A high-nitrogen vanadium microalloyed steel and its preparation method

By designing the chemical composition and optimizing the process of high-nitrogen vanadium microalloyed steel, the problems of difficulty in increasing nitrogen content and slab crack sensitivity in high-vanadium nitrogen steel were solved, achieving high yield and stable continuous casting production, and improving slab quality.

CN117737599BActive Publication Date: 2026-11-10ZHONG NAT ENG & RES CENT
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311704347.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-12
Publication Date
2026-11-10
Estimated Expiration
2043-12-12

AI Technical Summary

Technical Problem

In the production of high vanadium nitrogen steel, the nitrogen content is difficult to increase to above 0.01%, the yield of alloying elements in the smelting process is unstable, the billet is highly sensitive to cracking during continuous casting, which affects production stability and billet quality, and may even lead to safety accidents.

Method used

The chemical composition of the high-nitrogen vanadium microalloyed steel is designed, including 0.05%≤V≤0.1%, 0.012%≤N≤0.018%, and 0.01%≤Al≤0.015%. Through converter smelting, LF refining and continuous casting processes, silicon-manganese weak deoxidizer is used, the cooling water volume of the crystallizer and the secondary cooling water mode are controlled, the addition of alloying elements and inclusion control are optimized, and the precipitation strengthening effect of nitrogen and vanadium is ensured.

Benefits of technology

It improves the recovery rate of alloying elements in the smelting process and the stability of continuous casting production, significantly reduces the number and degree of corner cracks in the billet, improves the quality of the billet, and reduces the surface grinding rate of the billet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117737599B_ABST
    Figure CN117737599B_ABST
Patent Text Reader

Abstract

This invention discloses a high-nitrogen vanadium microalloyed steel and its preparation method, belonging to the field of metallurgical technology. The chemical composition of the high-nitrogen vanadium microalloyed steel provided by this invention includes the following mass fractions: 0.05% ≤ V ≤ 0.1%, 0.012% ≤ N ≤ 0.018%, and 0.01% ≤ Al ≤ 0.015%. The high-nitrogen vanadium microalloyed steel and its preparation method provided by this invention have a nitrogen content as high as 0.018%, which, while ensuring effective bonding with the v element to achieve precipitation strengthening, also significantly reduces the number and severity of corner cracks in the cast billet, thus improving the quality of the cast billet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metallurgical technology, and more specifically, to a high-nitrogen vanadium microalloyed steel and its preparation method. Background Technology

[0002] In the steel industry, vanadium (V) is an important microalloying element to improve steel performance. Steels with varying carbon contents can have their strength, toughness, and plasticity enhanced by adding V, thereby improving their processing properties. For V-containing steel, nitrogen (N) is a crucial alloying element. N optimizes V precipitation in steel, significantly improving its precipitation strengthening effect. Studies show that for every 0.001% increase in N by mass fraction, the strength of V-containing steel can increase by more than 6 MPa. Simultaneously, increasing N significantly reduces V consumption and production costs. However, when the N content in steel is high, it easily reacts with other elements such as Al and Ti to form precipitates such as AlN and TiN. If AlN and TiN precipitate at grain boundaries, microcracks will form when the ultimate stress is reached. Under subsequent thermal stress, straightening stress, and other stresses, these cracks will further propagate and form larger cracks.

[0003] The production of high-vanadium-nitrogen steel faces several challenges: Firstly, increasing the nitrogen content in the steel is difficult due to the low solubility of nitrogen in steel, making it challenging to raise the nitrogen content above 0.01% through nitrogen blowing. Furthermore, unstable recovery rates of alloying elements and inclusion control during the smelting process also constrain the stability of continuous casting production and the quality of the cast billet. Secondly, high-vanadium-nitrogen microalloyed steel billets are highly susceptible to cracking during continuous casting. Surface cracks in the billet severely impact the stability of continuous casting production and the performance of the steel grade. At best, the billet needs to be re-ground to remove cracks; at worst, it can lead to the billet being scrapped and unable to be further processed, potentially causing safety accidents such as leaks. This not only affects production but also increases costs, wastes resources, and hinders the improvement of steel plate quality and the company's economic benefits.

[0004] In view of this, the present invention is proposed. Summary of the Invention

[0005] The purpose of this invention is to overcome the defects of the prior art and provide a high-nitrogen vanadium microalloyed steel and its preparation method.

[0006] The technical problem solved by this invention is achieved by the following technical solution.

[0007] This invention provides a high-nitrogen vanadium microalloyed steel, wherein the chemical composition of the high-nitrogen vanadium microalloyed steel comprises the following mass fractions: 0.05% ≤ V ≤ 0.1%, 0.012% ≤ N ≤ 0.018%, and 0.01% ≤ Al ≤ 0.015%.

[0008] The present invention also provides a method for preparing the above-mentioned high-nitrogen vanadium microalloyed steel, the method comprising: a converter smelting process, an LF refining process, and a continuous casting process.

[0009] The present invention has the following beneficial effects:

[0010] This invention provides a high-nitrogen vanadium microalloyed steel and its preparation method. The chemical composition of the high-nitrogen vanadium microalloyed steel provided by this invention includes the following mass fractions: 0.05% ≤ V ≤ 0.1%, 0.012% ≤ N ≤ 0.018%, and 0.01% ≤ Al ≤ 0.015%. The high-nitrogen vanadium microalloyed steel provided by this invention has a nitrogen content as high as 0.018%. While ensuring that it can effectively combine with the v element to play a precipitation strengthening role, it not only improves the compositional fluctuation of alloying elements in the smelting process and the stability of continuous casting production, but also significantly reduces the number and degree of corner cracks in the billet, improves the billet quality, and reduces the surface grinding rate of the billet. Attached Figure Description

[0011] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0012] Figure 1 Photographs of corner cracks in cast billets produced using the process of Comparative Example 1;

[0013] Figure 2 Photographs of corner cracks in cast billets produced using the process of Example 1;

[0014] Figure 3 Photographs of corner cracks in cast billets produced using the process of Example 2;

[0015] Figure 4 Photographs of corner cracks in cast billets produced using the process of Example 3;

[0016] Figure 5 Photographs of corner cracks in cast billets produced using the process of Example 4. Detailed Implementation

[0017] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below.

[0018] This invention provides a high-nitrogen vanadium microalloyed steel, and adopts a reasonable smelting and continuous casting process for this steel, implements effective alloying methods and inclusion control measures, effectively reduces the number, depth and length of corner cracks in the billet, and improves the quality of the billet and the final rolled product.

[0019] The following is a detailed description of a high-nitrogen vanadium microalloyed steel and its preparation method provided by an embodiment of the present invention.

[0020] In a first aspect, embodiments of the present invention provide a high-nitrogen vanadium microalloyed steel, wherein the chemical composition of the high-nitrogen vanadium microalloyed steel, by mass percentage, includes: 0.05% ≤ V ≤ 0.1%, 0.012% ≤ N ≤ 0.018%, and 0.01% ≤ Al ≤ 0.015%.

[0021] Furthermore, the chemical composition of the high-nitrogen vanadium microalloyed steel, by mass percentage, further includes: C≤0.14%, 0.2≤Si≤0.8%, Mn≤1.4%, 0.6≤Ni≤1.5%, 0.4≤Cr≤1.0%, P≤0.015%, S≤0.01%, and Ti≤0.005%.

[0022] Secondly, embodiments of the present invention provide a method for preparing the above-mentioned high-nitrogen vanadium microalloyed steel, comprising the following steps:

[0023] (1) Converter smelting: Comparative Example 1 uses aluminum deoxidation, while the Example does not use aluminum deoxidation but uses silicon-manganese deoxidation alloying. During the converter smelting process, ferrosilicon, low-carbon ferrochrome, ferromolybdenum, ferrovanadium and metallic manganese are added according to the composition requirements. Vanadium-nitrogen alloy is added when the steel is tapped from the converter.

[0024] (2) LF refining: After the ladle enters the station, lime particles and fluorite are added according to the composition of the converter steel to carry out slag making. At the same time, ferrosilicon, ferrovanadium, silicon manganese nitride and other elements are added according to the alloy element content of the steel to finely adjust the content of silicon, vanadium and nitrogen.

[0025] (3) Continuous casting production: When casting begins, the molten steel in the tundish is injected into multiple crystallizers. The electromagnetic stirring parameters are optimized and the secondary cooling water intensity is combined to control the process. High nitrogen vanadium microalloyed steel billets are produced by a large billet continuous casting machine.

[0026] Furthermore, in step (1), the amount of ferrosilicon added is 6-8 kg / t steel, the amount of low-carbon ferrochrome added is 8-10 kg / t steel, the amount of ferromolybdenum added is 0.03-0.05 kg / t steel, the amount of ferrovanadium added is 0.35-0.5 kg / t steel, and the amount of sintered manganese balls added is 8-10 kg / t steel. Since the nitrogen content of this steel is relatively high, the amount of vanadium-nitrogen alloy added during the converter tapping process is increased to 0.5-1 kg / t steel.

[0027] Furthermore, step (1) also includes controlling the carbon content of the final molten steel in the converter to be below 0.12%, the oxygen content to be below 0.1%, and the tapping temperature to be 1620-1650℃.

[0028] Further, in step (2), the amount of lime particles added is 3-9 kg / t steel, the amount of fluorite added is 1-3 kg / t steel, and at the same time, according to the sample composition measured by sampling, one or more of the following are added: ferrovanadium 0-0.02 kg / t steel, silicon manganese nitride 0-0.07 kg / t steel, ferrosilicon 1.2-3 kg / t steel, low carbon ferrochrome 1.5-3 kg / t steel, and medium carbon ferromanganese 1-2.5 kg / t steel. Before tapping the steel, silicon calcium cored wire is added to the top slag for Ca treatment, and the amount added is 0.6-1.3 m / t steel.

[0029] Furthermore, in step (3), the ladle changing time during the casting process is controlled within 110s, the superheat of the molten steel is controlled at 25-45℃, the casting speed is controlled at 0.50-0.75m / min, and protective slag is added throughout the casting process.

[0030] Furthermore, in step (3), the flow rate of the cooling water in the crystallizer is controlled at 3000-3500 L / min, while the temperature of the inlet water in the crystallizer is not lower than 30℃, and the temperature difference between the inlet and outlet water is controlled at 5-8℃. Under the working speed, the vibration frequency of the crystallizer is controlled at 125-130 cpm, and the amplitude of the crystallizer is maintained at 2.5 mm.

[0031] Furthermore, in step (3), the secondary cooling water adopts a weak cooling mode, and the specific water volume is controlled within the range of 0.12 to 0.13 L / kg. For the three cooling zones of the secondary cooling zone, the cooling water proportion of the foot roller section is 48 to 52%, the water volume proportion of the first section of the moving fan is 29 to 31%, and the water volume proportion of the second section of the moving fan is 18 to 22%.

[0032] Furthermore, in step (3), the mold flux is a special mold flux for continuous casting of low carbon steel in billets, and the thickness of the liquid slag layer needs to be controlled at 5-12 mm. The composition of the mold flux is controlled as follows: 30%≤SiO2≤35%, 4%≤Al2O3≤11%, 25%≤CaO≤35%, 1%≤MgO≤5%, 8%≤Na2O≤15%, 4%≤F≤8%, and the physical properties are: basicity controlled at 0.9-1.1, melting point controlled at 1080-1180℃, and viscosity controlled at 0.2-1 Pa·s.

[0033] The above embodiments of the present invention provide a method for preparing high-quality, high-nitrogen, vanadium-based microalloyed steel, wherein: in the steelmaking process, a silicon-manganese weak deoxidizer is used for deoxidation instead of aluminum deoxidation, and vanadium and nitrogen elements are added in the form of vanadium-nitrogen alloy during the converter tapping process; in the refining process, silicon-manganese nitride and ferrovanadium alloy are added to ensure the required nitrogen and vanadium content of the steel grade; in the continuous casting process, the cooling water flow rate of the crystallizer needs to be controlled at 3000-3500 L / min, and the secondary cooling water adopts a weak cooling mode, controlling the specific water volume at 0.12-0.13 L / Kg. Production according to the above parameters results in a nitrogen content as high as 0.018%, which, while ensuring effective combination with vanadium for precipitation strengthening, also significantly reduces the number and severity of corner cracks in the billet, thus improving the billet quality.

[0034] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0035] This invention provides a high-quality nitrogen-vanadium microalloyed steel. The chemical composition of the high-nitrogen-vanadium microalloyed steel, by mass percentage, includes: 0.05% ≤ V ≤ 0.1%, 0.012% ≤ N ≤ 0.018%, and 0.01% ≤ Al ≤ 0.015%. Analysis of the steel composition shows that nitrogen content in the range of 0.012% to 0.018% can effectively precipitate and strengthen vanadium, thereby improving steel performance. However, the solubility of nitrogen in steel is relatively limited, making it difficult to increase the nitrogen content in molten steel through methods such as direct nitrogen blowing. This preparation method adds a vanadium-nitrogen alloy during the tapping process to achieve initial alloying of nitrogen and vanadium, meeting the steel composition requirements while simultaneously improving alloy yield. During refining, the alloying elements are fine-tuned to meet the steel composition requirements. Adding silicon manganese nitride and ferrovanadium alloys can ensure that the nitrogen content in the molten steel reaches the range of 0.012% to 0.018%, and the vanadium content reaches 0.05% to 0.10%.

[0036] This invention also provides a method for preparing the above-mentioned high-quality nitrogen-vanadium microalloyed steel. In the steelmaking refining process, deoxidation, alloying processes, and inclusion control are closely related. Inclusions in the molten steel during casting have a significant impact on the performance of the protective slag, casting stability, and the control of surface cracks in the billet. Therefore, optimizing and controlling the refining process is of great significance and importance for the preparation of high-nitrogen-vanadium microalloyed steel. During the converter tapping process, deoxidizers need to be added to remove oxygen from the molten steel to stabilize the yield of subsequent alloys. If a strong deoxidizer, aluminum, is used for deoxidation, the high nitrogen content of this steel grade will react with aluminum to form aluminum nitride inclusions, which will significantly affect the quality defects of the continuously cast billet and the performance of the steel. Therefore, for this type of high-nitrogen-vanadium microalloyed steel, a weak silicon-manganese deoxidizer is mainly considered for deoxidation.

[0037] During continuous casting, considering that the steel grade is peritectic steel, the shrinkage volume ratio of the billet is relatively large when it initially solidifies in the crystallizer. If the cooling is uneven, it is easy to cause surface depressions or cracks. Therefore, this invention considers controlling the cooling water volume of the crystallizer at 3000-3500 L / min.

[0038] The composition and physical properties of the mold flux used in the following examples and comparative examples are as follows:

[0039] The mold flux used is a special mold flux for continuous casting of low-carbon steel in billets, and the thickness of the liquid slag layer needs to be controlled between 5 and 12 mm. The composition of the mold flux is controlled as follows: 30% ≤ SiO2 ≤ 40%, 6% ≤ Al2O3 ≤ 11%, 25% ≤ CaO ≤ 40%, 1% ≤ MgO ≤ 5%, 2% ≤ Na2O ≤ 10%, 3% ≤ F ≤ 5%. The physical properties are: basicity controlled between 0.9 and 1.1, melting point controlled between 1100 and 1180℃, and viscosity controlled between 0.4 and 1 Pa·s. The composition of the mold flux in Examples 1-4 is shown in Table 1, and the composition of the mold flux in Comparative Example 1 is shown in Table 2.

[0040] Table 1. Composition and physical properties of the protective slag used in Examples 1-4

[0041]

[0042] Table 2 shows the composition and physical properties of the protective slag used in Comparative Example 1.

[0043]

[0044] Example 1

[0045] A high-quality high-nitrogen vanadium microalloyed steel, the chemical composition of which, by mass percentage, includes: C 0.09%, Si 0.5%, Mn 1.03%, Ni 1.12%, Cr 0.6%, P 0.009%, S 0.0028%, V 0.08%, N 0.0156%, Ti 0.001%, and Al 0.011%.

[0046] The production method includes the following steps:

[0047] 1) Converter smelting

[0048] During converter production, 750 kg of ferrosilicon, 900 kg of low-carbon ferrochrome, 40 kg of ferromolybdenum, 45 kg of ferrovanadium, and 940 kg of sintered manganese balls are added. Deoxidation is performed using ferrosilicon-manganese alloy. 70 kg of vanadium-nitrogen alloy is added at the converter tapping stage. The final tapping temperature is 1627℃, with carbon and oxygen contents of 0.043% and 0.089%, respectively.

[0049] 2) LF Refining

[0050] Slag-making operations were carried out based on the composition and temperature of the molten steel delivered from the converter. 845 kg of lime and 256 kg of fluorite were added. At the same time, based on the sample composition measured by sampling, 5 kg of ferrovanadium, 50 kg of silicon manganese nitride, 233 kg of ferrosilicon, 233 kg of low-carbon ferrochrome, and 216 kg / t of medium-carbon ferromanganese were added. Before leaving the station, 64 m of silicon-calcium cored wire was added to the top slag for Ca treatment.

[0051] 3) Continuous casting production

[0052] The production process uses large square billets with a cross-section of 320×410mm. Superheat is controlled between 26 and 41℃, casting speed is 0.55m / min, and the cooling water flow rate to the crystallizer is controlled at 3300L / min. Crystallizer vibration parameters are shown in Table 3. The secondary cooling water flow rate adopts a weak cooling mode, controlled between 0.12 and 0.13L / Kg. For the three cooling zones, the cooling water volume accounts for 48.5% in the foot roll section, 30% in the moving fan-shaped section A, and 21.5% in the moving fan-shaped section B. The crystallizer electromagnetic stirring maintains a constant current of 700A and frequency of 2Hz, while the end electromagnetic stirring is controlled at 320A and frequency of 5Hz. The mold flux used is a special mold flux for continuous casting of low-carbon steel in square billets. The composition and physical properties of the mold flux are shown in Table 1.

[0053] Table 3. Crystallizer Vibration Parameters

[0054] Pulling speed Vc (m / min) Travel distance s (mm) Frequency f (cpm) Negative slip time tn(s) Positive slip time tp(s) Vibration period tc(s) 0.55 5 128 0.193 0.2757 0.47 V on max ΔV maximum velocity difference NS negative slip rate Negative sliding time rate Xn negative slip lead Vibration mark spacing 2.01 2.56 -1.33 0.41 3.04 4.3

[0055] During continuous casting, the liquid level in the crystallizer remained stable, and no safety accidents occurred. The temperature of the billet corners in the straightening section was measured during production. The results showed that the corner temperature was higher than that of Comparative Example 1 at the same casting speed, effectively avoiding the brittle range where the steel grade would crack. The corners of the cooled billets were then ground to inspect their quality; the results are shown below. Figure 2 As shown in the figure. The results indicate that the corner quality of the large square billet high-nitrogen vanadium microalloyed steel with a cross-section of 320×410mm produced by this method is better, and the number, length, and depth of corner cracks are significantly improved.

[0056] Example 2

[0057] A high-quality high-nitrogen vanadium microalloyed steel, the chemical composition of which, by mass percentage, includes: C 0.08%, Si 0.51%, Mn 1.04%, Ni 1.14%, Cr 0.61%, P 0.008%, S 0.0027%, V 0.08%, N 0.0126%, Ti 0.001%, and Al 0.01%.

[0058] The production method includes the following steps:

[0059] 1) Converter production

[0060] During converter production, 720 kg of ferrosilicon, 880 kg of low-carbon ferrochrome, 40 kg of ferromolybdenum, 40 kg of ferrovanadium, and 900 kg of sintered manganese balls were added. Deoxidation was performed using ferrosilicon-manganese alloy. At the tapping stage, 70 kg of vanadium-nitrogen alloy was added to increase nitrogen and oxygen content. The final tapping temperature was 1642℃, with carbon and oxygen contents of 0.119% and 0.061%, respectively.

[0061] 2) LF Refining

[0062] Slag-making operations were carried out based on the composition and temperature of the molten steel delivered from the converter. 643 kg of lime and 129 kg of fluorite were added. At the same time, based on the sample composition measured by sampling, 5 kg of ferrovanadium, 250 kg of ferrosilicon, 233 kg of low-carbon ferrochrome, and 188 kg / t of medium-carbon ferromanganese were added. Before leaving the station, 64 m of silicon-calcium cored wire was added to the top slag for Ca treatment.

[0063] 3) Continuous casting production

[0064] The production process uses large square billets with a cross-section of 320×410mm. Superheat is controlled between 26 and 41℃, casting speed is 0.60 m / min, and the cooling water flow rate of the crystallizer is controlled at 3300 L / min. Crystallizer vibration parameters are shown in Table 4. The secondary cooling water flow rate adopts a weak cooling mode, controlled between 0.12 and 0.13 L / kg. For the three cooling zones, the cooling water volume accounts for 51.3% of the flow rate in the foot roller section, 30.2% in the moving fan-shaped section A, and 18.5% in the moving fan-shaped section B. The electromagnetic stirring of the crystallizer maintains a constant current of 700A and a frequency of 2Hz, while the end electromagnetic stirring is controlled at 300A and a frequency of 5Hz. The mold flux used is a special mold flux for continuous casting of low-carbon steel in square billets. The composition and physical properties of the mold flux are shown in Table 1.

[0065] Table 4. Crystallizer Vibration Parameters

[0066] Pulling speed Vc (m / min) Travel distance s (mm) Frequency f (cpm) Negative slip time tn(s) Positive slip time tp(s) Vibration period tc(s) 0.60 5 130 0.187 0.2746 0.46 V on max ΔV maximum velocity difference NS negative slip rate Negative sliding time rate Xn negative slip lead Vibration mark spacing 2.04 2.64 -1.17 0.41 2.91 4.6

[0067] During continuous casting, the liquid level in the crystallizer remained stable, and no safety accidents occurred. The corners of the cooled billet were ground to inspect their quality; the results are shown below. Figure 3 As shown in the figure. The results indicate that the corner quality of the large square billet high-nitrogen vanadium microalloyed steel with a cross-section of 320×410mm produced by this method is better, and the number, length, and depth of corner cracks are significantly improved.

[0068] Example 3

[0069] A high-quality high-nitrogen vanadium microalloyed steel, the chemical composition of which, by mass percentage, includes: C 0.08%, Si 0.47%, Mn 1.04%, Ni 1.16%, Cr 0.64%, P 0.007%, S 0.002%, V 0.09%, N 0.013%, Ti 0.002%, and Al 0.012%.

[0070] The production method includes the following steps:

[0071] 1) Converter smelting

[0072] During converter production, 660 kg of ferrosilicon, 850 kg of low-carbon ferrochrome, 35 kg of ferromolybdenum, 45 kg of ferrovanadium, and 880 kg of sintered manganese balls are added. Deoxidation is performed using ferrosilicon-manganese alloy. 80 kg of vanadium-nitrogen alloy is added at the converter tapping stage. The final tapping temperature is 1636℃, with carbon and oxygen contents of 0.043% and 0.061%, respectively.

[0073] 2) LF Refining

[0074] Slag-making operations were carried out based on the composition and temperature of the molten steel delivered from the converter. 342 kg of lime and 106 kg of fluorite were added. At the same time, based on the sample composition measured by sampling, 16 kg of ferrovanadium, 10 kg of silicon manganese nitride, 108 kg of ferrosilicon, 172 kg of low-carbon ferrochrome, and 224 kg / t of medium-carbon ferromanganese were added. Before leaving the station, 126 m of silicon-calcium cored wire was added to the top slag for Ca treatment.

[0075] 3) Continuous casting production

[0076] The production process uses large square billets with a cross-section of 320×410mm. Superheat is controlled between 26 and 41℃, casting speed is 0.55 m / min, and the cooling water flow rate to the crystallizer is controlled at 3300 L / min. Crystallizer vibration parameters are shown in Table 5. The secondary cooling water flow rate adopts a weak cooling mode, controlled between 0.12 and 0.13 L / kg. For the three cooling zones, the cooling water volume accounts for 50.5% in the foot roller section, 29% in the moving fan-shaped section A, and 20.5% in the moving fan-shaped section B. The crystallizer electromagnetic stirring maintains a constant current of 700A and frequency of 2Hz, while the end electromagnetic stirring is controlled at 320A and frequency of 5Hz. The mold flux used is a special mold flux for continuous casting of low-carbon steel in square billets. The composition and physical properties of the mold flux are shown in Table 1.

[0077] Table 5. Crystallizer Vibration Parameters

[0078] Pulling speed Vc (m / min) Travel distance s (mm) Frequency f (cpm) Negative slip time tn(s) Positive slip time tp(s) Vibration period tc(s) 0.55 5 128 0.193 0.2757 0.47 V on max ΔV maximum velocity difference NS negative slip rate Negative sliding time rate Xn negative slip lead Vibration mark spacing 2.01 2.56 -1.33 0.41 3.04 4.3

[0079] During continuous casting, the liquid level in the crystallizer remained stable, and no safety accidents occurred. The temperature of the corner of the billet in the straightening section was measured during production. The results showed that the corner temperature was higher than that in Comparative Example 1 at the same casting speed, effectively avoiding the brittle range where the steel grade would crack. The corners of the cooled billets were then ground to inspect their quality; the results are shown below. Figure 4 As shown in the figure. The results indicate that the corner quality of the large square billet high-nitrogen vanadium microalloyed steel with a cross-section of 320×410mm produced by this method is better, and the number, length, and depth of corner cracks are significantly improved.

[0080] Example 4

[0081] A high-quality high-nitrogen vanadium microalloyed steel, the chemical composition of which, by mass percentage, includes: C 0.09%, Si 0.53%, Mn 1.06%, Ni 1.15%, Cr 0.61%, P 0.007%, S 0.0031%, V 0.09%, N 0.0126%, Ti 0.002%, and Al 0.010%.

[0082] The production method includes the following steps:

[0083] 1) Converter smelting

[0084] During converter production, 700 kg of ferrosilicon, 900 kg of low-carbon ferrochrome, 40 kg of ferromolybdenum, 35 kg of ferrovanadium, and 950 kg of sintered manganese balls are added. Deoxidation is performed using ferrosilicon-manganese alloy. 80 kg of vanadium-nitrogen alloy is added at the converter tapping stage. The final tapping temperature is 1632℃, with carbon and oxygen contents of 0.054% and 0.074%, respectively.

[0085] 2) LF Refining

[0086] Slag-making operations were carried out based on the composition and temperature of the molten steel delivered from the converter. 464 kg of lime and 121 kg of fluorite were added. At the same time, based on the sample composition measured by sampling, 165 kg of ferrosilicon, 184 kg of low-carbon ferrochrome, and 198 kg / t of medium-carbon ferromanganese were added. Before leaving the station, 126 m of silicon-calcium cored wire was added to the top slag for Ca treatment.

[0087] 3) Continuous casting production

[0088] The production process uses large square billets with a cross-section of 320×410mm. Superheat is controlled between 26 and 41℃, casting speed is 0.60 m / min, and the cooling water flow rate of the crystallizer is controlled at 3300 L / min. Crystallizer vibration parameters are shown in Table 6. The secondary cooling water ratio is controlled in a weak cooling mode, between 0.12 and 0.13 L / kg. For the three cooling zones, the cooling water volume accounts for 49.5% in the foot roller section, 28.5% in the moving fan-shaped section A, and 22% in the moving fan-shaped section B. The crystallizer electromagnetic stirring maintains a constant current of 700A and frequency of 2Hz, while the end electromagnetic stirring is controlled at 320A and frequency of 5Hz. The mold flux used is a special mold flux for continuous casting of low-carbon steel in square billets. The composition and physical properties of the mold flux are shown in Table 1.

[0089] Table 6. Crystallizer Vibration Parameters

[0090] Pulling speed Vc (m / min) Travel distance s (mm) Frequency f (cpm) Negative slip time tn(s) Positive slip time tp(s) Vibration period tc(s) 0.60 5 130 0.187 0.2746 0.46 V on max ΔV maximum velocity difference NS negative slip rate Negative sliding time rate Xn negative slip lead Vibration mark spacing 2.04 2.64 -1.17 0.41 2.91 4.6

[0091] During continuous casting, the liquid level in the crystallizer remained stable, and no safety accidents occurred. The temperature of the billet corners in the straightening section was measured during production. The results showed that the corner temperature was higher than that of Comparative Example 1 at the same casting speed, effectively avoiding the brittle range where the steel grade would crack. The corners of the cooled billets were then ground to inspect their quality; the results are shown below. Figure 5 As shown in the figure. The results show that the corner quality of the 320×410mm high-nitrogen vanadium microalloyed steel billet produced using this patent is better, and the number, length, and depth of corner cracks are significantly improved.

[0092] Comparative Example 1

[0093] This comparative example is similar to the method in Example 1, except that: the converter smelting process uses aluminum deoxidation, the crystallizer cooling water flow rate is 3700 L / min, and the composition and physical properties of the protective slag are shown in Table 2. Figure 1 It can be seen that the cracks in the steel produced in Comparative Example 1 are very obvious.

[0094] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing high-nitrogen vanadium microalloyed steel, characterized in that, The preparation method includes: a converter smelting process, an LF refining process, and a continuous casting process, wherein: The converter smelting process includes: using silicon-manganese deoxidation alloying; during the converter smelting process, adding ferrosilicon, low-carbon ferrochrome, ferromolybdenum, ferrovanadium and sintered manganese balls according to the composition requirements; and adding vanadium-nitrogen alloy when tapping steel from the converter. The addition amount of ferrosilicon is 6~8 kg / t steel, the addition amount of low carbon ferrochrome is 8~10 kg / t steel, the addition amount of ferromolybdenum is 0.03~0.05 kg / t steel, the addition amount of ferrovanadium is 0.35~0.5 kg / t steel, the addition amount of sintered manganese balls is 8~10 kg / t steel, and the addition amount of vanadium-nitrogen alloy is 0.5~1 kg / t steel. The carbon content of the final molten steel in the converter is controlled below 0.12%, the oxygen content is controlled below 0.1%, and the tapping temperature is 1620-1650℃; The LF refining process includes: adding lime particles and fluorite to form slag according to the composition of the converter steel; and adding one or more of ferrosilicon, ferrovanadium, silicon manganese nitride, and low-carbon ferrochrome to finely adjust the content of silicon, vanadium, and nitrogen elements according to the alloy element content of the steel. The amount of lime particles added is 3~9 kg / t steel, the amount of fluorite added is 1~3 kg / t steel, and at the same time, according to the sample composition measured by sampling, one or more of the following are added: ferrovanadium 0~0.02 kg / t steel, silicon manganese nitride 0~0.07 kg / t steel, ferrosilicon 1.2~3 kg / t steel, and low carbon ferrochrome 1.5~3 kg / t steel. Before tapping, silicon-calcium cored wire is added to the top slag for Ca treatment, and the amount added is 0.6~1.3 m / t steel. The continuous casting process includes: at the start of casting, molten steel in the tundish is injected into multiple crystallizers, and cooling is carried out by combining the control of electromagnetic stirring parameters with the flow rate of secondary cooling water. High nitrogen vanadium microalloyed steel billets are produced by a large billet continuous casting machine. It also includes: controlling the ladle changing time within 110 seconds during the casting process, controlling the superheat of molten steel to 25~45℃, controlling the casting speed to 0.50~0.75m / min, and the billet cross-section to be 320×410mm; The flow rate of cooling water for the crystallizer is controlled at 3000~3500L / min, while the inlet water temperature of the crystallizer is not lower than 30℃, and the temperature difference between the inlet and outlet water is controlled at 5~8℃. At the operating speed, the crystallizer vibration frequency is controlled at 125~130 cpm, and the crystallizer amplitude is maintained at 2.5 mm. Protective slag is added throughout the casting process; The protective slag is designed as follows: its chemical composition, by mass percentage, includes: 30%≤SiO2≤40%, 6%≤Al2O3≤11%, 25%≤CaO≤40%, 1%≤MgO≤5%, 2%≤Na2O≤10%, and 3%≤F≤5%. Its physical properties are: alkalinity controlled at 0.9~1.1, melting point controlled at 1100~1180℃, and viscosity controlled at 0.4~1 Pa·s. The thickness of the liquid slag layer should be controlled to be 5~12mm; The secondary cooling system has a specific water volume of 0.12~0.13L / kg. The secondary cooling system is divided into three zones and adopts a weak cooling mode. The water volume of the secondary cooling system is allocated according to the principle of gradually reducing the cooling length and cooling intensity of each zone. The cooling water proportion in the foot roller section is 48-52%, the water proportion in the first section of the moving fan section is 29-31%, and the water proportion in the second section of the moving fan section is 18-22%. The chemical composition of the high-nitrogen vanadium microalloyed steel prepared by the aforementioned method, by mass percentage, includes: C≤0.14%, 0.2≤Si≤0.8%, Mn≤1.4%, 0.6≤Ni≤1.5%, 0.4≤Cr≤1.0%, P≤0.015%, S≤0.01%, Ti≤0.005%, 0.05%≤V≤0.1%, 0.012≤N≤0.018%, and 0.01%≤Al≤0.015%.

Citation Information

Patent Citations

  • Method for controlling the cross crack of blank angle of high nitrogen steel casting board containing vanadium

    CN101036939A

  • Method of controlling the net crack of high-nitrogen continuous-casting slab of high strength weathering steel containing vanadium

    CN101036940A