A sodium ion layered metal oxide material, preparation method thereof, positive electrode material and sodium ion battery

By doping F and M elements into sodium ion layered metal oxide materials and adopting specific calcining procedures, the problem of structural deterioration and capacity attenuation of the positive electrode material of sodium ion battery during charging and discharging is solved, and the stability of the material is improved and electrochemical properties, achieving high discharge specific capacity and cycling performance.

CN117747834BActive Publication Date: 2024-12-03HUBEI WANRUN NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311784522.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2024-12-03
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

The sodium ion layered transition metal oxide positive electrode material has serious structural deterioration and capacity attenuation problems during charging and discharging, especially the multiphase transition caused by O3 high-nickel materials when charged to a higher voltage leads to volume deformation and electrolyte. Decomposition leads to deterioration of the electrode material structure and capacity attenuation.

Method used

By doping F and M elements, especially Zn, Mg, Sn, Sb, Y and Cu, the lattice structure is adjusted, the diffusion rate of Na+ is increased, the lattice distortion caused by the Jahn-Teller effect of active ions such as Mn3+ is suppressed, and Specific calcination procedures are used to reduce side reactions and heterogeneous phase generation and improve material stability and uniformity.

Benefits of technology

It significantly improves the structural stability and electrochemical performance of sodium ion layered metal oxide materials, improves the discharge specific capacity and cycling performance, and extends the cycle life of the electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004625777050000011
    Figure HDA0004625777050000011
  • Figure HDA0004625777050000012
    Figure HDA0004625777050000012
  • Figure HDA0004625777050000021
    Figure HDA0004625777050000021
Patent Text Reader

Abstract

The present invention provides a sodium ion layered metal oxide material, a preparation method thereof, a positive electrode material and a sodium ion battery, belonging to the technical field of sodium ion batteries. The sodium ion layered metal oxide material has a chemical formula shown in formula I: Na x Ni a Mn b Ti (0.5‑b) M (0.5‑a) O (2‑y) F y Formula I; 0.9≤x≤1.0, 0.3≤a<0.5, 0.3≤b≤0.4, 0.1≤1‑a‑b≤0.35, 0≤y<0.1, M includes at least one of Zn, Mg, Sn, Sb, Y and Cu. By doping F element and M element, it is helpful to improve the structural stability of the material. In addition, the preparation method of the present invention can reduce the generation of impurities and make the distribution of M element in the finished product more uniform, so that the positive electrode sheet and sodium ion battery containing the sodium ion layered metal oxide material have higher discharge specific capacity and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a sodium ion layered metal oxide material, a preparation method thereof, a positive electrode material and a sodium ion battery. Background Art

[0002] The commercialization of electrochemical power sources, especially lithium-ion batteries (LIBs), has ushered in a new era of portable electronics and electric vehicles, greatly facilitating daily life. However, driven by concerns about the depletion of lithium resources and the volatile prices of lithium, nickel, and cobalt raw materials, sodium-ion batteries (NIBs) have been intensively studied and have become a strong competitor in energy storage fields such as national grid and home energy storage. The cathode is an indispensable part of NIBs and directly determines all key properties of NIBs, such as cost, safety, energy density, power density, and cycle life. In addition, the ideal cathode material should be relatively environmentally friendly and easy to mass produce, transport, and store.

[0003] Cost is the core factor driving the competition between sodium-ion batteries and lithium-ion batteries. Manganese has the advantages of being environmentally friendly, low in price, and high in annual output. x TMO2) has many electrochemical redox active elements such as Mn, Fe, Cu, Ni, Co, Cr, Ir, Ru and O, and its chemical composition can be flexibly designed. It has high specific capacity and good safety performance, making it a strong competitor for commercial sodium-ion battery cathode materials.

[0004] The general formula of the current sodium ion layered transition metal oxide cathode material is Na x TMO2, along with Na + The change of content forms different structures. Common structures include O3, P3, O'3 and P2 phases. The transition metal positions in layered oxides can be occupied by various metal ions (such as Li, Na, Mg, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Sn, Ir, Ru, etc.). The extranuclear electron configuration, oxidation state, and TM-O bond energy of these metal ions vary greatly, and with the change of Na + The change in content constitutes layered oxide positive electrode materials with different structures. The O3 type high nickel material has a high specific capacity, but when it is charged to a higher voltage, it not only causes multiphase transformation and leads to a large volume deformation, but also promotes the decomposition of the electrolyte to induce the co-embedding of solvent molecules, which ultimately leads to serious structural deterioration and capacity decay of the electrode material during the charge and discharge process. Summary of the invention

[0005] In view of the technical problems existing in the background technology, the present invention provides a sodium ion layered metal oxide material, a preparation method thereof, a positive electrode material and a sodium ion battery, aiming to solve the technical problems of serious structural deterioration and capacity attenuation of the positive electrode material during the charging and discharging process.

[0006] In a first aspect, the present invention provides a sodium ion layered metal oxide material having a chemical formula shown in Formula I:

[0007] Na x Ni a Mn b Ti (0.5-b) M (0.5-a) O (2-y) F y Formula I;

[0008] Among them, 0.9≤x≤1.0, 0.3≤a<0.5, 0.3≤b≤0.4, 0.1≤1-ab≤0.35, 0≤y<0.1, and M includes at least one of Zn, Mg, Sn, Sb, Y and Cu.

[0009] In the embodiment of the present invention, the M element helps to improve the stability of the material. - Radius and O 2- The radius is similar, so it is feasible for F to replace O. By controlling the doping amount of F, it is possible to avoid excessive impurities in the finished product due to F doping; the strong electronegativity of F can change the binding energy of oxygen elements in the lattice, thereby increasing the Na + The diffusion rate of Mn 3+ The Jahn-Teller effect of active ions causes lattice distortion and improves the stability of the structure.

[0010] Preferably, the sodium ion layered metal oxide material is an O3 type manganese-based layered oxide material.

[0011] In a second aspect, the present invention provides a method for preparing the sodium ion layered metal oxide material as described above, comprising the following steps:

[0012] A) mixing a Na source, a Ni source, a Mn source, a Ti source, a M source and a F source with a solvent according to the stoichiometric ratio in formula I and then coarsely grinding the mixture to obtain a first slurry;

[0013] B) grinding the first slurry to obtain a second slurry;

[0014] C) spray drying the second slurry to obtain a first powder;

[0015] D) calcining the powder according to the following procedure to obtain a second powder,

[0016] In an oxygen-containing atmosphere, heat from room temperature to 110-130°C at a heating rate of 3-5°C / min, keep warm for 2-4 hours, then heat to 440-460°C at a heating rate of 5-8°C / min, keep warm for 1-3 hours, then heat to 850-950°C at a heating rate of 5-8°C / min, keep warm for 10-20 hours;

[0017] E) crushing, screening and removing iron from the second powder to obtain a sodium ion layered metal oxide material having a chemical formula I;

[0018] Na x Ni a Mn b Ti (0.5-b) M (0.5-a) O (2-y) F y Formula I;

[0019] Among them, 0.9≤x≤1.0, 0.3≤a<0.5, 0.3≤b≤0.4, 0.1≤1-ab≤0.35, 0≤y<0.1, and M includes at least one of Zn, Mg, Sn, Sb, Y and Cu.

[0020] In an embodiment of the present invention, the second powder is calcined using a specific programmed temperature rise, which can reduce the occurrence of side reactions and the generation of impurities, while making the distribution of copper in the finished product more uniform, improving the uniformity of the material and the stability of the product, and further improving the electrochemical performance.

[0021] Preferably, the sodium ion layered metal oxide material is Na 0.95 Ni 0.45 Mn 0.3 Cu 0.05 Ti 0.2 O 1.95 F 0.05 ,NaNi 0.48 Mn 0.4 Y 0.02 Ti 0.1 O 1.999 F 0.001 and Na 0.9 Ni 0.48 Mn 0.39 Cu 0.02 Mg 0.01 Ti 0.1 One or more of O2.

[0022] Preferably, the calcination procedure is specifically:

[0023] In an oxygen-containing atmosphere, heat from room temperature to 120-125°C at a heating rate of 4-5°C / min, keep warm for 2-3 hours, then heat to 450-455°C at a heating rate of 5-7°C / min, keep warm for 1-2 hours, then heat to 850-950°C at a heating rate of 5-8°C / min, and keep warm for 13-20 hours.

[0024] Preferably, the solvent used for the coarse grinding in step A) is water and / or alcohol, the solid content of the first slurry is 10-40%, and the blockage of the coarse grinder, the sand mill and the connecting pipes is avoided while ensuring the output, and the particle size of the first slurry is D100<10μm, so as to avoid the particles in the slurry clogging the sand mill filter.

[0025] Preferably, the particle size of the second slurry is D50<3μm, D100<8μm, so as to ensure that the particle size distribution of the first powder obtained after spray drying is more concentrated and avoid the appearance of large particles; the slurry is uniform, and the particle size of the second slurry is smaller, which does not allow sufficient contact between the particles, which is conducive to ensuring the uniformity of the cation distribution in the finished product.

[0026] In the embodiment of the present invention, grinding after rough grinding can ensure that each insoluble particle in the slurry is fully ground, ensure the uniformity of the slurry, and improve the grinding efficiency.

[0027] Preferably, the particle size of the first powder is 2 μm<D50<15 μm, D100<40 μm, the moisture content is less than 1.5%, and BET>15 μm. 2 / g.

[0028] In an embodiment of the present invention, the first powder meets the above-mentioned indicators to ensure that less water vapor is generated during sintering of the first powder, thereby avoiding sodium precipitation. The small particle size and large BET of the first powder ensure more complete contact between particles during sintering, which facilitates ion exchange and migration, thereby ensuring that the sintered material has higher crystallinity, more uniform cation distribution, and fewer impurities.

[0029] Preferably, during the calcination process, the oxygen content is 20-35%, the moisture content is less than 3%, and the carbon dioxide concentration is less than 1%.

[0030] In an embodiment of the present invention, the moisture, oxygen content and carbon dioxide content in the high-temperature furnace are detected online during the sintering process, and the gas introduction amount, exhaust amount, and the ratio of oxygen and nitrogen in the introduced gas are adjusted in time to control the moisture, oxygen content and carbon dioxide content in the high-temperature furnace within a control range, thereby avoiding excessive oxygen content and the formation of too many impurities during the sintering process.

[0031] Preferably, rapid cooling is performed after calcination to obtain the second powder; the rapid cooling is a quenching treatment.

[0032] In the embodiment of the present invention, accelerating the cooling rate during the cooling process after calcination is helpful to form a 3+ And the metastable phase with high sodium content between the layers improves the reversible capacity of the electrode material.

[0033] In a third aspect, the present invention provides a positive electrode plate, comprising the sodium ion layered metal oxide material described above or the sodium ion layered metal oxide material prepared by the preparation method described above.

[0034] In an embodiment of the present invention, the positive electrode plate includes the above-mentioned sodium ion layered metal oxide material, and thus has better structural stability, higher discharge specific capacity and higher capacity retention rate.

[0035] In a fourth aspect, the present invention provides a sodium ion battery comprising the positive electrode sheet described above.

[0036] In an embodiment of the present invention, the sodium ion battery includes the above-mentioned positive electrode plate, and thus has a higher discharge specific capacity and higher cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0038] Figure 1 This is a SEM image of the sodium ion layered metal oxide material in Example 1 of the present invention;

[0039] Figure 2 is the XRD pattern of the sodium ion layered metal oxide material in Example 1 of the present invention;

[0040] Figure 3 : is the charge and discharge curve of the button battery in Example 1 of the present invention;

[0041] Figure 4 : is the charge and discharge curve of the button battery in Example 2 of the present invention;

[0042] Figure 5 This is a SEM image of the sodium ion layered metal oxide material in Example 2 of the present invention;

[0043] Figure 6 : is the charge and discharge curve of the button battery in Example 3 of the present invention;

[0044] Figure 7This is a SEM image of the sodium ion layered metal oxide material in Example 3 of the present invention. DETAILED DESCRIPTION

[0045] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0047] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0048] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0049] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0050] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0051] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0052] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0053] Among the current structures of sodium ion layered transition metal oxide positive electrode materials, O3-type high-nickel materials have a higher specific capacity. However, when charged to a higher voltage, it not only causes multiphase transformation leading to a larger volume deformation, but also promotes the decomposition of the electrolyte to induce the co-embedding of solvent molecules, ultimately leading to serious structural deterioration and capacity attenuation of the electrode material during the charge and discharge process.

[0054] In order to solve the above technical problems, the present invention provides a sodium ion layered metal oxide material, a preparation method thereof, a positive electrode sheet and a sodium ion battery, wherein doping with F and M elements helps to improve the stability of the material, and the strong electronegativity of F can change the binding energy of oxygen elements in the lattice, thereby increasing the Na + The diffusion rate of Mn 3+ The Jahn-Teller effect of active ions causes lattice distortion, which improves the stability of the structure. In addition, the present invention can reduce the occurrence of side reactions and the generation of impurities by calcining the second powder using a specific program temperature increase, while making the distribution of copper in the finished product more uniform, improving the uniformity of the material and the stability of the product, and further improving the electrochemical performance. As a result, the positive electrode sheet and sodium ion battery using the sodium ion layered metal oxide material have a higher discharge specific capacity and higher cycle performance.

[0055] In a first aspect, the present invention provides a sodium ion layered metal oxide material, which is an O3-type manganese-based layered oxide material having a chemical formula shown in Formula I:

[0056] Nax Ni a Mn b Ti (0.5-b) M (0.5-a) O (2-y) F y Formula I;

[0057] Among them, 0.9≤x≤1.0, 0.3≤a<0.5, 0.3≤b≤0.4, 0.1≤1-ab≤0.35, 0≤y<0.1, and M includes at least one of Zn, Mg, Sn, Sb, Y and Cu.

[0058] In one embodiment of the present invention, 0.9≤x≤1.0, preferably, 0.92≤x≤0.98, such as x is 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1.0, preferably a range value with any of the above values ​​as the upper or lower limit.

[0059] In one embodiment of the present invention, 0.3≤a<0.5, preferably, 0.35≤a≤0.45, such as a is 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, preferably a range value with any of the above values ​​as the upper or lower limit.

[0060] In one embodiment of the present invention, 0<(0.5-a)≤0.2, preferably, 0.01≤(0.5-a)≤0.05. Within this range, it is possible to avoid excessive proportion of the M element. Since the M element has poor compatibility with oxides of elements such as Ni, Mn, and Ti during the sintering process, there are more impurities in the finished product, which in turn causes the energy density of the material to be too low.

[0061] In one embodiment of the present invention, 0.3≤b≤0.4, preferably, 0.32≤b≤0.38, such as b is 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, preferably a range value with any of the above values ​​as the upper or lower limit.

[0062] In one embodiment of the present invention, 0.1≤1-ab≤0.35, preferably, 0.2≤1-ab≤0.3.

[0063] In one embodiment of the present invention, 0≤y<0.1, preferably, 0.01≤y≤0.08, such as y is 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, preferably with any of the above values ​​as the upper or lower limit of the range value. When the y value is within the above range, it can avoid that the F element accounts for too high a proportion, resulting in more impurities (such as nickel oxide) in the finished product, and the energy density of the material is too low and the structural stability is poor.

[0064] Specifically, in an embodiment of the present invention, the sodium ion layered metal oxide material is Na 0.95 Ni 0.45 Mn 0. 3Cu 0.05 Ti 0.2 O 1.95 F 0.05 ,NaNi 0.48 Mn 0.4 Y 0.02 Ti 0.1 O 1.999 F 0.001 and Na 0.9 Ni 0.48 Mn 0.39 Cu 0.02 Mg 0.01 Ti 0.1 One or more of O2.

[0065] After doping with F and M elements, the capacity retention rate of the material after 100 cycles of 1C is increased by 10% to 15%.

[0066] In a second aspect, the present invention further provides a method for preparing a sodium ion layered metal oxide material, comprising the following steps:

[0067] A) mixing a Na source, a Ni source, a Mn source, a Ti source, a M source and a F source with a solvent according to the stoichiometric ratio in formula I and then coarsely grinding the mixture to obtain a first slurry;

[0068] B) grinding the first slurry to obtain a second slurry;

[0069] C) spray drying the second slurry to obtain a first powder;

[0070] D) calcining the powder according to the following procedure to obtain a second powder,

[0071] In an oxygen-containing atmosphere, heat from room temperature to 110-130°C at a heating rate of 3-5°C / min, keep warm for 2-4 hours, then heat to 440-460°C at a heating rate of 5-8°C / min, keep warm for 1-3 hours, then heat to 850-950°C at a heating rate of 5-8°C / min, keep warm for 10-20 hours;

[0072] E) crushing, screening and removing iron from the second powder to obtain a sodium ion layered metal oxide material having a chemical formula I;

[0073] Na x Ni a Mn b Ti (0.5-b) M (0.5-a) O (2-y) F y Formula I.

[0074] In one embodiment of the present invention, the Na source is preferably one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, sodium acetate, sodium oxalate and sodium citrate; the Ni source is preferably one or more of nickelous oxide (NiO), nickel oxide (Ni2O3), nickel hydroxide [Ni(OH)2], nickel hydroxide [Ni(OH)3], nickel carbonate and nickel oxalate; the Mn source is preferably one or more of manganese tetraoxide, manganese dioxide, manganese trioxide, manganese monoxide, manganese carbonate and manganese oxalate; the Ti source is preferably titanium dioxide and / or metatitanate H2TiO3); the M source is preferably at least one of the oxide of M, the hydroxide of M, the carbonate of M, the oxalate of M and the citrate of M. When the M element is yttrium (Y), the M source is preferably the oxide of Y; the F source is preferably sodium fluoride. In the present invention, the Na source, Ni source, Mn source, Ti source, M source and F source are weighed and mixed according to the molar number of the metal elements in the chemical formula shown in Formula I, which is a common technical means in the field and will not be described in detail in the present invention.

[0075] In one embodiment of the present invention, the solvent used for coarse grinding is preferably water and / or alcohol, more preferably deionized water and / or alcohol, the coarse grinding time is preferably 1 to 3 hours, more preferably 1 to 2 hours; the working frequency of the coarse grinding is preferably 10 to 50 Hz, more preferably 20 to 40 Hz.

[0076] In one embodiment of the present invention, the solid content of the first slurry obtained after rough grinding is preferably 10-40%, more preferably 20-30%, such as 10%, 15%, 20%, 25%, 30%, 35%, 40%, preferably a range value with any of the above values ​​as the upper or lower limit; the particle size of the first slurry is preferably D100<10μm, more preferably D100<5μm.

[0077] After obtaining the first slurry, the present invention grinds the first slurry in a sand mill in an inverted jar circulation manner using an A / B jar circulation method to obtain a second slurry.

[0078] In one embodiment of the present invention, the grinding time is preferably 2 to 5 hours, more preferably 3 to 4 hours, the rotation speed of the sand mill is preferably 200 to 1500 r / min, more preferably 500 to 1000 r / min, and the particle size of the second slurry is preferably D50 < 3 μm, D100 < 8 μm, preferably, D50 < 2 μm, D100 < 5 μm.

[0079] After obtaining the second slurry, the present invention spray-dries the second slurry to obtain a first powder.

[0080] In one embodiment of the present invention, the particle size of the first powder obtained by spray drying is preferably 2 μm<D50<15 μm, D100<40 μm, the moisture content is less than 1.5%, and BET>15 μm. 2 / g, more preferably, 5μm<D50<12μm, D100<30μm, moisture content less than 1.0%, BET>15m 2 / g.

[0081] After obtaining the first powder, the present invention calcines the device, and the calcination is preferably carried out according to the following procedure:

[0082] In an oxygen-containing atmosphere, heat from room temperature to 110-130°C at a heating rate of 3-5°C / min, keep warm for 2-4 hours, then heat to 440-460°C at a heating rate of 5-8°C / min, keep warm for 1-3 hours, then heat to 890-910°C at a heating rate of 5-8°C / min, and keep warm for 10-20 hours.

[0083] In one embodiment of the present invention, the oxygen-containing atmosphere is preferably dry oxygen or dry air, or a mixture of dry oxygen and nitrogen, so as to avoid the material from contacting water and carbon dioxide and deteriorating during the material cooling process. Preferably, the oxygen-containing atmosphere is a mixture of dry oxygen and nitrogen, wherein the volume fraction of oxygen is preferably 25-35%, more preferably 30%, while controlling the oxygen content in the high-temperature furnace to avoid the adverse effects of water and carbon dioxide in the gas on the finished product, which helps to reduce the free sodium content and the pH of the finished product, and avoid the free sodium content and pH of the material being too high, resulting in slurry gelation during battery manufacturing.

[0084] In one embodiment of the present invention, in the first stage, the temperature is first increased from room temperature to 110-130°C at a heating rate of 3-5°C / min and kept warm for 2-4 hours. The purpose of this stage is mainly to reduce the water content of the first powder to avoid excessive moisture content in the high-temperature furnace atmosphere during the subsequent rapid heating process, which may cause side reactions and lead to excessive impurities in the finished product.

[0085] In this stage, the heating rate is preferably 3-5°C / min, more preferably 3-4°C / min; the calcination temperature is preferably 110-130°C, more preferably 115-125°C, such as 110°C, 115°C, 120°C, 125°C, 130°C, preferably a range value with any of the above values ​​as the upper or lower limit; the insulation time is preferably 2-4 hours, more preferably 2-3 hours.

[0086] After the first stage of calcination, the temperature is raised to 440~460℃ at a heating rate of 5~8℃ / min, and kept at this temperature for 1~3 hours before the second stage of calcination. This stage is mainly to promote the decomposition and melting of the compound of element M, improve the compatibility of element M with other elements, make the distribution of element M in the finished product more uniform, improve the uniformity of the material, and ensure the stability of the product. Otherwise, the distribution of element M in the finished product is uneven, resulting in inconsistent electrical properties of samples taken at different points in the finished product, and low product stability; or the compatibility of element M with other elements is poor, and the oxide impurities of element M in the finished product are high, resulting in poor electrical properties.

[0087] In one embodiment of the present invention, the heating rate of the second stage sintering is preferably 5~8°C / min, more preferably 6~7°C / min; the calcination temperature is preferably 440~460°C, more preferably 445~455°C, such as 440°C, 445°C, 450°C, 455°C, 460°C, preferably a range value with any of the above values ​​as the upper or lower limit; the insulation time is preferably 1~3 hours, more preferably 1~2 hours.

[0088] After the second stage of calcination is completed, the present invention heats up to 890-910°C at a heating rate of 5-8°C / min, keeps the temperature for 10-20 hours, and then performs the third stage of calcination. Calcination at this temperature and time is beneficial to avoid the formation of too many impurities during the sintering process caused by too high or too low temperature, which helps to improve the crystallinity and purity of the finished product, thereby improving the charge and discharge specific capacity.

[0089] In one embodiment of the present invention, the heating rate is preferably 5-8°C / min, more preferably 6-7°C / min; the calcination temperature is preferably 850-950°C, more preferably 860-940°C, such as 850°C, 860°C, 870°C, 880°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C, 950°C, preferably with any of the above values ​​as the upper or lower limit of the range value, the insulation time is preferably 10-20 hours, more preferably 15-16 hours.

[0090] During the entire calcination process, the water content in the high-temperature furnace is controlled to be less than 3%, the concentration of carbon dioxide is less than 1%, and the oxygen content is between 20% and 50% to avoid excessive oxygen content, which may cause excessive impurities to form during the sintering process. During the sintering process, the water content, oxygen content and carbon dioxide content in the high-temperature furnace are detected online, and the gas intake, exhaust volume, and the ratio of oxygen and nitrogen in the intake gas are adjusted in time to control the water content, oxygen content and carbon dioxide content in the high-temperature furnace within the control range.

[0091] After calcination, the product is cooled to room temperature to obtain a second powder. The product can be cooled naturally. In the present invention, the calcined product is preferably cooled to room temperature quickly, such as by quenching, to accelerate the cooling rate, which is helpful to form a product containing more Mn 3+ The metastable phase with a high sodium content between the layers is formed, thereby improving the reversible capacity of the electrode material. In the present invention, the quenching treatment is preferably performed by chilled water cooling or liquid nitrogen cooling.

[0092] After obtaining the second powder, the present invention crushes, screens and removes iron from the second powder to obtain a sodium ion layered metal oxide material. The environmental humidity of the crushing and screening is controlled to be lower than 15%. The particle size range of the obtained sodium ion layered metal oxide material is: 0.5μm<D50<12μm, D100<40μm, the content of magnetic foreign matter is lower than 150ppm, the manganese dissolution is lower than 0.5ppm, the free sodium is lower than 100ppm, and the moisture is lower than 1000ppm.

[0093] In one embodiment of the present invention, the pulverizing method is preferably a jet mill or a mechanical pulverizer; during screening, the material passes through at least two levels of screens, the mesh number of the first level screen is preferably 80~100 mesh, and the mesh number of the second level screen is preferably 120~320 mesh.

[0094] Crushing and screening can improve the uniformity of the finished product and prevent large particles in the finished product from having an adverse effect on the electrical properties; control the humidity of the crushing and screening environment below 15% to prevent the sample from absorbing water and causing material deterioration, producing impurities, and reducing electrical properties.

[0095] In one embodiment of the present invention, the process of crushing, screening and iron removal of the second powder is a continuous operation, which is connected by a pipeline and transported under negative pressure. The finished product enters the crushing equipment after degassing. Dry nitrogen is introduced into the crushing, screening and iron removal processes for protection to prevent the material from contacting water and carbon dioxide and producing impurities.

[0096] In a third aspect, the present invention provides a positive electrode plate, comprising the sodium ion layered metal oxide material described above. The present invention does not specifically limit other materials used in the positive electrode plate, such as current collectors, conductive agents, adhesives, etc., and conventional raw materials for preparing positive electrode plates commonly used in the art can be used.

[0097] In a third aspect, the present invention provides a sodium ion battery, including the positive electrode sheet described above. The present invention does not impose any special restrictions on other materials used in the sodium ion battery, such as the negative electrode, the separator, etc., and conventional raw materials for preparing sodium ion batteries commonly used in the art can be used.

[0098] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially. Example 1

[0099] The chemical formula of sodium ion layered metal oxide material is: Na 0.95 Ni 0.45 Mn 0.3 Cu 0.05 Ti 0.2 O 1.95 F 0.05 ,

[0100] According to the molar ratio of the metal elements in the chemical formula of the material, sodium carbonate, nickel oxide, manganese tetraoxide, titanium oxide, copper oxide, sodium fluoride and deionized water are put into a coarse grinder and mixed evenly. The mixing time is 2 hours and the working frequency is 30 Hz to obtain the first slurry (solid content is 25%, particle size is: D100<8.5μm);

[0101] The first slurry was ground and mixed in a sand mill by using an A / B tank cycle method for 3 hours at a sand mill speed of 1000 r / min to obtain a second slurry (particle size: D50 < 3 μm, D100 < 8 μm).

[0102] The second slurry was spray dried to obtain a first powder (particle size: D50 < 10 μm, D100 < 35 μm, moisture content 0.5%, BET 30 m2 / g);

[0103] The first powder is placed in a high-temperature furnace and calcined. The calcination temperature curve is: from room temperature to 120°C at 5°C / min, kept at this temperature for 2 hours, then to 450°C at 5°C / min, kept at this temperature for 2 hours, then to 900°C at 5°C / min, kept at this temperature for 13 hours. The atmosphere in the high-temperature furnace is a mixed gas of dry oxygen and nitrogen (with an oxygen ratio of 25%). Then, the calcined powder is quickly cooled to room temperature using chilled water to obtain a second powder.

[0104] In this sintering process, the 120℃ temperature is kept for 2 hours, mainly to reduce the water content of the first powder, to avoid excessive moisture content in the high-temperature furnace atmosphere during the subsequent rapid heating process, to avoid side reactions, and to cause excessive impurities in the finished product; the 450℃ temperature is kept for 2 hours, mainly to promote the decomposition and melting of copper oxide, to improve the compatibility of copper with other elements, to make the distribution of copper in the finished product more uniform, to improve the uniformity of the material, and to ensure the stability of the product. Otherwise, the copper element in the finished product is unevenly distributed, resulting in inconsistent electrical properties of samples taken at different points in the finished product, and low product stability; or the copper element has poor compatibility with other elements, and the copper oxide impurities in the finished product are high, resulting in poor electrical properties.

[0105] In this sintering process, the water content in the high temperature furnace is controlled to be lower than 3%, the concentration of carbon dioxide is lower than 1%, and the oxygen content is between 20% and 35%.

[0106] The second powder is crushed, screened and iron-removed to obtain a sodium ion layered metal oxide material, the humidity of the crushing and screening environment is controlled to be lower than 15%, and the particle size range of the obtained sodium ion layered metal oxide material is: D50 is 8.5 μm, D100 is 36 μm, the content of magnetic foreign matter is lower than 150 ppm, the manganese dissolution is lower than 0.5 ppm, the free sodium is lower than 100 ppm, and the water content is lower than 1000 ppm;

[0107] SEM images of sodium ion layered metal oxide materials Figure 1 As shown, the sodium ion layered metal oxide exhibits a typical layered structure, with small particles agglomerating to form large particles, and the primary particle size is 0.7~7um.

[0108] XRD patterns of sodium ion layered metal oxide materials Figure 2 As shown;

[0109] Using sodium ion layered metal oxide material as the positive electrode, a button cell was prepared. The charge and discharge curves in the range of 2-4.0V are as follows Figure 3As shown in the figure, the discharge capacity at 0.1C is 138mAh / g. Before Cu and F are not doped, the capacity retention rate of the material after 100 cycles at 1C is about 80%. After doping with F and Cu elements, compared with the undoped material, the discharge capacity at 0.1C is basically unchanged, but the capacity retention rate of the material after 100 cycles at 1C is 91.2%, an increase of about 11%, compared with the material doped with only Cu element, the capacity retention rate of 100 cycles at 1C is 85.3%, an increase of about 5%. The introduction of M element is also beneficial to improving the environmental stability of layered metal oxides. Compared with the material without M element, the discharge capacity of the material doped with M element is increased by 5%-10% when placed in the same air atmosphere for the same time.

[0110] Comparative Example 1

[0111] The sodium ion layered metal oxide material was prepared according to the method in Example 1 and a button cell was assembled. The difference was that the chemical formula of the sodium ion layered metal oxide material was Na 0.95 Ni 0.5 Mn 0.3 Ti 0.2 O2.

[0112] A button cell was prepared according to the method in Example 1, and the electrochemical performance was tested. The results showed that the discharge specific capacity at 0.1C was 135.5 mAh / g, and the capacity retention rate of the material after 100 cycles at 1C was about 80%.

[0113] Comparative Example 2

[0114] The sodium ion layered metal oxide material was prepared according to the method in Example 1 and a button cell was assembled. The difference was that the chemical formula of the sodium ion layered metal oxide material was Na 0.95 Ni 0.45 Mn 0.3 Cu 0.05 Ti 0.2 O2.

[0115] A button cell was prepared according to the method in Example 1, and the electrochemical performance was tested. The results showed that the discharge specific capacity at 0.1C was 137 mAh / g, and the capacity retention rate of the material after 100 cycles at 1C was about 85.3%.

[0116] Comparative Example 3

[0117] The sodium ion layered metal oxide material was prepared according to the method in Example 1 and a button cell was assembled. The difference was that the chemical formula of the sodium ion layered metal oxide material was Na 0.95 Ni 0.5 Mn 0.3 Ti 0.2 O 1.95 F 0.05 .

[0118] A button cell was prepared according to the method in Example 1, and the electrochemical performance was tested. The results showed that the discharge specific capacity at 0.1C was 136 mAh / g, and the capacity retention rate of the material after 100 cycles at 1C was about 82.4%.

[0119] Comparative Example 4

[0120] A sodium ion layered metal oxide material was prepared and a button cell was assembled according to the method in Example 1, except that there was no first stage heating process, and the temperature was directly increased to 450°C at 5°C / min, kept warm for 3 hours, and then increased to 900°C at 5°C / min, and kept warm for 13 hours.

[0121] A button cell was prepared according to the method in Example 1 and electrochemical performance was tested. The results showed that the discharge specific capacity in the 2-4.0 V charge and discharge range was 125 mAh / g.

[0122] Comparative Example 5

[0123] The sodium ion layered metal oxide material was prepared and the button cell was assembled according to the method in Example 1. The difference was that there was no first stage heating process. The temperature was directly increased to 900°C at 5°C / min and kept for 13 hours. The discharge specific capacity in the 2-4.0V charge and discharge range was 121mAh / g. Example 2

[0124] The chemical formula of sodium ion layered metal oxide material is: NaNi 0.48 Mn 0.4 Y 0.02 Ti 0.1 O 1.999 F 0.001 ,

[0125] According to the molar ratio of the metal elements in the chemical formula of the material, sodium bicarbonate, nickel oxide, manganese tetraoxide, titanium oxide, sodium fluoride, yttrium oxide and a certain amount of deionized water are put into a coarse grinder and mixed evenly. The mixing time is 2 hours and the working frequency is 30 Hz to obtain the first slurry (solid content is 30%, particle size is: D100<7μm);

[0126] The first slurry was ground and mixed in a sand mill by using an A / B tank circulation method for 3 hours at a sand mill speed of 1000 r / min to obtain a second slurry (particle size: D50 < 2 μm, D100 < 7 μm).

[0127] The second slurry was spray dried to obtain a first powder (particle size: 3μm<D50<10μm, D100<30μm, moisture content less than 1%, BET of 30m 2 / g);

[0128] The first powder is placed in a high temperature furnace for calcination, and the calcination temperature curve is: from room temperature to 120°C at 4°C / min, and kept at this temperature for 2 hours, then to 455°C at 6°C / min, and kept at this temperature for 2 hours, then to 850°C at 7°C / min, and kept at this temperature for 20 hours, and then the calcined material is rapidly cooled, and the rapid cooling method can be liquid nitrogen cooling or chilled water cooling;

[0129] In this sintering process, the temperature is kept at 120℃ for 2h, mainly to reduce the moisture content of the first powder, to avoid excessive moisture content in the high-temperature furnace atmosphere during the subsequent rapid heating process, to avoid side reactions, and to cause excessive impurities in the finished product; the maximum sintering temperature is 850℃, which can improve the compatibility of Y with other elements, making the distribution of Y elements in the finished product more uniform, improving the uniformity of the material, and ensuring the stability of the product. Otherwise, the Y element is unevenly distributed in the finished product, resulting in inconsistent electrical properties of samples taken at different points in the finished product, and poor consistency of the final product. In addition, the sintering temperature of 850℃ can prevent the primary particles of the finished product from being too large, resulting in reduced electrical properties.

[0130] In this sintering process, the water content in the high temperature furnace is controlled to be lower than 2%, the concentration of carbon dioxide is lower than 1%, and the oxygen content is between 20% and 50%.

[0131] The second powder is crushed, screened and iron-removed to obtain a sodium ion layered metal oxide material, and the environmental humidity of the crushing and screening is controlled to be lower than 10%. The particle size range of the obtained sodium ion layered metal oxide material is: 2μm<D50<10μm, 25μm<D100<35μm, the content of magnetic foreign matter is lower than 150ppm, the manganese dissolution is lower than 0.5ppm, the free sodium is lower than 100ppm, and the moisture is lower than 1000ppm.

[0132] SEM images of sodium ion layered metal oxide materials Figure 5 As shown, the sodium ion layered metal oxide exhibits a typical layered structure, with small particles agglomerating to form large particles, and the primary particle size is 0.2~4.5μm.

[0133] Using sodium ion layered metal oxide material as the positive electrode, a button cell was prepared. The charge and discharge curves in the range of 2-4.0V are as follows Figure 4 As shown, the discharge capacity at 0.1C is 135 mAh / g, and the capacity retention rate after 100 cycles at 1C is about 85.2%. 0.5 Mn 0.4 Ti 0.1O2), the capacity retention rate of the material after 100 cycles of 1C is about 80%, and the discharge specific capacity at 0.1C is 135.5mAh / g. After doping with Y and F elements, the discharge specific capacity at 0.1C is slightly reduced compared to that of undoped materials, but the capacity retention rate of the material after 100 cycles of 1C is increased by about 5%. After Y doping, the layered metal oxide material has a strong YO bond, forming a stable structure, and the material is surrounded by a Y2O3 protective layer. The expanded Na layer also causes Na ions to be inserted not only into the surface but also into the body. Therefore, the cycle performance of the material is improved after Y doping the material. In addition, yttrium oxide does not decompose or melt at 850°C, which is equivalent to introducing a small amount of impurity phase, but the amount of yttrium oxide added in this product is small and will not have a negative impact on the electrical properties. Example 3

[0134] The chemical formula of sodium ion layered metal oxide material is: Na 0.9 Ni 0.48 Mn 0.39 Cu 0.02 Mg 0.01 Ti 0.1 O2,

[0135] According to the molar ratio of the metal elements in the chemical formula of the material, sodium carbonate, nickel hydroxide, manganese dioxide, titanium oxide and alcohol are put into a coarse grinder and mixed evenly. The mixing time is 2 hours and the working frequency is 30 Hz to obtain the first slurry (solid content is 20%, particle size is: D100<10μm);

[0136] The first slurry was ground and mixed in a sand mill by using an A / B tank circulation method for 3 hours. The sand mill was turned at 1000r / min to obtain a second slurry (particle size: D50<3μm, D100<10μm).

[0137] The second slurry was spray dried to obtain a first powder (particle size: 3μm<D50<8μm, D100<35μm, moisture content less than 1%, BET of 30m 2 / g);

[0138] The first powder is placed in a high-temperature furnace for calcination, and the calcination temperature curve is: from room temperature to 120°C at 4°C / min, and kept warm for 3 hours, then increased to 450°C at 7°C / min, and kept warm for 1 hour, and then increased to 950°C at 8°C / min, and kept warm for 15 hours, and the atmosphere in the high-temperature furnace is dry oxygen, and then quickly cooled to room temperature to obtain a second powder, and the rapid cooling method can be liquid nitrogen cooling or chilled water cooling;

[0139] In this sintering process, the 120℃ temperature is kept for 3 hours, mainly to reduce the water content of the first powder, to avoid excessive moisture content in the high-temperature furnace atmosphere during the subsequent rapid heating process, to avoid side reactions, and to cause excessive impurities in the finished product; the 450℃ temperature is kept for 3 hours, mainly to promote the decomposition and melting of copper oxide, to improve the compatibility of copper with other elements, to make the distribution of copper in the finished product more uniform, to improve the uniformity of the material, and to ensure the stability of the product. Otherwise, the copper element in the finished product is unevenly distributed, resulting in inconsistent electrical properties of samples taken at different points in the finished product, and low product stability; or the copper element has poor compatibility with other elements, and the copper oxide impurities in the finished product are high, resulting in poor electrical properties.

[0140] In this sintering process, the water content in the high-temperature furnace is controlled to be less than 2%, and the concentration of carbon dioxide is controlled to be less than 1%. The water and carbon dioxide content in the high-temperature furnace are detected online during the sintering process, and the gas intake and exhaust volume are adjusted in time to control the water and carbon dioxide content in the high-temperature furnace within the control range.

[0141] The second powder is crushed, screened and iron-removed to obtain a sodium ion layered metal oxide material, and the environmental humidity of the crushing and screening is controlled to be lower than 10%. The particle size range of the obtained sodium ion layered metal oxide material is: 3μm<D50<10μm, 25μm<D100<40μm, the content of magnetic foreign matter is lower than 150ppm, the manganese dissolution is lower than 0.5ppm, the free sodium is lower than 100ppm, and the moisture is lower than 1000ppm.

[0142] SEM images of sodium ion layered metal oxide materials Figure 7 As shown, the sodium ion layered metal oxide exhibits a typical layered structure, with small particles agglomerating to form large particles, and the primary particle size is 0.5-5um.

[0143] The chemical formula is Na 0.9 Ni 0.48 Mn 0.39 Cu 0.02 Mg 0.01 Ti 0.1 The sodium ion layered metal oxide material of O2 was used as the positive electrode to prepare the button battery. The charge and discharge curves in the range of 2-4.0V are as follows Figure 6As shown, the discharge capacity at 0.1C is 129mAh / g, and the capacity retention rate after 100 cycles at 1C is 92.1%. Before Cu and Mg are not doped (i.e., Na0.9Ni0.5Mn0.4Ti0.1O2), the capacity retention rate after 100 cycles at 1C is about 80%, and the discharge capacity at 0.1C is 135.5mAh / g. After doping with Cu and Mg elements, the discharge capacity at 0.1C is reduced compared with that of undoped materials, but the capacity retention rate after 100 cycles at 1C is increased by about 12%. Doping Mg on the basis of doping Cu elements is equivalent to replacing trivalent manganese ions with divalent magnesium ions, which can increase the interlayer spacing, thereby promoting the diffusion of sodium ions, and can also reduce the lattice strain caused by the sodium ion insertion and extraction process to enhance the stability of the layered structure; in addition, doping with divalent magnesium ions can reduce the structural deformation or volume change caused by the charge and discharge cycle of sodium ion batteries, inhibit irreversible phase changes, and have an important impact on improving the reversible capacity of the material. In addition, Mg in this material is non-electrochemically active and does not participate in the redox reaction, but the amount of magnesium oxide added in this product is small and will not have a negative impact on the electrical properties.

[0144] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A sodium ion layered metal oxide material, wherein the sodium ion layered metal oxide material is an O3 type manganese-based layered oxide material; the sodium ion layered metal oxide material is Na 0.95 Ni 0.45 Mn 0.3 Cu 0.05 Ti 0.2 O 1.95 F 0.05 ,NaNi 0.48 Mn 0.4 Y 0.02 Ti 0.1 O 1.999 F 0.001 and Na 0.9 Ni 0.48 Mn 0.39 Cu 0.02 Mg 0.01 Ti 0.1 One or more of O2; The method for preparing the sodium ion layered metal oxide material comprises the following steps: A) mixing a Na source, a Ni source, a Mn source, a Ti source, a M source and a F source with a solvent in a stoichiometric ratio and then coarsely grinding the mixture to obtain a first slurry; B) grinding the first slurry to obtain a second slurry; C) spray drying the second slurry to obtain a first powder; D) calcining the powder according to the following procedure to obtain a second powder, In an oxygen-containing atmosphere, heat from room temperature to 110-130°C at a heating rate of 3-5°C / min, keep warm for 2-4 hours, then heat to 440-460°C at a heating rate of 5-8°C / min, keep warm for 1-3 hours, then heat to 850-950°C at a heating rate of 5-8°C / min, keep warm for 10-20 hours; E) crushing, screening and removing iron from the second powder to obtain the sodium ion layered metal oxide material.

2. The method for preparing the sodium ion layered metal oxide material according to claim 1, comprising the following steps: A) mixing a Na source, a Ni source, a Mn source, a Ti source, a M source and a F source with a solvent in a stoichiometric ratio and then coarsely grinding the mixture to obtain a first slurry; B) grinding the first slurry to obtain a second slurry; C) spray drying the second slurry to obtain a first powder; D) calcining the powder according to the following procedure to obtain a second powder, In an oxygen-containing atmosphere, heat from room temperature to 110-130°C at a heating rate of 3-5°C / min, keep warm for 2-4 hours, then heat to 440-460°C at a heating rate of 5-8°C / min, keep warm for 1-3 hours, then heat to 850-950°C at a heating rate of 5-8°C / min, keep warm for 10-20 hours; E) crushing, screening and removing iron from the second powder to obtain a sodium ion layered metal oxide material.

3. The preparation method according to claim 2, characterized in that: The solvent used for the coarse grinding in step A) is water and / or alcohol, the solid content of the first slurry is 10-40%, and the particle size of the first slurry is D100<10 μm.

4. The preparation method according to claim 2, characterized in that: The calcination procedure is specifically as follows: In an oxygen-containing atmosphere, heat from room temperature to 120-125°C at a heating rate of 4-5°C / min, keep warm for 2-3 hours, then heat to 450-455°C at a heating rate of 5-7°C / min, keep warm for 1-2 hours, then heat to 850-950°C at a heating rate of 5-8°C / min, and keep warm for 13-20 hours.

5. The preparation method according to claim 2, characterized in that: During the calcination process, the oxygen content is 20-35%, the moisture content is less than 3%, and the carbon dioxide concentration is less than 1%.

6. The preparation method according to claim 2, characterized in that: After the calcination is completed, rapid cooling is performed to obtain a second powder; The rapid cooling is a quenching treatment.

7. A positive electrode sheet, characterized in that: The invention comprises the sodium ion layered metal oxide material according to claim 1 or the sodium ion layered metal oxide material prepared by the preparation method according to any one of claims 2 to 6.

8. A sodium ion battery, characterized in that: Including the positive electrode sheet as described in claim 7.