An electromagnetic shielding and absorbing material C / MoS2 and its preparation method and application
MoS2 nanosheets were combined with cotton fiber-derived tubular carbon fibers by hydrothermal method to form C/MoS2 composite materials, which solved the problems of poor impedance matching of absorbing materials and narrow frequency bands, and achieved wide spectrum wide electromagnetic wave absorption performance, suitable for multiple electromagnetic shielding of such equipment.
Patent Information
- Application Number
- CN202311639848.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-01
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-12-01
AI Technical Summary
The existing wave absorbing materials have problems such as poor impedance matching, narrow frequency band and insufficient durability in electromagnetic wave absorption performance, which is difficult to meet the demand for electromagnetic wave shielding by military and civilian equipment.
The hydrothermal method is used to composite MoS2 nanosheets with cotton fiber-derived tubular carbon fibers to form a C/MoS2 composite material. By regulating the growth and wrapping structure of MoS2, the impedance matching and absorption performance of the material are improved.
It achieves low reflection loss in the frequency range of 2~18GHz, broad spectrum and wide electromagnetic wave absorption, and is suitable for electromagnetic shielding of various devices, improving the durability and performance of the material.
Smart Images

Figure CN117691367B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electromagnetic shielding technology, and in particular to an electromagnetic shielding absorbing material C / MoS 2 And its preparation method and application. Background Art
[0002] Absorbing materials are a type of functional materials that can absorb electromagnetic waves in space. They can convert electromagnetic radiation into heat or other forms of energy for consumption, thereby reducing the reflection intensity of electromagnetic waves on the surface of the material. In engineering applications, in addition to requiring absorbing materials to have a high absorption rate of electromagnetic waves in a wide frequency band, they are also required to have properties such as light weight, temperature resistance, moisture resistance, and corrosion resistance. With the development of modern science and technology, at airports, flights are delayed due to electromagnetic interference and cannot take off; in hospitals, mobile phones often interfere with the normal operation of various electronic diagnostic and treatment instruments. In addition, coating various weapons and military facilities with absorbing materials can absorb reconnaissance waves and attenuate reflected signals, thereby breaking through the defense zone of enemy radars. This is a powerful means of anti-radar reconnaissance. The rapid development of radar detection technology has put forward higher technical requirements for the electromagnetic wave stealth performance of military equipment, and also put forward lightweight, high-strength and broadband performance requirements for the absorbing materials used. On the other hand, today's household appliances and various operating equipment generally have electromagnetic radiation problems. Electromagnetic radiation causes direct and indirect harm to the human body through thermal effects, non-thermal effects, and cumulative effects. The increasingly serious electromagnetic radiation pollution problem also affects human health and the reliability of precision electronic equipment. Therefore, high-performance lightweight electromagnetic wave absorbing materials are facing urgent needs in both military and civilian industries.
[0003] Carbon-based nanomaterials have the advantages of being lightweight and easy to composite with other materials, and are one of the hot topics in the research of absorbing materials. There are many types of carbon-based nano-absorbing materials, among which biomass-derived carbon materials can better retain the residual structure of natural raw materials after carbonization, such as ordered pore structure, hollow tubular structure, hierarchical structure and other special structural forms, which help to improve the electromagnetic wave loss capacity of the material. Natural cotton fiber has a one-dimensional hollow tubular structure, which is composed of many concentric layers from the outside to the inside, and has a nearly circular cross-sectional shape. Its material composition is simple, mainly containing cellulose, water and trace amounts of organic matter, which is very suitable as a biomass-derived carbon source. However, pure cotton fiber-derived carbon has poor impedance matching and a single electromagnetic wave loss mechanism, which cannot meet the needs of practical applications. In order to optimize its absorbing performance, composite components can be introduced to design and regulate its microstructure. Nano-molybdenum disulfide (MoS 2 ) is a typical two-dimensional material that has a good response to electromagnetic waves and has an ultra-thin thickness and ultra-large specific surface area. It can be used as an impedance matching regulator and composited with cotton fiber-derived carbon materials to achieve the purpose of improving impedance matching and enhancing wave absorbing performance. Summary of the invention
[0004] The present invention aims to provide an electromagnetic shielding and absorbing material C / MoS 2 .
[0005] Another object of the present invention is to provide the electromagnetic shielding and absorbing material C / MoS 2 The preparation method of MoS was solved by hydrothermal method. 2 It eliminates technical problems such as agglomeration and uneven wrapping, and at the same time effectively improves the material's microwave absorbing performance.
[0006] The third object of the present invention is to provide the electromagnetic shielding and absorbing material C / MoS 2 application.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] An electromagnetic shielding absorbing material, characterized in that: the absorbing material is cotton fiber derived C / MoS 2 The composite material is specifically prepared from cotton fiber as raw material into biomass-derived tubular carbon fiber, and then MoS is hydrothermally deposited on the surface of the biomass-derived tubular carbon fiber. 2 , forming MoS 2 A composite structure that wraps around tubular carbon fibers.
[0009] Furthermore, the preparation of biomass-derived tubular carbon fibers is to take absorbent cotton balls and perform heat treatment in an inert atmosphere at a temperature of 600 to 800° C. for 5 to 6 hours to obtain tubular carbon fibers having a cotton fiber structure.
[0010] Furthermore, the hydrothermal deposition of MoS 2 Sodium molybdate dihydrate (Na 2 MoO 4 ·2H 2 O) and thiourea (CH 4 N 2 S) is dissolved in deionized water to form a mixed solution, and then the tubular carbon fiber is added to stir and mix, and a hydrothermal reaction is carried out at 190-210° C. for 20-24 hours, and then cooled to room temperature.
[0011] Furthermore, the mixed solution contains sodium molybdate dihydrate, CH 4 N 2 The dosage of S and deionized water is 1-2 mmol:4-8 mmol:30 mL, and the dosage ratio of the tubular carbon fiber to the mixed liquid is 1 mmol:3 mL.
[0012] Furthermore, after the hydrothermal reaction was completed, the product was separated by centrifugation at 8000 r / min for 2 min, and then the product was washed with deionized water and C2 H 6 After multiple washings to remove impurities, the mixture was dried in a drying oven at 60 °C for 24 h to obtain cotton fiber-derived C / MoS 2 Composite materials.
[0013] An electromagnetic shielding and absorbing material C / MoS 2 The preparation method is characterized in that: cotton thread is used as raw material to prepare biomass-derived tubular carbon fiber, and MoS is hydrothermally deposited on the surface of the biomass-derived tubular carbon fiber. 2 , forming MoS 2 C / MoS wrapped around tubular carbon fiber 2 The composite structure is prepared by taking absorbent cotton balls and heat treating them in an inert atmosphere at a temperature of 600 to 800° C. for 5 to 6 hours to obtain tubular carbon fibers with a cotton fiber structure.
[0014] Furthermore, the hydrothermal deposition of MoS 2 Sodium molybdate dihydrate (Na 2 MoO 4 ·2H 2 O) and thiourea (CH 4 N 2 S) is dissolved in deionized water to form a mixed solution, and then the tubular carbon fiber is added to stir and mix, and a hydrothermal reaction is carried out at 190-210° C. for 20-24 hours, and then cooled to room temperature.
[0015] Furthermore, the mixed solution contains sodium molybdate dihydrate, CH 4 N 2 The dosage of S and deionized water is 1-2 mmol:4-8 mmol:30 mL, and the dosage ratio of the tubular carbon fiber to the mixed liquid is 1 mmol:3 mL.
[0016] Furthermore, after the hydrothermal reaction was completed, the product was separated by centrifugation at 8000 r / min for 2 min, and then the product was washed with deionized water and C 2 H 6 After multiple washings to remove impurities, the mixture was dried in a drying oven at 60 °C for 24 h to obtain cotton fiber-derived C / MoS 2 Composite materials.
[0017] The most specific one is C / MoS, an electromagnetic shielding and absorbing material 2 The preparation method is characterized by comprising the following steps:
[0018] (1) taking an absorbent cotton ball, drying it under a vacuum environment, and then heat treating it under an inert atmosphere at a temperature of 600 to 800° C. for a holding time of 5 to 6 hours to obtain a tubular carbon fiber having a cotton fiber structure;
[0019] (2) Sodium molybdate dihydrate (Na 2 MoO 4 ·2H 2 O) and thiourea (CH 4 N 2 S) is dissolved in deionized water to form a mixed solution, and then the tubular carbon fiber is added and stirred and mixed, and a hydrothermal reaction is carried out at 190-210° C. for 20-24 hours, and then cooled to room temperature. The mixed solution contains sodium molybdate dihydrate, CH 4 N 2 The amount of S and deionized water is 1-2 mmol: 4-8 mmol: 30 mL, and the amount ratio of the tubular carbon fiber to the mixed solution is 1 mmol: 3 mL;
[0020] (3) After the thermal reaction, the product obtained by the hydrothermal reaction was separated by centrifugation at 8000 r / min for 2 min and then washed with deionized water and C 2 H 6 After multiple washings to remove impurities, the mixture was dried in a drying oven at 60 °C for 24 h to obtain cotton fiber-derived C / MoS 2 Composite materials.
[0021] Electromagnetic shielding and absorbing material C / MoS prepared by the above method 2 Application in the preparation of radar absorbing coatings.
[0022] An electromagnetic shielding and absorbing coating, characterized in that it comprises a resin material and an absorbing material C / MoS 2 , coupling agent, dispersant, anti-settling agent, plasticizer and solvent, the absorbing material C / MoS 2 The biomass-derived tubular carbon fibers were prepared from cotton fibers as raw materials, and then MoS was hydrothermally deposited on the surface of the biomass-derived tubular carbon fibers. 2 , forming MoS 2 C / MoS wrapped around tubular carbon fiber 2 Composite structure.
[0023] Furthermore, the preparation of biomass-derived tubular carbon fibers is to take absorbent cotton balls and perform heat treatment in an inert atmosphere at a temperature of 600 to 800° C. for 5 to 6 hours to obtain tubular carbon fibers having a cotton fiber structure.
[0024] Furthermore, the hydrothermal deposition of MoS 2 Sodium molybdate dihydrate (Na 2 MoO 4 ·2H 2 O) and thiourea (CH 4 N 2S) is dissolved in deionized water to form a mixed solution, and then the tubular carbon fiber is added to stir and mix, and a hydrothermal reaction is carried out at 190-210° C. for 20-24 hours, and then cooled to room temperature.
[0025] Furthermore, the mixed solution contains sodium molybdate dihydrate, CH 4 N 2 The dosage of S and deionized water is 1-2 mmol:4-8 mmol:30 mL, and the dosage ratio of the tubular carbon fiber to the mixed liquid is 1 mmol:3 mL.
[0026] Furthermore, after the hydrothermal reaction was completed, the product was separated by centrifugation at 8000 r / min for 2 min, and then the product was washed with deionized water and C 2 H 6 After multiple washings to remove impurities, the mixture was dried in a drying oven at 60 °C for 24 h to obtain cotton fiber-derived C / MoS 2 Composite materials.
[0027] During the preparation process, it was found that molybdenum disulfide easily agglomerates during the hydrothermal growth process, and the microwave absorption performance of the prepared composite material is not very ideal.
[0028] During the preparation process, cotton fibers are first made into biomass-derived tubular carbon fibers and then added to the hydrothermal reaction system. The carbon fibers inherit the natural tubular structure of the raw materials and can form a steric hindrance effect in the solution under the hydrothermal environment, inhibiting the formation of MoS 2 The accumulation and agglomeration of nanosheets increase the specific surface area of the material and produce more active sites. At the same time, carbon fibers also provide MoS 2 The growth during the hydrothermal process provides nucleation sites for MoS 2 Nanosheets can grow and cover the surface of carbon fibers, forming a uniform and complete wrapping of the tubular carbon fibers.
[0029] Molybdenum disulfide synthesized by hydrothermal method on the surface of cotton fiber biomass derived tubular carbon fiber has the characteristics of rich defects and many surface dangling bonds. The induced electrons in molybdenum disulfide move along the molecular network to form dissipative current, which has a good response to electromagnetic waves. The hollow tubular carbon fiber combined with molybdenum disulfide provides a longer transmission channel for the incident electromagnetic wave. The combination of the two can increase the multiple scattering and absorption of electromagnetic waves in the cavity. The one-dimensional tubular structure has a high specific surface area and high defect density, which can produce more space charge polarization and dipole polarization, accelerate the flow of electrons, and improve the conductivity loss of the material. The two components are obtained by in-situ growth and self-assembly. C / MoS 2 Composite materials can improve the impedance matching characteristics of composite materials, adjust electromagnetic parameters, increase polarization loss at heterogeneous interfaces, and thus improve the wave absorbing performance of composite materials.
[0030] By adjusting the ratio of molybdenum atoms to carbon atoms during the hydrothermal process, the C / MoS 2 The absorption performance of the composite material was improved through continuous attempts. 2 When the molar ratio of molybdenum to carbon atoms in the composite material is 1.5:10, a broadband and high-strength absorbing material can be obtained.
[0031] Furthermore, the resin material is obtained by mixing epoxy resin and acrylic resin in a ratio of 1:1.
[0032] Furthermore, the coupling agent is a titanate coupling agent, the dispersant includes at least one of polyvinyl pyrrolidone, polyethylene glycol, polyvinyl alcohol and propylene carbonate, the anti-settling agent includes any one of bentonite, polyamide wax and polyethylene wax, the plasticizer includes at least one of dibutyl phthalate (DBP) and dioctyl phthalate (DOP), and the solvent can be at least one of ethanol, n-butanol, isopropanol, ethyl acetate, acetone or deionized water.
[0033] Further, according to the mass fraction, the amount of each component in the coating is as follows:
[0034] Resin material is 40-45 parts, C / MoS 2 The amount of the solvent is 35-45 parts, the amount of the coupling agent is 2-4 parts, the amount of the dispersant is 1-2 parts, the amount of the dust suppressant is 0.5-1 parts, the amount of the plasticizer is 1-1.5 parts, and the amount of the solvent is 35-45 parts.
[0035] Further preferably, the amount of each component in the coating is 40 parts of resin material, C / MoS 2 The amount of the solvent is 40 parts, the amount of the coupling agent is 3 parts, the amount of the dispersant is 1.5 parts, the amount of the dust suppressant is 0.6 parts, the amount of the plasticizer is 1.2 parts, and the amount of the solvent is 40 parts.
[0036] The method for preparing the electromagnetic shielding and absorbing coating is characterized by comprising the following steps:
[0037] (1) The absorbing material C / MoS 2 , adding the coupling agent into the solvent and performing ultrasonic dispersion to obtain a mixed solution A, wherein the ultrasonic power is 800-1000W and the ultrasonic time is 20-40min;
[0038] (2) Adding resin material, plasticizer, dispersant and anti-settling agent to the mixed solution A and dispersing them by high-speed stirring. The stirring rate is 1500-2500 rpm and the stirring time is 1-1.5 h.
[0039] The present invention has the following technical effects:
[0040] The present invention uses cotton thread to derive carbon fiber to participate in the preparation of electromagnetic shielding and absorbing material C / MoS 2, can efficiently absorb electromagnetic waves to achieve the effect of shielding electromagnetic waves. It has a low reflection loss value of -41.7dB in the frequency range of 2 to 18GHz. In the thickness range of 1.0 to 5.0mm, the effective absorption width is large, and the effective absorption width is 12.32GHz, specifically 5.68 to 18GHz. The material has excellent electromagnetic wave shielding performance. The electromagnetic shielding absorbing material C / MoS prepared by the present invention 2 It can be applied to various equipment and products that require electromagnetic shielding in life and work, such as shale gas extraction equipment, mining machinery and equipment, medical equipment, communication equipment, aerospace equipment, so as to reduce the interference of electromagnetic waves on the normal operation of various equipment. In addition, it can be used in military equipment to achieve shielding function by absorbing electromagnetic waves. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 : Biomass-derived C / MoS prepared in Example 1 2 Scanning electron microscope image of .
[0042] Figure 2 : C / MoS prepared in Comparative Example 1 2 Scanning electron microscope image of .
[0043] Figure 3 : Biomass-derived C / MoS prepared in Example 1 2 Reflectivity map of .
[0044] Figure 4 : C / MoS prepared in Comparative Example 1 2 Reflectivity map of .
[0045] Figure 5 : Biomass-derived C / MoS prepared in Example 2 2 Reflectivity map of .
[0046] Figure 6 : Biomass-derived C / MoS prepared in Example 3 2 Reflectivity map of . DETAILED DESCRIPTION
[0047] The present invention is described in detail below through examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above-mentioned contents of the present invention.
[0048] Example 1
[0049] An electromagnetic shielding and absorbing material C / MoS 2 The preparation method comprises the following steps:
[0050] (1) taking an absorbent cotton ball, drying it under a vacuum environment, and then heat treating it under an inert atmosphere at a temperature of 700° C. for a holding time of 5.5 h to obtain a tubular carbon fiber having a cotton fiber structure;
[0051] (2) Sodium molybdate dihydrate (Na 2 MoO 4 ·2H 2 O) and thiourea (CH 4 N 2 S) is dissolved in deionized water to form a mixed solution, and then the tubular carbon fiber is added for stirring and mixing, and a hydrothermal reaction is performed at 200° C. for 24 hours, and then cooled to room temperature, wherein the amount of sodium molybdate dihydrate, thiourea and deionized water in the mixed solution is 1.5 mmol: 6 mmol: 30 mL, and the amount ratio of the tubular carbon fiber to the mixed solution is 1 mmol: 3 mL;
[0052] (3) After the thermal reaction, the product obtained by the hydrothermal reaction was separated by centrifugation at 8000 r / min for 2 min and then washed with deionized water and C 2 H 6 After multiple washings to remove impurities, the mixture was dried in a drying oven at 60 °C for 24 h to obtain cotton fiber-derived C / MoS 2 A composite material, wherein the molar ratio of molybdenum to carbon atoms in the composite material is 1.5:10.
[0053] from Figure 1 It can be seen that the biomass-derived carbon generated by carbonization of cotton fibers retains the fiber structure well, and MoS2 is grown in situ on the carbon fiber surface. 2 Nanosheets, MoS 2 Evenly distributed on the carbon fiber surface, and self-assembled to form C / MoS 2 The composite material improves the impedance matching characteristics of the composite material, adjusts the electromagnetic parameters, and increases the polarization loss of the heterogeneous interface, thereby improving the wave absorbing performance of the composite material.
[0054] By preparing C / MoS 2The composite material was mixed with paraffin, and its electromagnetic properties were tested by the coaxial method. Specifically, the sample to be tested was mixed with paraffin in a certain filling ratio, and then placed in a coaxial mold and pressed into a coaxial ring with an inner diameter of about 3mm, an outer diameter of about 7mm, and a thickness of about 2mm. The coaxial ring was placed in a coaxial line fixture and connected to the two coaxial lines ports of a vector network analyzer through a connector. The excitation signal emitted by the signal source of the network vector analyzer was divided into two signals by a signal separator. One signal entered the receiver test as a reference signal, and the other signal was extracted by a directional coupler. Finally, the amplitude and phase of the two signals were obtained by processing the display unit, and the scattering parameters and of the absorbing material in the frequency range of 2.0 to 18.0GHz were obtained. The transmission coefficient and reflection coefficient were obtained from the scattering parameters, and then the electromagnetic parameters of the absorbing material were determined. After obtaining the dielectric constant and magnetic permeability, the reflectivity values of the sample at different frequencies at different thicknesses were calculated according to the relevant formulas. The results are as follows Figure 3 As shown in the figure, when the coating thickness is 4.5 mm, C / MoS 2 The minimum reflection loss value is -41.7dB. In the thickness range of 1.0 to 5.0mm, the effective absorption width is 12.32GHz, which can effectively absorb more than 95% of electromagnetic waves in the range of 5.68-18GHz.
[0055] Comparative Example 1
[0056] A C / MoS 2 The preparation method comprises the following steps:
[0057] (1) Sodium molybdate dihydrate (Na 2 MoO 4 ·2H 2 O) and thiourea (CH 4 N 2 S) was dissolved in deionized water to form a mixed solution, and then the absorbent cotton balls were combed into fibers and added into the mixed solution for stirring and mixing, and a hydrothermal reaction was carried out at 200° C. for 24 hours, and then cooled to room temperature, wherein the amount of sodium molybdate dihydrate, thiourea and deionized water in the mixed solution was 1.5 mmol: 6 mmol: 30 mL;
[0058] (2) After the hydrothermal reaction, the mixture was centrifuged at 8000 r / min for 2 min to separate the product obtained from the hydrothermal reaction and then washed with deionized water and C 2 H 6 After multiple washings to remove impurities, the mixture was dried in a drying oven at 60 °C for 24 h to obtain C / MoS 2 Precursor;
[0059] (3) C / MoS 2The precursor was placed in an inert atmosphere for heat treatment at 700 °C for 5.5 h to obtain C / MoS 2 .
[0060] In Comparative Example 1, MoS was first generated on the cotton fiber surface. 2 The biggest problem in the preparation process is that it is impossible to increase the C / MoS ratio by adjusting the ratio of molybdenum to carbon atoms. 2 For the purpose of the material's microwave absorption performance, during the hydrothermal process, the cotton fiber that has not been carbonized cannot be MoS 2 Nucleation growth provides more attachment points, so MoS 2 The coating effect on the fiber surface is poor, C / MoS 2 The composite material cannot form many heterogeneous structures, and due to the lack of steric hindrance, MoS 2 Obvious agglomeration occurred, e.g. Figure 2 As shown, this has an adverse effect on the absorbing performance. Figure 4 It can be seen that the C / MoS prepared in Comparative Example 1 2 The minimum reflection loss value is -12.5dB. In the thickness range of 1.0 to 5.0mm, the effective absorption width is 10.5GHz.
[0061] During the preparation process, we also tried to directly use other tubular carbon fiber materials (non-cotton fiber biomass-derived carbon fibers) to prepare C / MoS 2 Composite materials, but the performance of the prepared composite materials is not as good as C / MoS prepared with cotton fiber as raw material 2 Composite materials have excellent performance.
[0062] Example 2
[0063] An electromagnetic shielding and absorbing material C / MoS 2 The preparation method comprises the following steps:
[0064] (1) taking an absorbent cotton ball, drying it under a vacuum environment, and then heat treating it under an inert atmosphere at a temperature of 800° C. for a holding time of 5 h to obtain a tubular carbon fiber having a cotton fiber structure;
[0065] (2) Sodium molybdate dihydrate (Na 2 MoO 4 ·2H 2 O) and thiourea (CH 4 N 2 S) was dissolved in deionized water to form a mixed solution, and then the tubular carbon fiber was added and stirred and mixed, and a hydrothermal reaction was carried out at 190° C. for 22 hours, and then cooled to room temperature. The mixed solution contained sodium molybdate dihydrate, CH4 N 2 The amount of S and deionized water is 1mmol:4mmol:30mL, and the amount ratio of the tubular carbon fiber to the mixed solution is 1mmol:3mL;
[0066] (3) After the thermal reaction, the product obtained by the hydrothermal reaction was separated by centrifugation at 8000 r / min for 2 min and then washed with deionized water and C 2 H 6 After multiple washings to remove impurities, the mixture was dried in a drying oven at 60 °C for 24 h to obtain cotton fiber-derived C / MoS 2 A composite material, wherein the molar ratio of molybdenum to carbon atoms in the composite material is 1:10.
[0067] like Figure 5 As shown in the figure, when the coating thickness is 5 mm, C / MoS 2 The minimum reflection loss value is -33.6dB. Within the thickness range of 1.0 to 5.0mm, the effective absorption width is 12.3GHz, which can achieve 95% effective absorption of electromagnetic waves in the range of 5-18GHz.
[0068] Example 3
[0069] An electromagnetic shielding and absorbing material C / MoS 2 The preparation method comprises the following steps:
[0070] (1) taking an absorbent cotton ball, drying it under a vacuum environment, and then heat treating it under an inert atmosphere at a temperature of 600° C. for a holding time of 6 h to obtain a tubular carbon fiber having a cotton fiber structure;
[0071] (2) Sodium molybdate dihydrate (Na 2 MoO 4 ·2H 2 O) and thiourea (CH 4 N 2 S) was dissolved in deionized water to form a mixed solution, and then the tubular carbon fiber was added and stirred and mixed, and a hydrothermal reaction was carried out at 210° C. for 20 h, and then cooled to room temperature. The mixed solution contained sodium molybdate dihydrate, CH 4 N 2 The amount of S and deionized water is 2mmol:8mmol:30mL, and the amount ratio of the tubular carbon fiber to the mixed solution is 1mmol:3mL;
[0072] (3) After the thermal reaction, the product obtained by the hydrothermal reaction was separated by centrifugation at 8000 r / min for 2 min and then washed with deionized water and C 2 H 6After multiple washings to remove impurities, the mixture was dried in a drying oven at 60 °C for 24 h to obtain cotton fiber-derived C / MoS 2 A composite material, wherein the molybdenum / carbon molar ratio of the composite material is 1:5.
[0073] The results are as follows Figure 3 As shown in the figure, when the coating thickness is 4.5 mm, C / MoS 2 The minimum reflection loss value is -41.7dB. Within the thickness range of 1.0 to 5.0mm, the effective absorption width is 12.32GHz.
[0074] like Figure 6 As shown in the figure, when the coating thickness is 5 mm, C / MoS 2 The minimum reflection loss value is -28.6dB. Within the thickness range of 1.0 to 5.0mm, the effective absorption width is 12.7GHz, which can achieve 95% effective absorption of electromagnetic waves in the range of 5-18GHz.
[0075] Example 4
[0076] The magnetic shielding absorbing material C / MoS prepared in Example 1 2 For preparing the radar absorbing coating, the preparation method comprises the following steps:
[0077] (1) The absorbing material C / MoS prepared in Example 1 2 , adding the coupling agent into the solvent and performing ultrasonic dispersion to obtain a mixed solution A, wherein the ultrasonic power is 1000 W and the ultrasonic time is 30 min;
[0078] (2) adding resin material, plasticizer, dispersant and anti-settling agent to the mixed solution A and performing high-speed stirring and dispersion, the stirring rate being 1500 rpm and the stirring time being 1.5 h;
[0079] The amount of each component in the coating is 40 parts of resin material, C / MoS 2 The resin material is a mixture of epoxy resin and acrylic resin in a ratio of 1:1, the coupling agent is a titanate coupling agent, the dispersant is polyvinyl pyrrolidone, the anti-settling agent is polyethylene wax, the plasticizer is dibutyl phthalate (DBP), and the solvent is ethanol and isopropanol mixed in a volume ratio of 1:1.
[0080] Example 5
[0081] The magnetic shielding absorbing material C / MoS prepared in Example 2 2 For preparing the radar absorbing coating, the preparation method comprises the following steps:
[0082] (1) The absorbing material C / MoS prepared in Example 2 2 , adding the coupling agent into the solvent and performing ultrasonic dispersion to obtain a mixed solution A, wherein the ultrasonic power is 900 W and the ultrasonic time is 20 min;
[0083] (2) adding resin material, plasticizer, dispersant and anti-settling agent to the mixed solution A and performing high-speed stirring and dispersion, the stirring rate being 2500 rpm and the stirring time being 1 h;
[0084] The resin material is a mixture of epoxy resin and acrylic resin in a ratio of 1:1, the coupling agent is a titanate coupling agent, the dispersant is polyethylene glycol, the anti-settling agent is bentonite, the plasticizer is dioctyl phthalate (DOP), and the solvent is ionized water. The amount of each component in the coating is 45 parts of the resin material, C / MoS 2 40 parts, coupling agent 4 parts, dispersant 2 parts, dust suppressant 1 part, plasticizer 1.5 parts, solvent 45 parts.
[0085] Example 6
[0086] The magnetic shielding absorbing material C / MoS prepared in Example 2 2 For preparing the radar absorbing coating, the preparation method comprises the following steps:
[0087] (1) The absorbing material C / MoS prepared in Example 3 2 , adding the coupling agent into the solvent and performing ultrasonic dispersion to obtain a mixed solution A, wherein the ultrasonic power is 800 W and the ultrasonic time is 40 min;
[0088] (2) Adding resin material, plasticizer, dispersant and anti-settling agent to the mixed solution A and dispersing them with high-speed stirring. The stirring rate is 1800 rpm and the stirring time is 1 hour.
[0089] The resin material is a mixture of epoxy resin and acrylic resin in a ratio of 1:1, the coupling agent is a titanate coupling agent, the dispersant is polyvinyl alcohol, the anti-settling agent is polyethylene wax, the plasticizer is dibutyl phthalate (DBP), and the solvent is ethyl acetate; the amount of each component in the coating is as follows, calculated by mass:
[0090] Resin material is 42 parts, C / MoS 2 The amount of the solvent is 35 parts, the amount of the coupling agent is 2 parts, the amount of the dispersant is 1 part, the amount of the dust suppressant is 0.5 parts, the amount of the plasticizer is 1 part, and the amount of the solvent is 35 parts.
[0091] The performance of the absorbing coatings prepared in Examples 4-6 was tested. The absorbing performance of the absorbing coating fabric was tested using a vector network analyzer in a microwave darkroom using a reflectivity bow measurement method. The test angle was 15° and the test range was 2 to 18 GHz. The test was performed with reference to GJB2038-1994 "Test Method for Reflectivity of Radar Absorbing Materials". The results are shown in Table 1.
[0092] Table 1:
[0093] Corresponding coating ≤-10dB bandwidth / GHz Minimum reflection loss Corresponding frequency / GHz Example 4 5.4 -40.3 10.4 Example 5 5.2 -31.4 8.9 Example 6 4.6 -26.5 11.2
[0094] It can be seen that the cotton fiber biomass prepared by the present invention can be derived into C / MoS 2 After being prepared into a coating, its microwave absorption performance remains at a high level.
Claims
1. An electromagnetic shielding and absorbing material, characterized in that: The wave absorbing material is a cotton fiber-derived C / MoS2 composite material, specifically, cotton fiber is used as a raw material to prepare biomass-derived tubular carbon fiber, and then MoS2 is hydrothermally deposited on the surface of the biomass-derived tubular carbon fiber to form a C / MoS2 composite structure in which MoS2 wraps the tubular carbon fiber. The hydrothermally deposited MoS2 is dissolved in deionized water to form a mixed solution, and then the tubular carbon fiber is added for stirring and mixing, and a hydrothermal reaction is carried out at 190-210°C for 20-24 hours, and then cooled to room temperature. The amount of sodium molybdate dihydrate, CH4N2S and deionized water in the mixed solution is 1-2 mmol:4-8 mmol:30 mL, and the amount ratio of the tubular carbon fiber to the mixed solution is 1 mmol:3 mL.
2. The electromagnetic shielding and absorbing material according to claim 1, characterized in that: The method for preparing the biomass-derived tubular carbon fiber is to take an absorbent cotton ball and perform a heat treatment in an inert atmosphere at a temperature of 600-800° C. for a holding time of 5-6 h to obtain a tubular carbon fiber having a cotton fiber residual structure.