring coil includes: dissolving the polymer, poloxamer, carrageenan, and sodium hyaluronate in a solvent according to the weight parts of the raw materials and sealing the solution; heating the solution to 60-90°C and stirring until it becomes clear; cooling the solution to obtain a spinning solution; spraying the solution onto the surface of a rotating spring coil body through electrospinning; and drying the solution under vacuum to form a fiber coating, thus obtaining the composite coated spring coil. The electrospinning process parameters are as follows: electrostatic voltage 13-18kV, rotation speed of the spring coil body 260-380rpm, receiving distance 12-18cm, injection speed 0.3-0.7ml / h, spinning diameter 1-150um, and wire diameter 24-50um.

2. The composite coated spring coil according to claim 1, characterized in that, It includes the following components in parts by weight: 50-58 parts polymer, 3-6 parts poloxamer, 1.2-2.4 parts carrageenan, and 0.2-0.5 parts sodium hyaluronate.

3. The composite coated spring coil according to claim 1, characterized in that, The polymer is selected from one or more of polycaprolactone, polylactic acid, polyurethane, polyhydroxyalkanoate, polyvinyl alcohol, and polyethylene glycol.

4. The composite coated spring coil according to claim 1, characterized in that, The poloxamer is selected from any one or more of poloxamer 124, poloxamer 188, poloxamer 237, poloxamer 338, and poloxamer 407.

5. The composite coated spring coil according to claim 4, characterized in that, The poloxamer is poloxamer 124 and poloxamer 407 in a weight ratio of (3-7):(0.4-0.8).

6. The composite coated spring coil according to any one of claims 1-4, characterized in that, The solvent is selected from any one or more of dichloromethane, trichloromethane, toluene, tetrahydrofuran, N,N-dimethylformamide, water, and ethyl acetate.

Citation Information

Patent Citations

  • Medical spring ring and preparation method thereof

    CN113855137A