Primer coating composition and coating film

By using a primer coating composition of a specific composition, a coating composition containing acrylic resin and epoxy resin, the problem of poor adhesion between the anti-corrosion coating composition and the topcoat film is solved, the coating time is extended and the coating composition is inhibited. The shrinkage phenomenon improves the efficiency and anti-corrosion properties of the coating process.

CN117730124BActive Publication Date: 2024-10-18NIPPON PAINT MARINE COATINGS CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202380012571.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-19
Publication Date
2024-10-18
Estimated Expiration
2043-07-19

AI Technical Summary

Technical Problem

When applying topcoat paint with existing anti-corrosion coating compositions, the adhesion may be poor, or the coating time may need to be shortened to ensure adhesion, resulting in complicated processes and harsh operating environments.

Method used

A primer coating composition containing an acrylic resin and an epoxy resin is used. The dissolution parameter and weight average molecular weight of the acrylic resin are within a specific range, combined with an amine curing agent and a curing accelerator to form a two-liquid coating composition. Forms a primer coating to improve adhesion and shrinkage resistance.

Benefits of technology

It is possible to maintain good adhesion of the topcoat film while extending the application time of the topcoat, effectively inhibit shrinkage, and improve the feasibility and anti-corrosion performance of the coating process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004634398030000121
    Figure BDA0004634398030000121
  • Figure BDA0004634398030000131
    Figure BDA0004634398030000131
  • Figure BDA0004634398030000181
    Figure BDA0004634398030000181
Patent Text Reader

Abstract

Provided is a primer coating composition, comprising an acrylic resin and an epoxy resin, wherein the acrylic resin has a solubility parameter of 9.0 to 12 and a weight average molecular weight of 1000 to 95000; the epoxy resin has a solubility parameter of 10 to 12 and a weight average molecular weight of 250 to 2500.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a coating composition for primers, a coating film formed from the coating composition for primers, and an article having the coating film. Background Art

[0002] Generally, in order to provide ships and the like with corrosion resistance in severe corrosive environments, an anticorrosive coating is applied to their surfaces. In many cases, an antifouling coating is repeatedly applied on top of the anticorrosive coating. For example, Japanese Patent Publication No. 2009-197106 (Patent Document 1) discloses an anticorrosive coating composition containing a bisphenol epoxy resin, (b) an ethylene-vinyl acetate copolymer, and (c) an amine curing agent.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2009-197106 Summary of the invention

[0006] Problems to be solved by the invention

[0007] In the past, when a topcoat is applied on an object after applying the anticorrosive coating composition, if the time from applying the anticorrosive coating composition to applying the topcoat is long, the adhesion between the coating film formed by the anticorrosive coating composition and the topcoat coating film may be poor. On the other hand, if the above time is shortened in order to ensure the adhesion to the topcoat coating film, the coating operation process becomes complicated or a harsh working environment is imposed on the coating operator.

[0008] The object of the present invention is to provide a new coating composition for primer, which can form a coating film with good adhesion to the topcoat coating film even if the time until the topcoat coating is applied is long, in other words, the time until the topcoat coating is applied can be extended while maintaining good adhesion to the topcoat coating film. Another object of the present invention is to provide a coating film formed using the coating composition for primer, an article having the coating film (primer coating film), and a method for forming a coating film using the coating composition for primer.

[0009] Means of solving problems

[0010] The present invention provides the following coating composition for primer, coating film, method for forming a coating film, method for forming a multilayer coating film, and article.

[0011] [1] A coating composition for a primer, comprising an acrylic resin and an epoxy resin, wherein the acrylic resin has a solubility parameter of 9.0 to 12 and a weight average molecular weight of 1,000 to 95,000; and the epoxy resin has a solubility parameter of 10 to 12 and a weight average molecular weight of 250 to 2,500.

[0012] [2] The primer coating composition according to [1], wherein the content of the acrylic resin is 4 parts by mass or more and 60 parts by mass or less relative to 100 parts by mass of the epoxy resin.

[0013] [3] The primer coating composition according to [1] or [2], further comprising an amine curing agent.

[0014] [4] The primer coating composition according to [3], further comprising a curing accelerator, wherein the content of the curing accelerator is 0.1 parts by mass or more and 16 parts by mass or less relative to 100 parts by mass of the epoxy resin.

[0015] [5] The primer coating composition according to [3] or [4] is a two-component primer coating composition comprising a first component and a second component, wherein the first component contains the acrylic resin and the epoxy resin, and the second component contains the amine curing agent.

[0016] [6] The primer coating composition according to any one of [1] to [5], further comprising mica, wherein the content of the mica is 2 parts by mass or more and 95 parts by mass or less relative to 100 parts by mass of the total content of the acrylic resin and the epoxy resin.

[0017] [7] A coating film formed from the primer coating composition according to any one of [1] to [6].

[0018] [8] A method for forming a coating film, comprising the step of forming a primer coating film on a substrate using the primer coating composition according to any one of [1] to [6].

[0019] [9] A method for forming a multilayer coating film, comprising: a step of forming a primer coating film on a substrate using the primer coating composition described in any one of [1] to [6]; and a step of forming a topcoat coating film on the primer coating film using a topcoat coating composition.

[0020]

[10] An article having a primer coating film formed from the primer coating composition according to any one of [1] to [6].

[0021]

[11] The article according to

[10] , further comprising a topcoat film on the primer film.

[0022] Effects of the Invention

[0023] A coating composition for primer can be provided, which can form a coating film having good adhesion to the topcoat coating even if the time until the topcoat coating is applied is long, in other words, the time until the topcoat coating is applied can be extended while maintaining good adhesion to the topcoat coating. In addition, a coating film formed using the coating composition for primer, an article having the coating film (primer coating film), and a method for forming a coating film using the coating composition for primer can be provided.

[0024] The primer coating composition of the present invention is useful as an anticorrosion coating composition suitable for articles such as marine structures such as bridges, tanks, and plants, in addition to ships. DETAILED DESCRIPTION

[0025] <Coating composition for primer>

[0026] Primer coating composition of the present invention (hereinafter, also referred to as "coating composition") comprises specific acrylic resin (A) and specific epoxy resin (B). Below, even if the time until the topcoat coating is applied is long, the coating film with good adhesion relative to the topcoat coating film can be formed, in other words, the characteristic of the time until the topcoat coating is applied while maintaining good adhesion relative to the topcoat coating film is called "excellent interval adhesion". According to the present invention, a coating composition with excellent interval adhesion can be provided.

[0027] In addition, according to the present invention, a coating composition having excellent interval adhesion and excellent shrinkage resistance can also be provided. Excellent shrinkage resistance means that when a topcoat film is further formed on a coating film (anticorrosion coating film) formed by the coating composition, the ability to suppress a phenomenon called shrinkage (also called lifting) is high. The so-called shrinkage phenomenon generally refers to a phenomenon in which wrinkles are generated in the primer film when the coating film is recoated, and the topcoat film formed thereon bulges together.

[0028] For example, in the case of film repairing of a structure (ships, etc.) having a film, sometimes, on the outermost old topcoat film located on the structure, a primer coating composition (anticorrosive coating composition) is used to form a primer film, and then a topcoat film is formed thereon. At this time, if a previous primer coating composition is used, shrinkage may occur sometimes. According to the primer coating composition of the present invention, this shrinkage can be effectively suppressed. It is believed that the reason for effectively suppressing shrinkage is that the coating composition comprises a specific acrylic resin (A) and a specific epoxy resin (B), and thus, the above-mentioned primer film is effectively suppressed: when a topcoat film is formed on the primer film formed by the coating composition, the solvent contained in the used topcoat coating composition oozes out to the topcoat film under the above-mentioned primer film, and the topcoat film is redissolved.

[0029] Hereinafter, the components contained or which may be contained in the coating composition will be described in detail.

[0030] (1) Acrylic resin

[0031] The acrylic resin contained in the coating composition is preferably a thermoplastic acrylic resin. Examples of the thermoplastic acrylic resin include (meth)acrylic acid homopolymers or (meth)acrylic acid copolymers containing structural units derived from (meth)acrylic acid esters. In this specification, "(meth)acrylic acid" means at least one of methacrylic acid and acrylic acid. In addition, in this specification, the acrylic resin includes a polymer that does not contain structural units derived from acrylates but contains structural units derived from methacrylates.

[0032] Examples of the (meth)acrylate include: (meth)acrylate chain or branched aliphatic esters (preferably (meth)acrylate chain or branched alkyl esters) having an ester portion having a carbon number of 1 to 20, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate; 2-hydroxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, (meth)acrylate alkyl esters containing a hydroxyl group having an ester portion having a carbon number of 1 or more and 20 or less, such as (meth)acrylate, propyl ester, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc.; (meth)acrylate aryl esters, such as (meth)acrylate, benzyl (meth)acrylate, etc.; (meth)acrylate alicyclic esters (for example, (meth)acrylate cycloalkyl esters), such as (meth)acrylate cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, etc.; (meth)acrylate aminoalkyl esters, such as (meth)acrylate N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, etc. The acrylic resin may contain a structural unit derived from one or more types of (meth)acrylate.

[0033] The (meth)acrylate forming the acrylic resin is preferably a (meth)acrylate not having a cycloalkyl group. By using an acrylic resin formed from a (meth)acrylate not having a cycloalkyl group, the spacer adhesion can be made more excellent. Examples of the (meth)acrylate not having a cycloalkyl group include (meth)acrylates other than the alicyclic (meth)acrylates exemplified above.

[0034] The acrylic resin may contain structural units derived from monomers other than (meth)acrylates. Examples of monomers other than (meth)acrylates include: unsaturated monobasic acids, such as (meth)acrylic acid, cinnamic acid, crotonic acid, etc.; unsaturated dibasic acids and their monoalkyl esters, such as maleic acid, fumaric acid, itaconic acid, and their monoalkyl esters; unsaturated monobasic acid hydroxyalkyl ester dibasic acid adducts, such as maleic acid adducts of 2-hydroxyethyl (meth)acrylate, phthalic acid adducts of 2-hydroxyethyl (meth)acrylate, succinic acid adducts of 2-hydroxyethyl (meth)acrylate, etc.; polymerizable unsaturated esters other than (meth)acrylates, such as crotonates, maleic acid diesters, itaconic acid diesters, etc.; other polymerizable vinyl compounds, such as (meth)acrylamide, (meth)acrylonitrile, styrene, α-methylstyrene, o-, m- or p-methylstyrene, vinyl acetate, vinyl chloride, vinyl propionate, vinyl benzoate, vinyl toluene, etc. The acrylic resin may contain one or two or more structural units derived from a monomer other than (meth)acrylic acid ester.

[0035] The acrylic resin can be prepared by heating a monomer composition in the presence of a free radical polymerization initiator. Examples of the free radical polymerization initiator include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), benzoyl peroxide, cumene hydroperoxide, lauryl peroxide, di-tert-butyl peroxide, and tert-butyl peroxy-2-ethylhexanoate.

[0036] Examples of the polymerization method include solution polymerization in an organic solvent. Examples of the organic solvent include aromatic hydrocarbon organic solvents such as toluene and xylene; ketone organic solvents such as methyl ethyl ketone and methyl isobutyl ketone; ester organic solvents such as butyl acetate; alcohol organic solvents such as isopropanol; aliphatic hydrocarbons such as mineral spirits, n-hexane, n-octane, 2,2,2-trimethylpentane, isooctane, n-nonane, cyclohexane, and methylcyclohexane. These can be used alone or in combination.

[0037] The coating composition includes an acrylic resin (A) having a solubility parameter SP (hereinafter, also referred to as "SP") of 9.0 to 12 and a weight average molecular weight (hereinafter, also referred to as "Mw") of 1000 to 95000. On the premise that the coating composition includes a specific epoxy resin (B) described later, the coating composition includes an acrylic resin (A), which can improve the spacing adhesion and further improve the shrinkage resistance. In this specification, the weight average molecular weight refers to a value obtained by converting the molecular weight measured by gel permeation chromatography (GPC) based on the molecular weight of polystyrene. The coating composition may include two or more acrylic resins (A).

[0038] From the viewpoint of improving the inter-space adhesion and further improving the shrinkage resistance, the SP of the acrylic resin (A) is preferably 9.2 to 12, more preferably 9.4 to 12, further preferably 9.5 to 11.8, and further preferably 9.5 to 11.6.

[0039] In the present specification, the solubility parameter SP of a resin can be measured by the following method (reference: SUH, CLARKE, JPSA-1, 5, 1671 to 1681 (1967)).

[0040] At a measurement temperature of 20°C, weigh 0.5g of resin into a 100mL beaker, add 10mL of a good solvent (acetone) using a hole pipette, and dissolve it using a magnetic stirrer to prepare a dilute solution. Next, use a 50mL burette to slowly drop a low SP poor solvent (n-hexane) into the dilute solution, and take the point at which the dilute solution becomes turbid as the amount of low SP poor solvent added. In addition, slowly drop a high SP poor solvent (ion exchange water) into the above-mentioned dilute solution, and take the point at which the dilute solution becomes turbid as the amount of high SP poor solvent added. The SP value can be calculated by the known calculation method described in the above-mentioned references, etc., from the amount of each of the above-mentioned poor solvents added until the turbidity point is reached.

[0041] The SP of the acrylic resin (A) can be controlled by adjusting the type and amount of the monomers constituting the acrylic resin (A). For example, when a monomer having a polar group (e.g., (meth)acrylic acid, 2-hydroxyethyl (meth)acrylate, etc.) is used, the SP of the acrylic resin (A) tends to increase, and when a monomer such as an alkyl (meth)acrylate is used, the SP of the acrylic resin (A) tends to decrease.

[0042] From the viewpoint of obtaining a coating composition with a moderate viscosity and improving the curability of the coating composition, the Mw of the acrylic resin (A) is preferably 5000 or more, more preferably 10000 or more, further preferably 30000 or more, and further preferably 50000 or more. From the viewpoint of obtaining a coating composition with a moderate viscosity and improving the compatibility with the epoxy resin, the Mw of the acrylic resin (A) is preferably 90000 or less, more preferably 78000 or less. From the viewpoint of improving the spacer adhesion and / or shrinkage resistance, it is also advantageous for the Mw of the acrylic resin (A) to be within the above range. If the Mw of the acrylic resin (A) is too large, shrinkage cannot be fully suppressed.

[0043] From the viewpoint of improving the spacer adhesion and shrinkage resistance, the glass transition temperature (hereinafter, also referred to as "Tg") of the acrylic resin (A) is preferably 40°C to 90°C, more preferably 42°C to 88°C, further preferably 45°C to 85°C, further preferably 50°C to 80°C, particularly preferably 55°C to 75°C, and most preferably 60°C to 72°C. If the Tg of the acrylic resin (A) is lower than 40°C, the coating film is easily softened, and therefore, there is a disadvantageous tendency in improving the spacer adhesion and shrinkage resistance. In addition, if the Tg of the acrylic resin (A) exceeds 90°C, the coating film is easily cracked, and therefore, there is a disadvantageous tendency in improving the spacer adhesion and shrinkage resistance.

[0044] In this specification, the glass transition temperature is a temperature measured using a differential scanning calorimeter (DSC) in accordance with JIS K 7121.

[0045] The coating composition may also contain an acrylic resin (A') other than the acrylic resin (A). However, from the viewpoint of improving the spacer adhesion and shrinkage resistance, the content of the acrylic resin (A') is preferably small. The content of the acrylic resin (A') in the coating composition is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, further preferably 10 parts by mass or less, further preferably 5 parts by mass or less, particularly preferably 2 parts by mass or less, and most preferably 0 parts by mass, relative to 100 parts by mass of the acrylic resin (A).

[0046] The content of the acrylic resin (A) in the coating composition is preferably 1.0% by mass or more and 40% by mass or less, more preferably 1.3% by mass or more and 20% by mass or less, and further preferably 2.0% by mass or more and 18% by mass or less, in the solid content contained in the coating composition. If the content of the acrylic resin (A) is less than 1.0% by mass, the improvement of the spacing adhesion and / or shrinkage resistance may become insufficient. The solid content contained in the coating composition refers to the total of the components other than the solvent contained in the coating composition.

[0047] The content of the acrylic resin (A) in the coating composition is usually 4 parts by mass or more and 60 parts by mass or less relative to 100 parts by mass of the epoxy resin (B) described later, and is preferably 10 parts by mass or more and 60 parts by mass or less, more preferably 10 parts by mass or more and 55 parts by mass or less, further preferably 15 parts by mass or more and 55 parts by mass or less, further preferably 20 parts by mass or more and 50 parts by mass or less, and particularly preferably 25 parts by mass or more and 45 parts by mass or less from the viewpoint of improving the spacer adhesion.

[0048] (2) Epoxy resin

[0049] As the epoxy resin contained in the coating composition, for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD ​​type epoxy resin, bisphenol S type epoxy resin, biphenyl type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, rubber modified epoxy resin, etc. can be listed. Among them, bisphenol A type epoxy resin is preferred. By using bisphenol A type epoxy resin (A), the curability of the coating composition can be improved, and the adhesion to the substrate can be made good.

[0050] The coating composition includes an epoxy resin (B) having a solubility parameter of 10 to 12 and a weight average molecular weight of 250 to 2500. On the premise that the coating composition includes the acrylic resin (A), the coating composition includes the epoxy resin (B), which can improve the spacer adhesion and further improve the shrinkage resistance. The coating composition may include two or more epoxy resins (B).

[0051] From the viewpoint of compatibility with the acrylic resin (A), the SP of the epoxy resin (B) is preferably 10.2 to 12, more preferably 10.4 to 12, further preferably 10.5 to 11.8, and still further preferably 10.6 to 11.6.

[0052] From the viewpoint of improving the intermittent adhesion, the absolute value of the difference between the SP of the acrylic resin (A) and the SP of the epoxy resin (B) is preferably within a range of 2.5 or less.

[0053] From the viewpoint of improving the spacer adhesion and further improving the shrinkage resistance, the Mw of the epoxy resin (B) is preferably 250 to 2200, more preferably 300 to 2000, further preferably 350 to 1800, and further preferably 350 to 1500. In addition, when the Mw of the epoxy resin (B) is within the above range, it is easy to obtain a coating composition having excellent coating film properties and coating workability.

[0054] The epoxy equivalent of the epoxy resin (B) is preferably 100 or more and 3000 or less, more preferably 150 or more and 1000 or less, and further preferably 180 or more and 500 or less. If the epoxy equivalent is 100 or more, there is a tendency to easily obtain good curability, and the toughness of the obtained coating film tends to become good. If the epoxy equivalent exceeds 3000, there is a tendency that the curability deteriorates and the coating film tends to harden.

[0055] The coating composition may also contain an epoxy resin (B') other than the epoxy resin (B). However, from the viewpoint of improving the spacer adhesion and shrinkage resistance, the content of the epoxy resin (B') is preferably small. The content of the epoxy resin (B') in the coating composition is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, further preferably 10 parts by mass or less, further preferably 5 parts by mass or less, particularly preferably 2 parts by mass or less, and most preferably 0 parts by mass, relative to 100 parts by mass of the epoxy resin (B).

[0056] The content of the epoxy resin (B) in the coating composition is preferably 10% by mass or more and 55% by mass or less, more preferably 13% by mass or more and 52% by mass or less, and further preferably 15% by mass or more and 45% by mass or less, based on the solid content of the coating composition. If the content of the epoxy resin (B) is less than 10% by mass, the curability of the coating composition may become insufficient.

[0057] (3) Amine curing agent

[0058] The coating composition may contain an amine curing agent. The amine curing agent is a curing agent for curing epoxy resin. Examples of the amine curing agent include polyamine curing agents, modified polyamine curing agents, polyamide curing agents, modified polyamide curing agents, and the like. The coating composition may contain one or more amine curing agents.

[0059] Examples of polyamine curing agents include aliphatic polyamines (m-xylene diamine, isophorone diamine, diethylene triamine, triethylene tetramine, diamino diphenyl methane, etc.); alicyclic polyamines; aromatic polyamines, etc. Modified polyamine curing agents are modified products of the above-mentioned polyamines, and examples thereof include aliphatic, alicyclic or aromatic polyamines modified by epoxide addition, Michael addition, Mannich addition, thiourea addition, acrylonitrile addition, ketone end-capping, etc.

[0060] Examples of polyamide curing agents include polyamide amines which are generated by condensation of dimer acid and polyamine and have reactive primary and secondary amino groups in the molecule. The polyamines forming the polyamide amines may be the above-mentioned aliphatic polyamines, alicyclic polyamines, aromatic polyamines, and the like.

[0061] The modified polyamide-based curing agent is a modified product of polyamide, and examples thereof include epoxy adducts obtained by adding an epoxy compound to polyamide, and Mannich-modified products of modified polyamide.

[0062] The coating composition may contain an amine curing agent and a curing accelerator. As the curing accelerator, a tertiary amine curing accelerator may be cited. As the tertiary amine curing accelerator, for example, 2,4,6-tris(dimethylaminomethyl)phenol (TAP), dimethylaminoethanol (DMAE), N,N-dimethylaniline (DMA), triethanolamine, triethylenediamine (1,4-diazabicyclo(2,2,2)octane) and the like may be cited.

[0063] From the viewpoint of improving the interval adhesion and then improving the shrinkage resistance, in addition, from the viewpoint of corrosion resistance, curability and adhesion to the substrate, the amine curing agent preferably includes polyamide amine. In addition, from the same viewpoint, the polyamide amine is preferably an aliphatic polyamide amine as a condensate of dimer acid and aliphatic polyamines. More preferably, the amine curing agent is composed of polyamide amine only. On the other hand, from the viewpoint of further improving the interval adhesion, the amine curing agent preferably does not contain aminosilane.

[0064] The amine equivalent of the amine curing agent is usually 50 or more and 1000 or less, preferably 50 or more and 800 or less, more preferably 60 or more and 655 or less, and further preferably 70 or more and 500 or less. When the amine equivalent of the amine curing agent is within the above range, a coating composition having excellent adhesion to the spacer, shrinkage resistance, corrosion resistance, curability, and adhesion to the substrate can be easily obtained.

[0065] From the viewpoint of improving the interval adhesion and further improving the shrinkage resistance, in addition, from the viewpoint of curability and adhesion to the substrate, the coating composition preferably contains a polyamide amine curing agent and a tertiary amine curing accelerator. In addition, from the same viewpoint, the polyamide amine curing agent is preferably an aliphatic polyamide amine which is a condensate of a dimer acid and an aliphatic polyamine.

[0066] When the coating composition contains a polyamide amine curing agent and a tertiary amine curing accelerator, from the viewpoint of suppressing a decrease in corrosion resistance, the content ratio of the polyamide amine curing agent to the tertiary amine curing accelerator is preferably 2 / 1 to 240 / 1, more preferably 3 / 1 to 50 / 1, and even more preferably 4 / 1 to 30 / 1.

[0067] The content of the amine curing agent in the coating composition is preferably 20 parts by mass or more and 60 parts by mass or less, more preferably 25 parts by mass or more and 55 parts by mass or less, and further preferably 30 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the content of the epoxy resin (B), from the viewpoints of interlayer adhesion, shrinkage resistance, corrosion resistance, curability, and adhesion to the substrate.

[0068] When the amine curing agent contains polyamide amine, the content of polyamide amine in the coating composition is preferably 20 parts by mass or more and 60 parts by mass or less, more preferably 25 parts by mass or more and 55 parts by mass or less, and further preferably 30 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the content of the epoxy resin (B), from the viewpoints of interval adhesion, shrinkage resistance, corrosion resistance, curability and adhesion to the substrate.

[0069] When the amine curing agent contains a curing accelerator such as a tertiary amine curing accelerator, the content of the curing accelerator in the coating composition is preferably 0.1 part by mass or more and 16 parts by mass or less, more preferably 0.5 part by mass or more and 15 parts by mass or less, and further preferably 1 part by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the content of the epoxy resin (B).

[0070] (4) Other components that may be contained in the coating composition

[0071] The coating composition may contain one or more other ingredients other than the above. As other ingredients, for example, pigments, silane coupling agents, defoamers, anti-sagging agents, plasticizers, antifouling agents, water-binding agents, anti-color separation agents, anti-settling agents, coating film consumption regulators, ultraviolet absorbers, surface regulators, viscosity regulators, leveling agents, pigment dispersants, solvents, etc. These ingredients can be used alone or in combination of two or more.

[0072] Examples of the pigment include coloring pigments, extender pigments, and rust-proof pigments. Examples of the coloring pigment include titanium oxide, carbon black, lead white, graphite, zinc sulfide, zinc oxide (zinc white), chromium oxide, yellow nickel titanium, yellow chromium titanium, yellow iron oxide, red iron oxide, black iron oxide, phthalocyanine blue, phthalocyanine green, ultramarine blue, benzimidazolone yellow, quinacridone red, and azo red / yellow pigments. Two or more coloring pigments may be used.

[0073] Examples of the extender pigment include mica (suzorite-mica, kurarite-mica, etc.), talc, clay, bentonite, calcium carbonate, magnesium carbonate, barium sulfate, silicic acid, silicates, feldspar, alumina, white silica, alumina hydrate, calcium sulfate, micaceous iron oxide (MIO), glass flakes, etc. Two or more extender pigments may be used.

[0074] Among them, the coating composition preferably contains mica. The inclusion of mica is conducive to the improvement of interval adhesion and shrinkage resistance. From the viewpoint of improving interval adhesion and shrinkage resistance, the aspect ratio of mica is preferably 7.5 or more. If the aspect ratio is within the above range, since the exudation of the above solvent can be more effectively suppressed, the shrinkage resistance can be further improved.

[0075] The aspect ratio is obtained by randomly selecting 20 particles from a microscope observation image containing 20 or more particles and calculating the average value of the aspect ratios of the 20 particles. The aspect ratio is the value obtained by dividing the major axis of a particle by its thickness.

[0076] When the coating composition contains mica, the content of mica in the coating composition is preferably 2 parts by mass or more and 95 parts by mass or less, more preferably 3 parts by mass or more and 90 parts by mass or less, and further preferably 5 parts by mass or more and 65 parts by mass or less, relative to 100 parts by mass of the total content of the acrylic resin (A) and the epoxy resin (B).

[0077] Examples of the rust-proof pigment include zinc molybdate, aluminum molybdate, lead cyanamide, red lead, lead oxide, zinc chromate, zinc powder (Zn), basic lead chromate, basic lead sulfate, calcium plumbate, aluminum tripolyphosphate, zinc phosphate, calcium phosphate, aluminum powder (Al), hemihydrate gypsum, etc. Two or more rust-proof pigments may be used.

[0078] Preferred examples of the silane coupling agent are alkoxysilane compounds. Examples of the alkoxysilane compound include γ-glycidyloxyalkyltrialkoxysilanes such as γ-glycidyloxypropyltrimethoxysilane and γ-glycidyloxypropyltriethoxysilane.

[0079] The coating composition may contain two or more silane coupling agents. By containing a silane coupling agent, it is possible to improve the interlayer adhesion, shrinkage resistance, corrosion resistance, curability, adhesion to the substrate, and the like.

[0080] When the coating composition contains a silane coupling agent, the content of the silane coupling agent in the coating composition is preferably 0.5 parts by mass or more and 20 parts by mass or less, more preferably 0.75 parts by mass or more and 15 parts by mass or less, and further preferably 1 part by mass or more and 10 parts by mass or less, based on 100 parts by mass of the total content of the acrylic resin (A) and the epoxy resin (B).

[0081] As the solvent, for example, the following can be listed: hydrocarbons, such as toluene, xylene, ethylbenzene, cyclopentane, octane, heptane, cyclohexane, petroleum solvent, etc.; ethers, such as dioxane, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol dibutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, butyl cellosolve, etc.; esters, such as butyl acetate, propyl acetate, benzyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, etc.; ketones, such as ethyl isobutyl ketone, methyl isobutyl ketone, etc.; alcohols, such as n-butanol, propanol, etc.

[0082] <Preparation of primer coating composition>

[0083] The primer coating composition of the present invention can be prepared in the same manner as a conventional anticorrosive coating using an epoxy resin. The coating composition is preferably a two-component coating composition. The two-component coating composition is preferably composed of a first agent (main agent) containing at least an acrylic resin and an epoxy resin and a second agent (curing agent) containing at least an amine curing agent. Both the first agent and the second agent may contain a solvent. The second agent preferably contains a curing accelerator such as a tertiary amine curing accelerator. In a two-component coating composition, the first agent and the second agent are usually mixed when about to be used and applied to the object to be coated.

[0084] In the two-component coating composition, the acrylic resin, mica and other mixed components may be mixed in either the first component or the second component, or may be mixed in both. Usually, the acrylic resin and mica are mixed in the first component.

[0085] <Application of primer coating composition>

[0086] The coating composition can be applied to the object by conventional methods such as brushes, rollers, sprays, etc. In the case of a two-component coating composition, the coating composition obtained by mixing the first agent and the second agent just before use is applied using the above method. After the first agent and the second agent are mixed, the coating composition obtained by mixing the first agent and the second agent is applied to the object within the usable time. The coating composition of the present invention typically shows a usable time of about 30 minutes to 8 hours. After coating, a drying treatment can be performed to form an anticorrosive coating film. The drying temperature is usually room temperature (about 20 to 35°C), but it can also be performed at a lower temperature.

[0087] The object to be coated (the object to be coated with the coating composition) is not particularly limited as long as it is an object to be coated that needs to be protected from corrosion, and may be, for example, a ship (the inner surface of the ballast tank of the ship, the bottom of the ship, the outer plate, etc.), and may also be an object such as a bridge, a storage tank, a complete set of equipment (petroleum complete set of equipment, etc.), a pipeline, and other marine structures. The material of the surface of the object to be coated with the coating composition may be, for example, a ferrous metal such as steel, a non-ferrous metal, concrete, an old coating film, and the like formed by the coating. The old coating film refers to a paint film or a part thereof that has been formed and used before.

[0088] The coating composition can be suitably applied to the formation method of the coating film of the process of forming a primer coating film on the substrate (the surface of the coated object).For example, the coating composition can be suitably applied to the manufacture method of the multilayer coating film of the process of forming a primer coating film on the substrate and the process of forming a topcoat coating film on the primer coating film.In these methods, the coating composition can be used to form a primer coating film.The primer coating film can be the laminated structure of multiple coating films, in which case, the coating composition of the present invention is preferably at least used for the formation of the most superficial (connected with the topcoat coating film) primer coating film.

[0089] The surface of the object to be coated, which is the base of the primer coating formed by the coating composition, may be a surface of a coating film coated with rust-proof coating, pre-coating, organic or inorganic zinc primer, etc. The surface of the object to be coated may be sandblasted.

[0090] The film thickness of the anticorrosion coating formed by the coating composition can be appropriately set according to the type and purpose of the coated object, and is usually calculated as 10 μm or more and 500 μm or less in terms of dry film thickness. In addition, the anticorrosion coating formed by the coating composition can also form a dry coating with a desired film thickness by repeatedly applying the composition multiple times. There is no particular restriction on the amount of coating at this time, and the coating is usually applied in a manner that the dry film thickness of each coating is 10 μm or more and 500 μm or less. In the case of repeated application, it is possible to form a multi-layer wet coating by repeated application and then dry it to obtain a coating with a desired film thickness, or it is possible to obtain a dry coating with a desired film thickness by forming a multi-layer dry coating.

[0091] As the topcoat coating used for the topcoat film formed on the anticorrosion coating film, the topcoat coating conventionally used in the anticorrosion coating can be used. Specific examples of topcoat coatings include: oily coatings, long oil-based phthalic acid resin coatings, silicone alkyd resin coatings, phenolic resin coatings, chlorinated rubber resin coatings, epoxy resin coatings, modified epoxy resin coatings, tar epoxy resin coatings, vinyl chloride resin coatings, polyurethane resin coatings, fluororesin coatings, siloxane modified resin coatings and antifouling coatings for preventing biological attachment, etc. As antifouling coatings, acrylic resin antifouling coatings, vinyl resin antifouling coatings, etc. can be listed. The topcoat coating is preferably epoxy resin coatings, polyurethane resin coatings, fluororesin coatings, acrylic resin antifouling coatings, vinyl resin antifouling coatings, etc. The dry film thickness of the topcoat coating is usually more than 10 μm and less than about 300 μm.

[0092] In addition, the topcoat coating may be the coating composition of the present invention. In the case where the coating composition of the present invention is a topcoat coating, a coating film formed by the coating composition of the present invention is formed on an old coating film formed by the coating composition of the present invention, for example, for repair. The dry film thickness of the topcoat coating film formed by the anticorrosive coating composition of the present invention is usually 10 μm or more and about 300 μm or less.

[0093] The anticorrosion coating film formed from the coating composition of the present invention has excellent anticorrosion properties, can exhibit excellent interlayer adhesion, and further exhibits excellent shrinkage resistance.

[0094] Example

[0095] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited thereto. In addition, parts and % in Examples and Comparative Examples are by mass unless otherwise specified.

[0096] <Resin Production Examples 1 to 14: Production of Acrylic Resins 1 to 14>

[0097] In a four-necked flask equipped with a thermometer, a cooling tube, a stirrer, a dropping funnel, a nitrogen inlet tube and a temperature controller, xylene [A] parts by mass as a solvent was added, and the temperature was maintained at [B]°C. Then, a mixed solution consisting of the monomers shown in Table 2 in the amounts (unit: parts by mass) shown in the table (a total of 100 parts by mass), xylene [C] parts by mass as a solvent, and tert-butyl peroxy-2-ethylhexanoate [D] parts by mass as a radical polymerization initiator was added to the dropping funnel, and the mixture was dropped into the four-necked flask at a constant rate for 3 hours, and the temperature was kept for [E] minutes after the dropwise addition was completed. Then, a mixed solution consisting of xylene [F] parts by mass and 0.3 parts by mass of tert-butyl peroxy-2-ethylhexanoate was dropped into the four-necked flask at a constant rate for 30 minutes, and the temperature was kept for [G] hours after the dropwise addition was completed, thereby obtaining resin compositions (solutions) 1 to 14 containing acrylic resins 1 to 14, respectively.

[0098] Table 1 summarizes the numerical values ​​of [A] to [G] in each of Resin Production Examples 1 to 14.

[0099] [Table 1]

[0100]

[0101] The glass transition temperature Tg, solubility parameter SP, weight average molecular weight Mw of the obtained acrylic resins 1 to 14 and the solid content of the resin compositions 1 to 14 were measured. The results are shown in Table 2. The measurement method is as follows.

[0102] [i] Glass transition temperature Tg

[0103] The glass transition temperature Tg was measured using a differential scanning calorimeter (DSC) in accordance with JIS K 7121. The differential scanning calorimeter (DSC) used was "X-DSC7000" manufactured by SII Nanotechnologies Corporation.

[0104] [ii] Dissolution parameter SP

[0105] Determine using the method already described.

[0106] [iii] Weight average molecular weight Mw

[0107] The weight average molecular weight Mw of the acrylic resin is a weight average molecular weight in terms of polystyrene measured by GPC. The measurement conditions are as follows.

[0108] Device: Tosoh Corporation "HLC-8220GPC"

[0109] Chromatographic column: TSKgel SuperHZM-M×2

[0110] Eluent: Tetrahydrofuran

[0111] Measurement temperature: 35°C

[0112] Detector: RI

[0113] [iv] Solid content

[0114] The solid content was calculated according to the following formula.

[0115] Solid content (mass %) = 100 × (total mass of raw materials used in the preparation of the resin composition excluding the solvent) / (mass of the obtained resin composition)

[0116] [Table 2]

[0117]

[0118] The details of the abbreviations of the monomers shown in Table 2 are as follows.

[0119] (1) n-BA: n-butyl acrylate

[0120] (2)MMA: methyl methacrylate

[0121] (3) ST: Styrene

[0122] (4) EA: Ethyl acrylate

[0123] (5) HEMA: 2-Hydroxyethyl methacrylate

[0124] (6) n-BMA: n-butyl methacrylate

[0125] (7) EHMA: 2-ethylhexyl methacrylate

[0126] (8) CHMA: Cyclohexyl methacrylate

[0127] <Examples 1 to 35, Comparative Examples 1 to 8>

[0128] The first component (main component) and the second component (curing agent) were prepared by mixing the formulation components shown in Tables 3 to 7 to obtain two-component anticorrosive coating compositions. The units of the formulation amounts shown in the tables are tangible parts by mass.

[0129] In the table, "Acrylic resin parts / 100 parts of epoxy resin" refers to the content (mass parts) of acrylic resin relative to 100 parts of epoxy resin. "Mica parts / 100 parts of resin" refers to the content (mass parts) of mica relative to 100 parts of the total content of acrylic resin and epoxy resin. "Curing accelerator parts / 100 parts of epoxy resin" refers to the content (mass parts) of curing accelerator (curing accelerators 1 to 3) relative to 100 parts of epoxy resin.

[0130] The details of the ingredients shown in Tables 3 to 7 are as follows.

[0131] [1] Epoxy resin 1: “jER 828” manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight: 370, SP: 11.5, epoxy equivalent: 184 to 194, non-volatile content: 100% by mass

[0132] [2] Epoxy resin 2: “jER 1001” manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight: 900, SP: 10.8, epoxy equivalent: 450 to 500, non-volatile content: 100% by mass

[0133] [3] Epoxy resin 3: “jER 1003” manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight: 1300, SP: 10.6, epoxy equivalent: 670 to 770, non-volatile content: 100% by mass

[0134] [4] Epoxy resin 4: "Epotohto YD-907" manufactured by Nippon Steel Chemical Materials Co., Ltd., bisphenol A type epoxy resin, weight average molecular weight: 3000, SP: 11.3, epoxy equivalent: 1300-1700, non-volatile content: 100% by mass

[0135] [5] Mica 1: "MICA POWDER W-5" manufactured by Lingshou Huajing Mica Co., Ltd., aspect ratio: 26, non-volatile content: 100% by mass

[0136] [6] Mica 2: "MICA POWDER W-7" manufactured by Lingshou Huajing Mica Co., Ltd., aspect ratio: 14, non-volatile content: 100% by mass

[0137] [7] Mica 3: MinTech Corporation “MT-MICA D325W”, aspect ratio: 18, non-volatile content: 100% by mass

[0138] [8] Mica 4: "Muscovite 200M" manufactured by Kirara Co., Ltd., aspect ratio: 57, non-volatile content: 100% by mass

[0139] [9] Mica 5: "M101" manufactured by Shiraishi Calcium Co., Ltd., aspect ratio: 7, non-volatile content: 100% by mass

[0140]

[10] Pigment 1: "CR50" manufactured by Ishihara Sangyo Co., Ltd., titanium oxide (white pigment), non-volatile content: 100% by mass

[0141]

[11] Pigment 2: "TAROX synthetic iron oxide LL-XLO" manufactured by Titanium Industry Co., Ltd., yellow iron oxide, non-volatile content: 100% by mass

[0142]

[12] Pigment 3: "Talc 34-N" manufactured by Fuji Talc Industries, Ltd., non-volatile content: 100% by mass

[0143]

[13] Pigment 4: "Unispar PG-K10" manufactured by Sibelco Japan Co., Ltd., feldspar, non-volatile content: 100% by mass

[0144]

[14] Pigment 5: "Baryte Powder FBA" manufactured by Fuji Talc Industries, Ltd., barium sulfate, non-volatile content: 100% by mass

[0145]

[15] Additive 1: DYNASYLAN GLYMO manufactured by Evonik Degussa, silane coupling agent, γ-glycidyloxypropyltrimethoxysilane, non-volatile content: 100 mass%

[0146]

[16] Additive 2: "DISPARLON 6700" manufactured by Kusumoto Chemicals Co., Ltd., anti-sagging agent, non-volatile content: 100% by mass

[0147]

[17] Amine curing agent 1: Air Products & Chemicals, Inc., “ANCAMIDE 2050”, polyamide amine curing agent, dimer acid-modified aliphatic polyamide amine (amine component: a mixture of triethylenetetramine and tetraethylenepentamine), amine equivalent: 225 mgKOH / g, non-volatile content: 69 mass %

[0148]

[18] Amine curing agent 2: Air Products & Chemicals, Inc., “SUNMIDE 308D-65T”, polyamide amine curing agent, dimer acid-modified aliphatic polyamide amine (amine component: pentaethylenehexamine), amine equivalent: 180-200 mgKOH / g, non-volatile content: 65% by mass

[0149]

[19] Amine curing agent 3: Shin-Etsu Chemical Co., Ltd. "KBM-603", aminosilane, silane coupling agent with ethylenediamine structure

[0150]

[20] Curing accelerator 1: 2,4,6-tris(dimethylaminomethyl)phenol (TAP), purity: 100% by mass

[0151]

[21] Curing accelerator 2: dimethylaminoethanol (DMAE), purity: 100% by mass

[0152]

[22] Curing accelerator 3: N,N-dimethylaniline (DMA), purity: 100% by mass

[0153]

[23] Solvent 1: Xylene

[0154]

[24] Solvent 2: Methyl isobutyl ketone

[0155] The first agent (main agent) and the second agent (curing agent) of the obtained two-component anticorrosive coating composition were mixed according to the quantitative ratio (parts / parts) recorded in the "first agent / second agent" column in Tables 3 to 7, and stirred thoroughly and homogenized. The following evaluation tests were performed on the obtained mixed coating (anticorrosive coating composition). The results are shown in Tables 3 to 7.

[0156] [1] Topcoat adhesion evaluation test (interval adhesion test)

[0157] [1-1] When the topcoat is an antifouling coating composition

[0158] First, a grid blasted steel plate (7 cm × 15 cm × 3.2 mm) was painted with an inorganic zinc pre-coating primer (trade name "NIPPON CERAMO") manufactured by Nippon Paint Marine Coatings Co., Ltd., and the dried coating thickness was 15 μm, and dried at room temperature for 7 days, thereby preparing a primer-treated steel plate. Next, the above-prepared anticorrosive coating composition was applied to the primer-treated steel plate using an air atomizer, and the dried coating thickness was about 250 μm, thereby obtaining a test coated plate.

[0159] Then, the test plate is exposed to the outdoors, after arranging the interval of 3 days, on the anticorrosion coating film of the test plate, as topcoat coating, (a) hydrolyzable acrylic resin antifouling coating "ECOLOFLEX SPC 200" (made by Nippon Paint Marine Coatings Co., Ltd.) is applied by a sprayer, and its dry film thickness is about 150 μm. Then, the plate coated with topcoat coating is dried indoors for 24 hours. Then, the plate is immersed in actual seawater for 6 months, and immediately after taking out, the cross cutting method based on JIS K 5600-5-6 is carried out with a gap interval of 5mm and a grid number of 9, and the topcoat adhesion is evaluated. The evaluation criteria are as follows. The evaluation result is preferably more than 3.

[0160] 5: The peeling area of ​​the cut part is less than 5%;

[0161] 4: The peeling area of ​​the cut part is greater than 5% and less than 15%;

[0162] 3: The peeling area of ​​the cut part is greater than 15% and less than 35%;

[0163] 2: The peeling area of ​​the cut part is greater than 35% and less than 65%;

[0164] 1: The peeling area of ​​the cut portion is greater than 65% and less than 100%.

[0165] In addition, the same topcoat adhesion evaluation test as above was conducted using the following coatings (b) to (f) different from the above-mentioned (a) as topcoat coatings. The results were the same as those when the above-mentioned antifouling coating (a) was used.

[0166] (b) Hydrolyzable acrylic resin antifouling paint "ECOLOFLEX SPC 150HyB" (manufactured by Nippon Paint Marine Coatings Co., Ltd.)

[0167] (c) Hydrolyzable acrylic resin antifouling paint "ECOLOFLEX SPC 250HyB" (manufactured by Nippon Paint Marine Coatings Co., Ltd.)

[0168] (d) Hydrolyzable acrylic resin antifouling paint "ECOLOFLEX SPC 600HyB" (manufactured by Nippon Paint Marine Coatings Co., Ltd.)

[0169] (e) Hydrolyzable acrylic resin antifouling paint "LF-Sea 150HyB" (manufactured by Nippon Paint Marine Coatings Co., Ltd.)

[0170] (f) Hydrolyzable acrylic resin antifouling paint "LF-Sea 250HyB" (manufactured by Nippon Paint Marine Coatings Co., Ltd.)

[0171] [1-2] When the topcoat is other than an antifouling coating composition

[0172] As topcoat, except using Nippon A-Marine Finish (Japan Paint Marine Coatings Co., Ltd. system) of (g) acrylic resin coating, and, except that the interval to coating topcoat is changed from 3 days to 7 days, the topcoat adhesion evaluation test is carried out in the same manner as above-mentioned [1-1]. At this time, topcoat is applied by a sprayer, and the dry coating thickness is about 125 μm. The evaluation criteria are the same as above-mentioned [1-1]. The evaluation result is preferably more than 3.

[0173] In addition, as topcoat coating, the following coating (h)~(m) different from the above (g) is used, and, except that the dry coating thickness of the topcoat coating is as described below, the same topcoat adhesion evaluation test as above is carried out. The result is the same as when using the above-mentioned topcoat (g).

[0174] (h) Epoxy resin paint "NIPPON EPOXY FINISH M" (manufactured by Nippon Paint Marine Coatings Co., Ltd.), dry film thickness: 100 μm

[0175] (i) Alkyd resin paint "CR MARINE FINISH" (manufactured by Nippon Paint Marine Coatings Co., Ltd.), dry coating thickness: 35 μm

[0176] (j) Acrylic resin paint "NIPPON A-MARINE FINISH" (manufactured by Nippon Paint Marine Coatings Co., Ltd.), dry coating thickness: 50 μm

[0177] (k) Polyurethane resin coating "POLYURE MIGHTYLAC M" (manufactured by Nippon Paint Marine Coatings Co., Ltd.), dry coating thickness: 30 μm × 2 (meaning that after forming a 30 μm thick dry coating film, a 30 μm thick dry coating film is further formed thereon.)

[0178] (l) Epoxy resin paint "NOA A / C II" (manufactured by Nippon Paint Marine Coatings Co., Ltd.), dry film thickness: 75 μm

[0179] (m) Epoxy resin paint "NIPPON E-MARINE A / C II" (manufactured by Nippon Paint Marine Coatings Co., Ltd.), dry film thickness: 75 μm

[0180] [2] Shrinkage resistance evaluation test

[0181] First, (j) acrylic resin coating "NIPPON A-MARINE FINISH" (manufactured by Nippon Paint Marine Coatings Co., Ltd.) was applied to a tin plate "29.7 cm × 42 cm × 0.3 mm" in a manner of a dry coating thickness of about 50 μm, and dried at room temperature for 1 day. Next, the above-prepared anticorrosive coating composition was applied using an air atomizer to a dry coating thickness of about 100 μm, and dried for 3 days in an atmosphere of 20°C × 65% RH, thereby forming an anticorrosive coating film.

[0182] Next, on the anticorrosion coating film, an applicator (20MIL) was used to apply (j) an acrylic resin coating "NIPPON A-MARINE FINISH" (manufactured by Nippon Paint Marine Coatings Co., Ltd.), and it was dried indoors for 24 hours to prepare a test coating plate consisting of three layers of acrylic resin coating film (equivalent to topcoat coating film) / anticorrosion coating film (primer coating film) / acrylic resin coating film (equivalent to topcoat coating film), and the occurrence of shrinkage was visually confirmed. The evaluation criteria are as follows. The evaluation result is preferably 3 or more.

[0183] 5: No shrinkage occurs;

[0184] 4: Only a small shrinkage occurs at the edges;

[0185] 3: The area of ​​small shrinkage is less than 20%;

[0186] 2: The area of ​​small shrinkage exceeds 20% and is less than 100%;

[0187] 1: Small contractions aggregate to produce larger contractions.

[0188] In the above, small shrinkage refers to shrinkage that cannot be visually recognized at a distance of 5 m from the test coating plate, and large shrinkage refers to shrinkage that can be visually recognized at a distance of 5 m from the test coating plate.

[0189] In addition, the same shrinkage resistance evaluation test as above was conducted using the above coating materials (h) and (k) different from the above "NIPPON A-MARINE FINISH". The results were the same as in the case of using the above coating material (j) "NIPPON A-MARINE FINISH".

[0190] [Table 3]

[0191]

[0192] [Table 4]

[0193]

[0194] [Table 5]

[0195]

[0196] [Table 6]

[0197]

[0198] [Table 7]

[0199]

Claims

1. A primer coating composition comprising an acrylic resin, an epoxy resin and an amine curing agent, The acrylic resin has a solubility parameter of 9.0 or more and 12 or less, and a weight average molecular weight of 1000 or more and 95000 or less; The epoxy resin has a solubility parameter of 10 to 12, and a weight average molecular weight of 250 to 2500; The content of the acrylic resin is 4 parts by mass or more and 60 parts by mass or less relative to 100 parts by mass of the epoxy resin. 2 . The primer coating composition according to claim 1 , further comprising a curing accelerator, wherein the content of the curing accelerator is 0.1 parts by mass or more and 16 parts by mass or less relative to 100 parts by mass of the epoxy resin. 3 . The primer coating composition according to claim 1 , which is a two-component primer coating composition comprising a first component and a second component, wherein the first component contains the acrylic resin and the epoxy resin, and the second component contains the amine curing agent. 4 . The primer coating composition according to claim 1 , further comprising mica, wherein the content of the mica is 2 parts by mass or more and 95 parts by mass or less relative to 100 parts by mass of the total content of the acrylic resin and the epoxy resin.

5. A coating film formed from the primer coating composition according to any one of claims 1 to 4.

6. A method for forming a coating film, comprising: A step of forming a primer coating film on a substrate using the primer coating composition according to any one of claims 1 to 4.

7. A method for forming a multilayer coating, comprising: A step of forming a primer coating film on a substrate using the primer coating composition according to any one of claims 1 to 4; and, A step of forming a topcoat coating film on the primer coating film using a topcoat coating composition. 8 . An article having a primer coating film formed from the primer coating composition according to claim 1 .

9. The article according to claim 8, further comprising a topcoat film on the primer film.

Citation Information

Patent Citations

  • Epoxy resin coating composition, method for forming coating film, and coated article

    JP2009197106A

  • Cured electrodeposition coating film and process for forming multi layered coating film

    CN102344708A

  • Cationic electrodeposition paint composition capable even of coating sections having narrow clearance, and electrodeposition paint-film formation method using same

    CN103635547A

  • Powder paint, coated article, and production method for coated article

    CN107429103A

  • Cationic electrodeposition coating composition

    CN114040947A