Carbon paper for proton exchange membrane fuel cell and preparation method thereof
By combining modified polyacrylonitrile-based carbon fiber and polyvinyl alcohol, and utilizing the chemical reaction of phenolic resin and hydroxyethyl cellulose, the problems of insufficient electrical conductivity, mechanical strength and breathability of carbon paper for proton exchange membrane fuel cells are solved. Efficient carbon paper preparation is achieved, which is suitable for gas diffusion layer materials of fuel cells.
Patent Information
- Application Number
- CN202311681467.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-12-08
AI Technical Summary
Existing carbon paper for proton exchange membrane fuel cells cannot simultaneously ensure excellent electrical conductivity, mechanical strength and air permeability, and suffers from insufficient tensile strength.
Modified polyacrylonitrile-based carbon fiber and modified polyvinyl alcohol are used as raw materials, and combined with hydroxyethyl cellulose through the esterification reaction of phenolic resin and 4-(2-amino-2-carboxyethyl)benzoic acid. Wet molding and carbonization are used to form carbon paper with excellent electrical conductivity, mechanical strength and breathability.
The electrical conductivity, mechanical strength and air permeability properties of carbon paper for proton exchange membrane fuel cells have been significantly improved. The resistivity is low, the tensile strength is high, and the air permeability is high. It is suitable for gas diffusion layer materials.
Smart Images

Figure BDA0004596305690000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to carbon paper for proton exchange membrane fuel cells and a preparation method thereof. Background Art
[0002] Fuel cells are a new and environmentally friendly power generation device that can directly convert chemical energy stored in fuel into electrical energy. Since there is no violent combustion in power generation and the conversion process is green and environmentally friendly, the use of fuel cells is an effective way to solve the current energy crisis. Among various fuel cells, proton exchange membrane fuel cells are considered to be one of the most promising power sources because of their high power density, high energy conversion efficiency, low temperature start-up, no pollution, and light size. Fuel cells produce a lot of water during operation. If there is no way to discharge it in time, it will cause flooding of the catalyst layer, block the entire battery channel, and hinder the transmission of gas. Therefore, it is particularly important to have a channel that can both effectively transmit gas and manage the water produced by the reaction.
[0003] Carbon paper is the main material of the gas diffusion layer of proton exchange membrane fuel cells. It supports catalysts and provides gas channels, electron channels and drainage channels for electrode reactions. It is one of the key components that affect electrode performance. CN114457620A discloses a carbon paper for proton exchange membrane fuel cells and a preparation method thereof. However, it has the problem of insufficient tensile strength.
[0004] In summary, after extensive searching by the applicant, at least there is a problem in the art that the existing carbon paper for proton exchange membrane fuel cells cannot simultaneously ensure excellent electrical conductivity, mechanical strength and air permeability. Therefore, it is necessary to develop or improve a carbon paper for proton exchange membrane fuel cells and a preparation method thereof. Summary of the invention
[0005] Based on this, in order to solve the problem that the existing carbon paper for proton exchange membrane fuel cells cannot simultaneously ensure excellent electrical conductivity, mechanical strength and air permeability, the present invention provides a carbon paper for proton exchange membrane fuel cells and a preparation method thereof. The specific technical scheme is as follows:
[0006] A carbon paper for proton exchange membrane fuel cells, the preparation raw materials of which include modified polyacrylonitrile-based carbon fibers and modified polyvinyl alcohol;
[0007] The raw materials for preparing the modified polyacrylonitrile-based carbon fiber include polyacrylonitrile-based carbon fiber, phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid;
[0008] The mass ratio of the polyacrylonitrile-based carbon fiber, the phenolic resin and the 4-(2-amino-2-formylethyl)benzoic acid is 95-105:5-10:3-7;
[0009] The raw materials for preparing the modified polyvinyl alcohol include polyvinyl alcohol and ethyl 4-amino-2-methylphenylacetate;
[0010] The mass ratio of the polyvinyl alcohol to ethyl 4-amino-2-methylphenylacetate is 19-21:1-2.
[0011] Furthermore, the method for preparing the modified polyacrylonitrile-based carbon fiber comprises the following steps:
[0012] The 1-10 mm polyacrylonitrile-based carbon fiber is cleaned to obtain a polyacrylonitrile-based carbon fiber precursor;
[0013] Hydrolyzing the polyacrylonitrile-based carbon fiber precursor to obtain partially hydrolyzed polyacrylonitrile-based carbon fiber;
[0014] Phenolic resin is added to ethanol, stirred at a speed of 800-900 r / min for 8-10 hours, and then partially hydrolyzed polyacrylonitrile-based carbon fiber is added, stirred evenly at a speed of 1200-1300 r / min, and then 4-(2-amino-2-formylethyl)benzoic acid is added, stirred at a speed of 1000-1200 r / min for 6-10 hours, and then the temperature is raised to 65-75°C and refluxed for reaction for 3.2-3.8 hours, and then naturally cooled, filtered and separated to obtain the modified polyacrylonitrile-based carbon fiber.
[0015] Furthermore, the cleaning process comprises the following steps:
[0016] The polyacrylonitrile-based carbon fiber is immersed in a 5-9wt% sodium hydroxide solution for 5-7h, then filtered and separated, then added to ethanol, ultrasonicated at a frequency of 70-90kHz for 30-40min, then washed with ethanol until the pH is 6.5-7.5, and then heated to 80-90°C and dried under an argon atmosphere to obtain the polyacrylonitrile-based carbon fiber precursor.
[0017] Furthermore, the hydrolysis treatment comprises the following steps:
[0018] The polyacrylonitrile-based carbon fiber precursor is added to a 15-17 wt % sodium hydroxide aqueous solution, stirred evenly at a speed of 700-800 r / min, and then heated to 62-68° C. for reaction for 25-30 min to obtain partially hydrolyzed polyacrylonitrile-based carbon fiber.
[0019] Furthermore, the preparation method of the modified polyvinyl alcohol comprises the following steps:
[0020] The polyvinyl alcohol is added into water, stirred evenly at a speed of 920-1000 r / min, then ethyl 4-amino-2-methylphenylacetate is added, the temperature is raised to 110-120° C., reacted for 2.2-2.8 hours, cooled, filtered and separated, to obtain modified polyvinyl alcohol.
[0021] The present technical solution also provides a method for preparing carbon paper, which comprises the following steps:
[0022] Add modified polyacrylonitrile-based carbon fiber into water, perform ultrasonic treatment at a frequency of 110 to 130 kHz for 15 to 25 minutes, then add modified polyvinyl alcohol, stir evenly at a speed of 1250 to 1280 r / min, then add 0.5 to 1.1 wt% hydroxyethyl cellulose aqueous solution, stir evenly, and then add into a former for wet forming to obtain carbon paper base paper;
[0023] The carbon paper base paper is immersed in the impregnation liquid for 2.2 to 2.8 hours, and then dried at 80 to 90° C. in an argon atmosphere, and then cured and carbonized in an argon atmosphere to obtain the carbon paper for proton exchange membrane fuel cells;
[0024] The mass ratio of the modified polyacrylonitrile-based carbon fiber, the modified polyvinyl alcohol and the hydroxyethyl cellulose is 98-102:5-11:1-2;
[0025] The immersion liquid includes a conductive material, a dispersant and a solvent.
[0026] Furthermore, the dispersant includes at least one of polytetrafluoroethylene, polychlorotrifluoroethylene, vinylidene fluoride-chlorotrifluoroethylene copolymer, copolymer of tetrafluoroethylene and hexafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, ethylene-chlorotrifluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer.
[0027] Furthermore, the curing treatment is carried out under the conditions of keeping the temperature at 220-280° C. for 2.1-2.5 hours;
[0028] The carbonization treatment is carried out under the conditions of keeping the temperature at 2300-2360° C. for 0.9-1.5 hours.
[0029] Further, the conductive material includes at least one of conductive carbon fiber, carbon nanotube, acetylene black, mesoporous carbon, conductive carbon black, carbon aerogel, graphite and graphene;
[0030] The solvent includes at least one of water, ethanol, ethylene glycol, acetone, glycerol, N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide and N-methylpyrrolidone.
[0031] Furthermore, the method for preparing the impregnation solution comprises the following steps:
[0032] The conductive material is added to the solvent, ultrasonicated at a frequency of 70 to 90 kHz for 30 to 40 minutes, and then the dispersant is added, and stirred evenly at a speed of 1000 to 1100 r / min to obtain the impregnation solution.
[0033] The carbon paper for proton exchange membrane fuel cells provided by the above technical solution has excellent electrical conductivity, mechanical strength and air permeability. Specifically, the partially hydrolyzed polyacrylonitrile-based carbon fiber contains abundant hydroxyl groups, the phenolic resin also contains hydroxyl groups, and the 4-(2-amino-2-formylethyl)benzoic acid contains a para-carboxyl group, which can undergo an esterification reaction with the hydroxyl group to link the polyacrylonitrile-based carbon fiber and the phenolic resin. In addition, the phenolic resin and the 4-(2-amino-2-formylethyl)benzoic acid both contain benzene rings, which can effectively form large-sized spatial channels and Large π-bond electron cloud; further, the polyvinyl alcohol modified with ethyl 4-amino-2-methylphenylacetate can also effectively link ethyl 4-amino-2-methylphenylacetate, which contains a benzene ring, an ester group and an amino group. These groups can form a larger-scale tough plane with phenolic resin and polyacrylonitrile-based carbon fiber modified with 4-(2-amino-2-formylethyl)benzoic acid during wet molding, thereby making the final carbon paper for proton exchange membrane fuel cells have excellent electrical conductivity, mechanical strength and air permeability. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.
[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0036] A carbon paper for a proton exchange membrane fuel cell in one embodiment of the present invention, the raw materials for preparing the carbon paper include modified polyacrylonitrile-based carbon fibers and modified polyvinyl alcohol;
[0037] The raw materials for preparing the modified polyacrylonitrile-based carbon fiber include polyacrylonitrile-based carbon fiber, phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid;
[0038] The mass ratio of the polyacrylonitrile-based carbon fiber, the phenolic resin and the 4-(2-amino-2-formylethyl)benzoic acid is 95-105:5-10:3-7;
[0039] The raw materials for preparing the modified polyvinyl alcohol include polyvinyl alcohol and ethyl 4-amino-2-methylphenylacetate;
[0040] The mass ratio of the polyvinyl alcohol to ethyl 4-amino-2-methylphenylacetate is 19-21:1-2.
[0041] In one embodiment, the method for preparing the modified polyacrylonitrile-based carbon fiber comprises the following steps:
[0042] The 1-10 mm polyacrylonitrile-based carbon fiber is cleaned to obtain a polyacrylonitrile-based carbon fiber precursor;
[0043] Hydrolyzing the polyacrylonitrile-based carbon fiber precursor to obtain partially hydrolyzed polyacrylonitrile-based carbon fiber;
[0044] Phenolic resin is added to ethanol, stirred at a speed of 800-900 r / min for 8-10 hours, and then partially hydrolyzed polyacrylonitrile-based carbon fiber is added, stirred evenly at a speed of 1200-1300 r / min, and then 4-(2-amino-2-formylethyl)benzoic acid is added, stirred at a speed of 1000-1200 r / min for 6-10 hours, and then the temperature is raised to 65-75°C and refluxed for reaction for 3.2-3.8 hours, and then naturally cooled, filtered and separated to obtain the modified polyacrylonitrile-based carbon fiber.
[0045] In one embodiment, the cleaning process comprises the following steps:
[0046] The polyacrylonitrile-based carbon fiber is immersed in a 5-9wt% sodium hydroxide solution for 5-7h, then filtered and separated, then added to ethanol, ultrasonicated at a frequency of 70-90kHz for 30-40min, then washed with ethanol until the pH is 6.5-7.5, and then heated to 80-90°C and dried under an argon atmosphere to obtain the polyacrylonitrile-based carbon fiber precursor.
[0047] In one embodiment, the hydrolysis process comprises the following steps:
[0048] The polyacrylonitrile-based carbon fiber precursor is added to a 15-17 wt % sodium hydroxide aqueous solution, stirred evenly at a speed of 700-800 r / min, and then heated to 62-68° C. for reaction for 25-30 min to obtain partially hydrolyzed polyacrylonitrile-based carbon fiber.
[0049] In one embodiment, the preparation method of the modified polyvinyl alcohol comprises the following steps:
[0050] The polyvinyl alcohol is added into water, stirred evenly at a speed of 920-1000 r / min, then ethyl 4-amino-2-methylphenylacetate is added, the temperature is raised to 110-120° C., reacted for 2.2-2.8 hours, cooled, filtered and separated, to obtain modified polyvinyl alcohol.
[0051] In one embodiment, the present technical solution provides a method for preparing carbon paper, which comprises the following steps:
[0052] Add modified polyacrylonitrile-based carbon fiber into water, perform ultrasonic treatment at a frequency of 110 to 130 kHz for 15 to 25 minutes, then add modified polyvinyl alcohol, stir evenly at a speed of 1250 to 1280 r / min, then add 0.5 to 1.1 wt% hydroxyethyl cellulose aqueous solution, stir evenly, and then add into a former for wet forming to obtain carbon paper base paper;
[0053] The carbon paper base paper is immersed in the impregnation liquid for 2.2 to 2.8 hours, and then dried at 80 to 90° C. in an argon atmosphere, and then cured and carbonized in an argon atmosphere to obtain the carbon paper for proton exchange membrane fuel cells;
[0054] The mass ratio of the modified polyacrylonitrile-based carbon fiber, the modified polyvinyl alcohol and the hydroxyethyl cellulose is 98-102:5-11:1-2;
[0055] The immersion liquid includes a conductive material, a dispersant and a solvent.
[0056] In one embodiment, the dispersant includes at least one of polytetrafluoroethylene, polychlorotrifluoroethylene, vinylidene fluoride-chlorotrifluoroethylene copolymer, copolymer of tetrafluoroethylene and hexafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, ethylene-chlorotrifluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer.
[0057] In one embodiment, the curing treatment condition is to keep the temperature at 220-280°C for 2.1-2.5h;
[0058] The carbonization treatment is carried out under the conditions of keeping the temperature at 2300-2360° C. for 0.9-1.5 hours.
[0059] In one embodiment, the conductive material includes at least one of conductive carbon fiber, carbon nanotube, acetylene black, mesoporous carbon, conductive carbon black, carbon aerogel, graphite and graphene;
[0060] The solvent includes at least one of water, ethanol, ethylene glycol, acetone, glycerol, N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide and N-methylpyrrolidone.
[0061] In one embodiment, the method for preparing the impregnation solution comprises the following steps:
[0062] The conductive material is added to the solvent, ultrasonicated at a frequency of 70 to 90 kHz for 30 to 40 minutes, and then the dispersant is added, and stirred evenly at a speed of 1000 to 1100 r / min to obtain the impregnation solution.
[0063] The embodiments of the present invention will be described in detail below with reference to specific examples.
[0064] Embodiment 1:
[0065] Preparation of modified polyacrylonitrile-based carbon fiber: 3 mm polyacrylonitrile-based carbon fiber is immersed in a 7 wt % sodium hydroxide solution for 6 h, then filtered and separated, then added to ethanol, ultrasonicated at a frequency of 80 kHz for 35 min, then washed with ethanol until the pH is 7, and then heated to 85 ° C under an argon atmosphere and dried to obtain a polyacrylonitrile-based carbon fiber precursor; the polyacrylonitrile-based carbon fiber precursor is added to a 16 wt % sodium hydroxide aqueous solution, stirred evenly at a speed of 750 r / min, and then heated to 65 ° C for reaction for 28 min to obtain a partially hydrolyzed polyacrylonitrile-based carbon fiber. Fiber; adding phenolic resin to ethanol, stirring at a speed of 850r / min for 9h, then adding partially hydrolyzed polyacrylonitrile-based carbon fiber, stirring evenly at a speed of 1250r / min, then adding 4-(2-amino-2-formylethyl)benzoic acid, stirring at a speed of 1100r / min for 8h, then heating to 70°C for reflux reaction for 3.5h, then cooling naturally, filtering and separating, and obtaining modified polyacrylonitrile-based carbon fiber, wherein the mass ratio of polyacrylonitrile-based carbon fiber, phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid is 100:7:5;
[0066] Preparation of modified polyvinyl alcohol: Add polyvinyl alcohol to water, stir evenly at a speed of 960 r / min, then add ethyl 4-amino-2-methylphenylacetate, heat to 115°C and react for 2.5 hours, cool and filter to separate, and obtain modified polyvinyl alcohol, wherein the mass ratio of polyvinyl alcohol to ethyl 4-amino-2-methylphenylacetate is 20:1.5;
[0067] Preparation of the impregnation solution: conductive carbon black is added to water, ultrasonicated at a frequency of 80 kHz for 35 minutes, then a 40 wt % polytetrafluoroethylene aqueous solution is added, and stirred at a speed of 1050 r / min to obtain an impregnation solution;
[0068] Preparation of carbon paper for proton exchange membrane fuel cell: add modified polyacrylonitrile-based carbon fiber into water, ultrasonicate at a frequency of 120kHz for 20 minutes, then add modified polyvinyl alcohol, stir evenly at a speed of 1270r / min, then add 0.8wt% hydroxyethyl cellulose aqueous solution, stir evenly and add into a former for wet forming to obtain carbon paper base paper; immerse the carbon paper base paper in the impregnation liquid for 2.5 hours, then dry at 85°C under an argon atmosphere, then keep warm at 250°C for 2.3 hours under an argon atmosphere for curing treatment and keep warm at 2330°C for 1.2 hours for carbonization treatment to obtain carbon paper for proton exchange membrane fuel cell, wherein the mass ratio of modified polyacrylonitrile-based carbon fiber, modified polyvinyl alcohol and hydroxyethyl cellulose is 100:8:1.5.
[0069] Embodiment 2:
[0070] The other parts are the same as those in Example 1, except that the mass ratio of polyacrylonitrile-based carbon fiber, phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid is 100:7:3, and the mass ratio of polyvinyl alcohol and ethyl 4-amino-2-methylphenylacetate is 20:1.
[0071] Embodiment 3:
[0072] The other parts are the same as those in Example 1, except that the mass ratio of polyacrylonitrile-based carbon fiber, phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid is 100:7:7, and the mass ratio of polyvinyl alcohol and ethyl 4-amino-2-methylphenylacetate is 20:2.
[0073] Comparative Example 1:
[0074] Preparation of modified polyvinyl alcohol: Add polyvinyl alcohol to water, stir evenly at a speed of 960 r / min, then add ethyl 4-amino-2-methylphenylacetate, heat to 115°C and react for 2.5 hours, cool and filter to separate, and obtain modified polyvinyl alcohol, wherein the mass ratio of polyvinyl alcohol to ethyl 4-amino-2-methylphenylacetate is 20:1.5;
[0075] Preparation of the impregnation solution: conductive carbon black is added to water, ultrasonicated at a frequency of 80 kHz for 35 minutes, then a 40 wt % polytetrafluoroethylene aqueous solution is added, and stirred at a speed of 1050 r / min to obtain an impregnation solution;
[0076] Preparation of carbon paper for proton exchange membrane fuel cells: Add polyacrylonitrile-based carbon fibers into water, ultrasonicate at a frequency of 120kHz for 20 minutes, then add modified polyvinyl alcohol, stir evenly at a speed of 1270r / min, then add 0.8wt% hydroxyethyl cellulose aqueous solution, stir evenly and add into a former for wet forming to obtain carbon paper base paper; immerse the carbon paper base paper in the impregnation liquid for 2.5 hours, then dry at 85°C under an argon atmosphere, then keep warm at 250°C for 2.3 hours under an argon atmosphere for curing treatment and keep warm at 2330°C for 1.2 hours for carbonization treatment to obtain carbon paper for proton exchange membrane fuel cells, wherein the mass ratio of polyacrylonitrile-based carbon fibers, modified polyvinyl alcohol and hydroxyethyl cellulose is 100:8:1.5.
[0077] Comparative Example 2:
[0078] Preparation of modified polyacrylonitrile-based carbon fiber: 3 mm polyacrylonitrile-based carbon fiber is immersed in a 7 wt % sodium hydroxide solution for 6 h, then filtered and separated, then added to ethanol, ultrasonicated at a frequency of 80 kHz for 35 min, then washed with ethanol until the pH is 7, and then heated to 85 ° C under an argon atmosphere and dried to obtain a polyacrylonitrile-based carbon fiber precursor; the polyacrylonitrile-based carbon fiber precursor is added to a 16 wt % sodium hydroxide aqueous solution, stirred evenly at a speed of 750 r / min, and then heated to 65 ° C for reaction for 28 min to obtain a partially hydrolyzed polyacrylonitrile-based carbon fiber. Fiber; adding phenolic resin to ethanol, stirring at a speed of 850r / min for 9h, then adding partially hydrolyzed polyacrylonitrile-based carbon fiber, stirring evenly at a speed of 1250r / min, then adding 4-(2-amino-2-formylethyl)benzoic acid, stirring at a speed of 1100r / min for 8h, then heating to 70°C for reflux reaction for 3.5h, then cooling naturally, filtering and separating, and obtaining modified polyacrylonitrile-based carbon fiber, wherein the mass ratio of polyacrylonitrile-based carbon fiber, phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid is 100:7:5;
[0079] Preparation of the impregnation solution: conductive carbon black is added to water, ultrasonicated at a frequency of 80 kHz for 35 minutes, then a 40 wt % polytetrafluoroethylene aqueous solution is added, and stirred at a speed of 1050 r / min to obtain an impregnation solution;
[0080] Preparation of carbon paper for proton exchange membrane fuel cell: add modified polyacrylonitrile-based carbon fiber into water, ultrasonicate at a frequency of 120kHz for 20 minutes, then add polyvinyl alcohol, stir evenly at a speed of 1270r / min, then add 0.8wt% hydroxyethyl cellulose aqueous solution, stir evenly and add into a former for wet forming to obtain carbon paper base paper; immerse the carbon paper base paper in the impregnation liquid for 2.5 hours, then dry at 85°C under an argon atmosphere, then keep warm at 250°C for 2.3 hours under an argon atmosphere for curing treatment and keep warm at 2330°C for 1.2 hours for carbonization treatment to obtain carbon paper for proton exchange membrane fuel cell, wherein the mass ratio of modified polyacrylonitrile-based carbon fiber, polyvinyl alcohol and hydroxyethyl cellulose is 100:8:1.5.
[0081] The carbon papers obtained in the above Examples 1 to 3 and Comparative Examples 1 to 2 were tested for electrical conductivity, mechanical strength and air permeability. The test results are shown in Table 1.
[0082] Table 1:
[0083]
[0084]
[0085] As can be seen from Table 1, since Examples 1 to 3 simultaneously use phenolic resin and polyacrylonitrile-based carbon fibers modified with 4-(2-amino-2-formylethyl)benzoic acid and polyvinyl alcohol modified with 4-amino-2-methylphenylethyl acetate, the carbon paper for proton exchange membrane fuel cells provided by the present invention has excellent electrical conductivity, mechanical strength and air permeability; specifically, the resistivity is as low as 8 or less, the tensile strength is as high as 36 MPa or more, and the air permeability is as high as 2200 or more; more specifically, the partially hydrolyzed polyacrylonitrile-based carbon fibers contain abundant hydroxyl groups, the phenolic resin also contains hydroxyl groups, and the 4-(2-amino-2-formylethyl)benzoic acid contains a para-carboxyl group, which can undergo an esterification reaction with the hydroxyl group to link the polypropylene. Nitrile-based carbon fiber and phenolic resin. In addition, both phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid contain benzene rings, which can effectively form large-size spatial channels and large π-bond electron clouds. Furthermore, polyvinyl alcohol modified with ethyl 4-amino-2-methylphenylacetate can also effectively link ethyl 4-amino-2-methylphenylacetate. Ethyl 4-amino-2-methylphenylacetate contains benzene rings, ester groups and amino groups. These groups can form a tough plane on a larger scale with phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid-modified polyacrylonitrile-based carbon fiber during wet molding, so that the finally obtained carbon paper for proton exchange membrane fuel cells has excellent conductivity, mechanical strength and air permeability.
[0086] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0087] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A carbon paper for a proton exchange membrane fuel cell, characterized in that: The raw materials for its preparation include modified polyacrylonitrile-based carbon fiber and modified polyvinyl alcohol; The raw materials for preparing the modified polyacrylonitrile-based carbon fiber include polyacrylonitrile-based carbon fiber, phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid; The mass ratio of the polyacrylonitrile-based carbon fiber, the phenolic resin and the 4-(2-amino-2-formylethyl)benzoic acid is 95-105:5-10:3-7; The raw materials for preparing the modified polyvinyl alcohol include polyvinyl alcohol and ethyl 4-amino-2-methylphenylacetate; The mass ratio of the polyvinyl alcohol to ethyl 4-amino-2-methylphenylacetate is 19-21:1-2; The preparation method of the modified polyacrylonitrile-based carbon fiber comprises the following steps: The 1-10 mm polyacrylonitrile-based carbon fiber is cleaned to obtain a polyacrylonitrile-based carbon fiber precursor; Hydrolyzing the polyacrylonitrile-based carbon fiber precursor to obtain partially hydrolyzed polyacrylonitrile-based carbon fiber; Phenolic resin is added to ethanol, stirred at a speed of 800-900 r / min for 8-10 hours, and then partially hydrolyzed polyacrylonitrile-based carbon fiber is added, stirred evenly at a speed of 1200-1300 r / min, and then 4-(2-amino-2-formylethyl)benzoic acid is added, stirred at a speed of 1000-1200 r / min for 6-10 hours, and then the temperature is raised to 65-75°C and refluxed for reaction for 3.2-3.8 hours, and then naturally cooled, filtered and separated to obtain the modified polyacrylonitrile-based carbon fiber.
2. The carbon paper according to claim 1, characterized in that The cleaning process comprises the following steps: The polyacrylonitrile-based carbon fiber is immersed in a 5-9wt% sodium hydroxide solution for 5-7h, then filtered and separated, then added to ethanol, ultrasonicated at a frequency of 70-90kHz for 30-40min, then washed with ethanol until the pH is 6.5-7.5, and then heated to 80-90°C and dried under an argon atmosphere to obtain the polyacrylonitrile-based carbon fiber precursor.
3. The carbon paper according to claim 1, characterized in that The hydrolysis treatment comprises the following steps: The polyacrylonitrile-based carbon fiber precursor is added to a 15-17 wt % sodium hydroxide aqueous solution, stirred evenly at a speed of 700-800 r / min, and then heated to 62-68° C. for reaction for 25-30 min to obtain partially hydrolyzed polyacrylonitrile-based carbon fiber.
4. The carbon paper according to claim 1, characterized in that The preparation method of the modified polyvinyl alcohol comprises the following steps: The polyvinyl alcohol is added into water, stirred evenly at a speed of 920-1000 r / min, then ethyl 4-amino-2-methylphenylacetate is added, the temperature is raised to 110-120° C., reacted for 2.2-2.8 hours, cooled, filtered and separated, to obtain modified polyvinyl alcohol.
5. The method for preparing carbon paper according to claim 1, characterized in that: It includes the following steps: Add modified polyacrylonitrile-based carbon fiber into water, perform ultrasonic treatment at a frequency of 110 to 130 kHz for 15 to 25 minutes, then add modified polyvinyl alcohol, stir evenly at a speed of 1250 to 1280 r / min, then add 0.5 to 1.1 wt% hydroxyethyl cellulose aqueous solution, stir evenly, and then add into a former for wet forming to obtain carbon paper base paper; The carbon paper base paper is immersed in the impregnation liquid for 2.2 to 2.8 hours, and then dried at 80 to 90° C. in an argon atmosphere, and then cured and carbonized in an argon atmosphere to obtain the carbon paper for proton exchange membrane fuel cells; The mass ratio of the modified polyacrylonitrile-based carbon fiber, the modified polyvinyl alcohol and the hydroxyethyl cellulose is 98-102:5-11:1-2; The immersion liquid includes a conductive material, a dispersant and a solvent.
6. The preparation method according to claim 5, characterized in that: The dispersant includes at least one of polytetrafluoroethylene, polychlorotrifluoroethylene, vinylidene fluoride-chlorotrifluoroethylene copolymer, copolymer of tetrafluoroethylene and hexafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, ethylene-chlorotrifluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer.
7. The preparation method according to claim 5, characterized in that: The curing treatment condition is to keep the temperature at 220-280°C for 2.1-2.5h; The carbonization treatment is carried out under the conditions of keeping the temperature at 2300-2360° C. for 0.9-1.5 hours.
8. The preparation method according to claim 5, characterized in that: The conductive material comprises at least one of conductive carbon fiber, carbon nanotube, acetylene black, mesoporous carbon, conductive carbon black, carbon aerogel, graphite and graphene; The solvent includes at least one of water, ethanol, ethylene glycol, acetone, glycerol, N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide and N-methylpyrrolidone.
9. The preparation method according to claim 5, characterized in that: The preparation method of the impregnation liquid comprises the following steps: The conductive material is added to the solvent, ultrasonicated at a frequency of 70 to 90 kHz for 30 to 40 minutes, and then the dispersant is added, and stirred evenly at a speed of 1000 to 1100 r / min to obtain the impregnation solution.
Citation Information
Patent Citations
Carbon paper for proton exchange membrane fuel cell and preparation method thereof
CN114457620A
Porous electrode base material and process for producing the same
CN101002354A
Composite conductive paper of carbon fiber
CN101003956A
Gas diffusion layer for proton exchange membrane fuel cells and preparation method thereof
CN101771155A
High-performance carbon paper for fuel cell and preparation method and application thereof
CN110512459A