A method for evaluating mechanical properties of single crystal blades

By preparing performance simulation parts at cylindrical positions in single-crystal blade castings and machining mechanical performance specimens, the accuracy problem of evaluating the mechanical performance of single-crystal blades was solved, and real mechanical performance data was obtained, ensuring the accuracy of the design and the safety of the engine.

CN117740512BActive Publication Date: 2024-11-12AECC HUNAN AVIATION POWERPLANT RES INST
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311616869.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-11-12
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

Existing technologies struggle to accurately evaluate the mechanical properties of single-crystal blades, especially when they are small in size, have complex structures, and exhibit significant differences in crystal orientation, leading to inaccurate and inconsistent test results.

Method used

Performance simulation parts were prepared by designing a cylindrical position parallel to the stacking axis of the single-crystal blade casting. Tensile, endurance, and rotational bending fatigue specimens were then machined and tested and evaluated using appropriate testing machines to ensure that the material and crystal orientation of the specimens were consistent with those of the single-crystal blade.

Benefits of technology

To minimize testing errors caused by other factors, we can obtain the true mechanical performance data of single-crystal blades, ensuring that the design meets requirements and the engine is safely in service.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117740512B_ABST
    Figure CN117740512B_ABST
Patent Text Reader

Abstract

The present application discloses a method for evaluating the mechanical properties of a single crystal blade, including the following steps: S1, selection of blade sampling position: selecting a design circle at the center position where the outer contour of the blade tip section is the thickest, and extending a cylinder from the circle to the blade tip and the tenon in parallel with the blade stacking axis; S2, preparation of blade performance simulation parts: designing a blade performance simulation part model including the above-mentioned cylinder in the three-dimensional digital model of the single crystal blade casting, and preparing the blade performance simulation part using the same process technology as the blade casting; S3, mechanical performance sample processing: processing mechanical performance samples on the cylinder of the blade performance simulation part based on the spatial coordinates of the blade casting; S4, testing and evaluation of mechanical properties: testing the performance of the samples respectively through the corresponding testing machine and test requirements, and comparing with the blade design requirements to obtain evaluation results. The present application can eliminate the test errors caused by other factors to the greatest extent, and accurately reflect the true mechanical performance level of the single crystal blade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of blade testing, and in particular to a method for evaluating the mechanical properties of a single crystal blade. Background Art

[0002] Single crystal high temperature alloy is developed on the basis of directionally solidified columnar crystal. The alloy structure grows in a predetermined direction to form a single columnar crystal. The thermal strength of the alloy is significantly improved and the comprehensive performance is excellent. Single crystal high temperature alloy is a key material for manufacturing hot end components such as turbine blades and guide vanes of advanced aircraft engines.

[0003] The evaluation of the mechanical properties of single crystal blades has always been an important focus of design and manufacturing. Single crystal blades are subjected to high temperatures and high pressures during use, and turbine blades also have harsh working environments such as high speeds. The static strength, endurance life, fatigue and other mechanical performance indicators of single crystal blades are required to be evaluated during their use and design.

[0004] The evaluation of the mechanical properties of single crystal blades is also a technical difficulty. Turbine working blades are small in size and complex in structure, making it difficult to directly sample and analyze them on the blades. In addition, the mechanical properties of single crystal blades are also affected by crystal orientation factors, and the properties vary in different crystal orientation directions. Therefore, the evaluation method of single crystal mechanical properties involves many links such as blade structure, size, sampling, metallurgy, and inspection. Whether the evaluation method is reasonable seriously affects the evaluation results of single crystal blades, and thus affects the design of single crystal blades and the safe service of the engine.

[0005] At present, the evaluation methods of the mechanical properties of single crystal blades can adopt single casting mechanical properties test bar test, blade sampling test and other methods, but they all have disadvantages:

[0006] The single-cast mechanical properties test bar test is to prepare the mechanical properties test bar using the same process on other modules, and then test and evaluate the tensile, endurance, fatigue and other mechanical properties. However, the size and shape of the single-cast mechanical properties test bar are significantly different from those of the single-crystal blade. In addition, the crystal orientation and microstructure of the single-cast mechanical properties test bar are also different from those of the single-crystal blade. Therefore, the mechanical properties of the single-cast mechanical properties test bar cannot completely replace the mechanical properties of the single-crystal blade.

[0007] The blade sampling test is to prepare a small non-standard sample on a single crystal blade for mechanical property testing. Its size is usually about 10mm. Although this method ensures that the mechanical performance structure is consistent with that of a single crystal blade, the crystal orientation of the test is quite different from that of a single crystal blade. In addition, the shape of the sample taken on the blade is completely non-standard, with a curved surface structure, and poor sample consistency. Factors such as crystal orientation, shape, and sample make the test results extremely scattered, and the test data cannot represent the mechanical properties of the blade. Summary of the invention

[0008] In view of the deficiencies in the prior art, the present invention provides a method for evaluating the mechanical properties of a single crystal blade. The method evaluates the mechanical properties of a single crystal blade through a blade performance simulation part. The purpose of the method is to eliminate the test errors caused by other factors to the greatest extent possible and to accurately reflect the actual mechanical performance level of the single crystal blade.

[0009] The technical solutions adopted in this application are as follows:

[0010] A method for evaluating the mechanical properties of a single crystal blade comprises the following steps:

[0011] S1. Selection of blade sampling position: select the design circle at the center position where the outer contour of the blade tip section is the thickest, and extend a cylinder from the blade tip and the tenon parallel to the blade stacking axis based on the circle. The cylinder position is the blade sampling position;

[0012] S2. Preparation of blade performance simulation parts: a blade performance simulation part model including the above-mentioned cylinder is designed in the three-dimensional digital model of the single crystal blade casting, and the blade performance simulation part is prepared by using the same process technology as the blade casting;

[0013] S3. Mechanical properties specimen processing: Based on the spatial coordinates of the blade casting, mechanical properties specimens are processed on the cylinder of the blade performance simulation part to obtain tensile specimens, endurance specimens, and rotary bending fatigue specimens;

[0014] S4. Testing and evaluation of mechanical properties: The tensile performance test, endurance performance test and rotary bending fatigue performance test are carried out on the obtained tensile, endurance and rotary bending fatigue specimens through universal tensile testing machine, endurance testing machine and rotary bending fatigue testing machine according to the corresponding test requirements, and the evaluation results are compared with the blade design requirements.

[0015] Furthermore, in step S1, the diameter of the designed circle is 6-8 mm, and the cylinder exceeds the tip and the tenon by 5-20 mm respectively.

[0016] Furthermore, in step S2, when the three-dimensional digital model design of the single crystal blade casting includes the blade performance simulation model of the above-mentioned cylinder, the cylinder exceeds the boundary of the original casting to perform a smooth transition to a guide circle, and the transition between the seeding end and the cylinder is smooth.

[0017] Furthermore, in step S2, when the blade performance simulation part is prepared by the same process technology as the blade casting, a wax mold is prepared according to the blade performance simulation part model, and the blade performance simulation part is prepared by the same master alloy, wax mold pressing, shell mold, directional solidification, and heat treatment process as the blade casting.

[0018] Furthermore, in step S3, based on the spatial coordinates of the blade casting, before machining the mechanical properties specimen of the blade performance simulation part, the following steps are also included:

[0019] The blade performance simulation parts are inspected for grain size and crystal orientation, and blade performance simulation parts that meet the requirements of single crystal blades are selected for sample processing.

[0020] Furthermore, in step S3, the deviation between the center line of the tensile specimen, the endurance specimen, and the rotary bending fatigue specimen and the blade stacking axis is less than 2°.

[0021] Furthermore, in step S3, the working end diameters of the tensile specimen and the endurance specimen are 2.5 to 4 mm, the lengths are 10 to 20 mm, and the center diameter of the rotary bending fatigue specimen is 3.5 to 4 mm.

[0022] Furthermore, the step S4 comprises the steps of:

[0023] S41. Test the tensile properties at 1 to 4 temperatures in the range of 600°C to 1200°C. Use 2 to 4 tensile specimens at each tensile test temperature to perform tensile strength tests on a universal tensile testing machine according to ASTME 21 or HB5195. Take the minimum value and compare it with the blade design static strength to obtain the evaluation result.

[0024] Furthermore, the step S4 comprises the steps of:

[0025] S42. Test the endurance performance at 1 to 4 temperatures in the range of 600℃ to 1200℃, and conduct 3 to 6 stress tests at each temperature. Use 1 to 3 endurance specimens in an endurance testing machine for each endurance performance test condition. Test the endurance fracture life according to ASTME139 or HB 5150. Use the Larson-Miller equation to process the test data, calculate the endurance strength and compare it with the blade design strength to obtain the evaluation result.

[0026] Furthermore, the step S4 comprises the steps of:

[0027] S43, test the rotary bending fatigue performance at 1 to 4 temperatures in the range of 600℃ to 1100℃. For each rotary bending fatigue test temperature, 10 to 15 rotary bending fatigue specimens are used in a rotary bending fatigue testing machine. The lifting method is used to test different load cycles according to HB5153. Calculate 10 7 The rotational bending fatigue strength corresponding to the cycles is compared with the blade design strength to obtain the evaluation results.

[0028] Compared with the prior art, this application has the following beneficial effects:

[0029] The present application provides a method for evaluating the mechanical properties of a single crystal blade. The method evaluates the mechanical properties of a single crystal blade through a blade performance simulation part. Specifically, a cylindrical specimen processing position parallel to the stacking axis of the single crystal blade casting is designed and the performance simulation part is prepared. The mechanical property specimen is then processed and tested and evaluated using a corresponding testing machine to obtain the mechanical properties of the single crystal blade. The material, crystal orientation and microstructure of the mechanical property specimen obtained by the method are basically consistent with those of the single crystal blade. At the same time, the standardization of the specimen is guaranteed. Therefore, the test results exclude the test errors caused by other factors to the greatest extent, and can accurately reflect the actual mechanical property level of the single crystal blade, thereby obtaining accurate real mechanical performance data of the single crystal blade, ensuring that the design of the single crystal blade meets the requirements and the safe service of the engine.

[0030] In addition to the above-described purposes, features and advantages, the present application also has other purposes, features and advantages. The present application will be further described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0032] Figure 1 This is a schematic flow chart of a method for evaluating the mechanical properties of a single crystal blade according to a preferred embodiment of the present application.

[0033] Figure 2 This is a schematic diagram of the sub-step flow of step S4 of the preferred embodiment of the present application.

[0034] Figure 3 This is a schematic flow chart of the sub-steps of step S4 of another preferred embodiment of the present application.

[0035] Figure 4 This is a schematic flow chart of the sub-steps of step S4 of another preferred embodiment of the present application. DETAILED DESCRIPTION

[0036] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0037] like Figure 1 The preferred embodiment of the present application provides a method for evaluating the mechanical properties of a single crystal blade, comprising the steps of:

[0038] S1. Selection of blade sampling position: select the design circle at the center position where the outer contour of the blade tip section is the thickest, and extend a cylinder from the blade tip and the tenon parallel to the blade stacking axis based on the circle. The cylinder position is the blade sampling position;

[0039] S2. Preparation of blade performance simulation parts: a blade performance simulation part model including the above-mentioned cylinder is designed in the three-dimensional digital model of the single crystal blade casting, and the blade performance simulation part is prepared by using the same process technology as the blade casting;

[0040] S3. Mechanical properties specimen processing: Based on the spatial coordinates of the blade casting, mechanical properties specimens are processed on the cylinder of the blade performance simulation part to obtain tensile specimens, endurance specimens, and rotary bending fatigue specimens;

[0041] S4. Testing and evaluation of mechanical properties: The tensile performance test, endurance performance test and rotary bending fatigue performance test are carried out on the obtained tensile, endurance and rotary bending fatigue specimens through universal tensile testing machine, endurance testing machine and rotary bending fatigue testing machine according to the corresponding test requirements, and the evaluation results are compared with the blade design requirements.

[0042] The present embodiment provides a method for evaluating the mechanical properties of a single crystal blade, which evaluates the mechanical properties of a single crystal blade through a blade performance simulation part, specifically by designing a cylindrical specimen processing position parallel to its stacking axis on the single crystal blade casting, and preparing the performance simulation part, and then processing the mechanical property specimen, and using a corresponding testing machine for testing and evaluation to obtain the mechanical properties of the single crystal blade. The material, crystal orientation, and microstructure of the mechanical property specimen obtained by this method are basically consistent with those of the single crystal blade, and the standardization of the specimen is guaranteed. Therefore, the test results exclude the test errors caused by other factors to the greatest extent, and have the advantages of data standardization and accurately reflecting the actual mechanical property level of the single crystal blade, thereby obtaining accurate real mechanical performance data of the single crystal blade to truly reflect the mechanical properties of the blade, ensuring that the design of the single crystal blade meets the requirements and the safe service of the engine.

[0043] Preferably, in step S1, the diameter of the designed circle is 6-8 mm, and the cylinder exceeds the tip and the tenon by 5-20 mm, respectively, in order to ensure that a specimen for mechanical property testing is processed.

[0044] Preferably, in step S2, when the three-dimensional digital model design of the single crystal blade casting includes the blade performance simulation model of the above-mentioned cylinder, the cylinder extends beyond the boundary of the original casting to perform a smooth transition to a guide circle, and the transition between the seeding end and the cylinder is smooth, the purpose of which is to improve the casting processability of the blade performance simulation part.

[0045] Preferably, in step S2, when the blade performance simulation part is prepared by the same process technology as the blade casting, a wax mold is prepared according to the blade performance simulation part model, and the blade performance simulation part is prepared by the same master alloy, wax mold pressing, shell mold, directional solidification, and heat treatment process as the blade casting, so that the performance parameters of the blade performance simulation part are as similar as possible to those of the blade casting.

[0046] Preferably, in step S3, based on the spatial coordinates of the blade casting, before machining the mechanical properties specimen of the blade performance simulation part, the step of:

[0047] The blade performance simulation parts are inspected for grain size and crystal orientation, and blade performance simulation parts that meet the requirements of single crystal blades are selected for sample processing.

[0048] Before processing the mechanical property specimens, the present embodiment will also conduct grain size and crystal orientation inspections on the blade performance simulation parts, and select blade performance simulation parts that meet the requirements of single crystal blades for specimen processing. Thus, on the basis of the aforementioned preparation of the blade performance simulation parts to make various performance parameters as similar as possible to those of the blade castings, through secondary screening, some blade performance simulation parts whose grain size and crystal orientation do not meet the requirements of single crystal blades are eliminated, thereby further avoiding the disadvantage that the crystal orientation and microstructure of the specimen are different from those of the single crystal blade, resulting in the mechanical properties of the specimen not being able to completely replace the mechanical properties of the single crystal blade. The crystal orientation and microstructure of the mechanical property specimen are made as consistent as possible with those of the single crystal blade, ensuring that the mechanical properties of the mechanical property specimen can completely replace the mechanical properties of the single crystal blade, thereby eliminating the test errors caused by inconsistent crystal orientation and microstructure, and achieving the purpose of accurately reflecting the true mechanical property level of the single crystal blade.

[0049] Preferably, in step S3, the deviation between the center line of the tensile specimen, the endurance specimen, and the rotary bending fatigue specimen and the blade stacking axis is less than 2°, the purpose and benefit of which is to enable the processed specimen to accurately represent the blade performance.

[0050] Preferably, in step S3, the working end diameters of the tensile specimen and the endurance specimen are 2.5 to 4 mm, the lengths are 10 to 20 mm, and the center diameter of the rotary bending fatigue specimen is 3.5 to 4 mm. The benefit and purpose is to ensure that the tensile, endurance, and rotary bending fatigue performance data obtained from the test are stable and valid.

[0051] like Figure 2 As shown, in a preferred embodiment of the present application, step S4 includes the steps of:

[0052] S41. Test the tensile properties at 1 to 4 temperatures in the range of 600°C to 1200°C. Use 2 to 4 tensile specimens at each tensile test temperature to perform tensile strength tests on a universal tensile testing machine according to ASTME 21 or HB5195. Take the minimum value and compare it with the blade design static strength to obtain the evaluation result.

[0053] In this embodiment, a universal tensile testing machine is used to perform tensile strength tests on multiple tensile specimens at multiple temperatures within a temperature test range according to ASTME 21 or HB5195, and the minimum value is taken for comparison and evaluation with the blade design static strength to obtain an evaluation result, thereby obtaining a more comprehensive and reliable tensile performance evaluation result.

[0054] like Figure 3 As shown, in a preferred embodiment of the present application, step S4 includes the steps of:

[0055] S42. Test the endurance performance at 1 to 4 temperatures in the range of 600℃ to 1200℃, and conduct 3 to 6 stress tests at each temperature. Use 1 to 3 endurance specimens in an endurance testing machine for each endurance performance test condition. Test the endurance fracture life according to ASTME139 or HB 5150. Use the Larson-Miller equation to process the test data, calculate the endurance strength and compare it with the blade design strength to obtain the evaluation result.

[0056] In this embodiment, a durability tester is used to test the durability fracture life of multiple durability specimens according to ASTME139 or HB 5150 at multiple temperatures within a temperature test range, and the Larson-Miller equation is used to process the test data, and the durability strength is calculated and compared with the blade design strength to obtain an evaluation result, thereby obtaining a more comprehensive and reliable durability performance evaluation result.

[0057] like Figure 4 As shown, in a preferred embodiment of the present application, step S4 includes the steps of:

[0058] S43, test the rotary bending fatigue performance at 1 to 4 temperatures in the range of 600℃ to 1100℃. For each rotary bending fatigue test temperature, 10 to 15 rotary bending fatigue specimens are used in a rotary bending fatigue testing machine. The lifting method is used to test different load cycles according to HB5153. Calculate 10 7 The rotational bending fatigue strength corresponding to the cycles is compared with the blade design strength to obtain the evaluation results.

[0059] In this embodiment, a plurality of rotating bending fatigue specimens are subjected to a lifting method at multiple temperatures within a temperature test range by a rotating bending fatigue testing machine, and different load cycles are tested according to HB 5153. The load cycles are calculated for 10 7The rotational bending fatigue strength corresponding to the cycles is compared with the blade design strength to obtain the evaluation result, so as to obtain a more comprehensive and reliable rotational bending fatigue performance evaluation result.

[0060] In summary, the evaluation method of the present application is to prepare tensile, endurance, and rotational bending fatigue mechanical property specimens on a single crystal blade performance simulation part that are consistent with the crystal orientation of the blade stacking axis, and use a universal tensile testing machine, an endurance testing machine, and a rotary bending fatigue testing machine to respectively test the tensile, endurance, and rotational bending fatigue mechanical property specimens to obtain the tensile, endurance, and rotational bending fatigue performance data of the single crystal blade, and evaluate the mechanical properties of the single crystal blade respectively.

[0061] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for evaluating the mechanical properties of single crystal blades. It is characterized in that Includes steps: S1. Selection of blade sampling position: select the design circle at the center position where the outer contour of the blade tip section is the thickest, and extend a cylinder from the blade tip and the tenon parallel to the blade stacking axis based on the circle. The cylinder position is the blade sampling position; S2. Preparation of blade performance simulation parts: a blade performance simulation part model including the above-mentioned cylinder is designed in the three-dimensional digital model of the single crystal blade casting, and the blade performance simulation part is prepared by using the same process technology as the blade casting; S3. Mechanical properties specimen processing: Based on the spatial coordinates of the blade casting, mechanical properties specimens are processed on the cylinder of the blade performance simulation part to obtain tensile specimens, endurance specimens, and rotary bending fatigue specimens; S4. Testing and evaluation of mechanical properties: The tensile performance test, endurance performance test and rotary bending fatigue performance test are respectively carried out on the obtained tensile, endurance and rotary bending fatigue specimens by means of a universal tensile testing machine, an endurance testing machine and a rotary bending fatigue testing machine according to the corresponding test requirements, and the evaluation results are compared with the blade design requirements; The diameter of the designed circle is 6-8 mm, and the cylinder protrudes 5-20 mm at the tip and the tenon respectively; In step S3, based on the spatial coordinates of the blade casting, before the cylindrical mechanical properties specimen of the blade performance simulation part is processed, the following steps are also included: Conduct grain size and crystal orientation tests on blade performance simulation parts, and select blade performance simulation parts that meet the requirements of single crystal blades for sample processing; In step S3, the working end diameters of the tensile specimen and the endurance specimen are 2.5 to 4 mm, the lengths are 10 to 20 mm, and the center diameter of the rotary bending fatigue specimen is 3.5 to 4 mm.

2. The method for evaluating mechanical properties of a single crystal blade according to claim 1, It is characterized in that In step S2, when the three-dimensional digital model design of the single crystal blade casting includes the blade performance simulation model of the cylinder, the cylinder exceeds the boundary of the original casting to perform a smooth transition to a guide circle, and the transition between the seeding end and the cylinder is smooth.

3. The method for evaluating mechanical properties of a single crystal blade according to claim 1, It is characterized in that In step S2, when the blade performance simulation part is prepared using the same process technology as the blade casting, a wax mold is prepared according to the blade performance simulation part model, and the blade performance simulation part is prepared using the same master alloy, wax mold pressing, shell mold, directional solidification, and heat treatment process as the blade casting.

4. The method for evaluating mechanical properties of a single crystal blade according to claim 1, It is characterized in that In step S3, the deviation between the center line of the tensile test specimen, the endurance test specimen, and the rotary bending fatigue test specimen and the blade stacking axis is less than 2°.

5. The method for evaluating mechanical properties of a single crystal blade according to claim 1, It is characterized in that The step S4 comprises the steps of: S41. Test the tensile properties at 1 to 4 temperatures in the range of 600°C to 1200°C. Use 2 to 4 tensile specimens at each tensile test temperature to perform tensile strength tests on a universal tensile testing machine according to ASTME 21 or HB5195. Take the minimum value and compare it with the blade design static strength to obtain the evaluation result.

6. The method for evaluating mechanical properties of a single crystal blade according to claim 1, It is characterized in that The step S4 comprises the steps of: S42. Test the endurance performance at 1 to 4 temperatures in the range of 600℃ to 1200℃, and conduct 3 to 6 stress tests at each temperature. Use 1 to 3 endurance specimens in an endurance testing machine for each endurance performance test condition. Test the endurance fracture life according to ASTME139 or HB 5150. Use the Larson-Miller equation to process the test data, calculate the endurance strength and compare it with the blade design strength to obtain the evaluation result.

7. The method for evaluating mechanical properties of a single crystal blade according to claim 1, It is characterized in that The step S4 comprises the steps of: S43, test the rotary bending fatigue performance at 1 to 4 temperatures in the range of 600℃ to 1100℃. For each rotary bending fatigue test temperature, 10 to 15 rotary bending fatigue specimens are used in a rotary bending fatigue testing machine. The lifting method is used to test different load cycles according to HB 5153. Calculate 10 7 The rotational bending fatigue strength corresponding to the cycles is compared with the blade design strength to obtain the evaluation results.

Citation Information

Patent Citations

  • Test method based on creep properties of single crystal blade

    CN110320117A

  • Simulation evaluation method for mechanical property attenuation of turbine blade in full-area corrosion environment

    CN114705534A

  • Preparation process of seed crystal for casting nickel-based single crystal blade with precisely controllable three-dimensional orientation

    CN114850406A

  • Method for designing thermal mechanical fatigue simulation piece at turbulent flow column part of single-crystal turbine blade

    CN114861356A

  • Method and device for testing primary orientation of single-crystal high-temperature alloy and storage medium

    CN115656234A