A method for preparing nylon 10 from 10-aminodecanoic acid

By using a multi-stage controlled polymerization reaction and a spiral agitator design, the problem of molecular weight control in the preparation of nylon 10 was solved, resulting in high-performance, environmentally friendly nylon 10 resin, and achieving molecular weight uniformity and material uniformity.

CN117757059BActive Publication Date: 2026-11-10WUXI YINDA NYLON
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311845995.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2026-11-10
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

There is a lack of effective methods for preparing nylon 10 in the existing technology, and the use of organic solvents in traditional methods leads to safety risks and performance impacts, making it difficult to control the molecular weight distribution and material uniformity of nylon 10 during the reaction process.

Method used

Using 10-aminodecanoic acid as raw material, combined with molecular weight regulators, catalysts and antioxidants, a multi-stage controlled polymerization reaction is carried out under specific pressure and temperature conditions. Inert gas is used to regulate pressure and moisture to control molecular weight growth. A ribbon agitator is used to prevent wall adhesion and agglomeration. Water is used as an environmentally friendly solvent.

Benefits of technology

The process achieved a uniform molecular weight distribution of nylon 10, avoiding material charring and agglomeration, resulting in high-performance nylon 10 resin that meets green production standards, exhibits a normal molecular weight distribution, and has a good resin appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117757059B_ABST
    Figure CN117757059B_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing nylon 10 from 10-aminodecanoic acid, comprising the following steps: adding 10-aminodecanoic acid, a molecular weight regulator, a catalyst, an antioxidant, and deionized water to a reactor in a specified ratio; heating and pressurizing the reactor to carry out a condensation reaction under nitrogen purging; specifically, the process includes five steps, which can be summarized as pressurized and maintained polymerization, secondary depressurization and dehydration, secondary molecular homogenization, and monitoring by instruments; and polymerizing to obtain nylon 10 resin with a uniform molecular weight distribution; and then extruding, stretching, cooling, and pelletizing to obtain nylon 10 particles. The preparation method of this invention can effectively control the polymerization rate of nylon 10 resin, resulting in nylon 10 resin with a uniform molecular weight distribution and good viscosity consistency, suitable for both large-scale and small-batch production, and offering flexible and convenient operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer technology, specifically relating to a method for preparing nylon 10 from 10-aminodecanoic acid. Background Technology

[0002] Nylon is a general term for polymers whose main molecular chain repeating units contain amide groups. Long-chain nylons typically refer to nylons with methylene groups longer than 10 carbons in their chain segments, including nylon 11, nylon 12, nylon 1010, and nylon 1012. From the molecular structure of long-chain nylon resins, the methylene groups in the molecular chain are longer, and the amide group density is lower. Therefore, in addition to the general properties of nylon (such as lubricity, wear resistance, pressure resistance, and ease of processing), long-chain nylons also possess properties that conventional nylons do not have, such as higher toughness, flexibility, low water absorption, and dimensional stability.

[0003] Long-chain nylons can be classified into AB-type single-number nylons and AABB-type double-number nylons according to the different polymer monomers. Among the AB-type long-chain single-number nylons, Nylon 11 and Nylon 12 are industrially produced; there are no other single-number nylons. It is worth noting that Nylon 10, as a type of long-chain AB-type nylon, not only possesses the high toughness and low water absorption characteristics of long-chain nylons, but also exhibits excellent physical, mechanical, and chemical properties. This is because, compared to Nylon 11 and Nylon 12, its methylene group length is shorter and its amide group density is relatively higher, resulting in superior tensile strength and other mechanical properties. Therefore, it is a new long-chain nylon material with better overall performance.

[0004] Because there is currently no engineered method for preparing the monomer (10-aminodecanoic acid) of nylon 10, there are no nylon 10 products available on the market.

[0005] The applicant has proposed a method for preparing 10-aminodecanoic acid in the inventions with application numbers 2023117592392 and 2023117798770; therefore, it is necessary to develop a process for preparing nylon 10 from 10-aminodecanoic acid.

[0006] The polymerization mechanism of Nylon 10 is similar to that of Nylon 11, but the polymerization rate constant is different.

[0007] Nylon 11 is produced by the dehydration condensation of 11-aminoundecanoic acid upon heating. Industrially, the production of nylon 11 is difficult to control. The monomer 11-aminoundecanoic acid is poorly soluble in water and cannot be treated as an aqueous solution like ε-caprolactam. Furthermore, its melting point is 187°C, and it becomes viscous after melting. When heated to its melting point, dehydration and condensation begin. This phase transition from solid to molten state is accompanied by a condensation reaction. Therefore, if the control methods are not properly implemented, phenomena such as coking, nodules, and agglomeration frequently occur, making it impossible to produce qualified nylon 11 resin.

[0008] The carbon chain of 10-aminodecanoic acid is shorter than that of 11-aminoundecanoic acid, resulting in a faster reaction rate and making the process more difficult to control than that of nylon 11. During the depressurization process of venting water vapor, the polymerization rate of nylon 10 increases as the moisture content in the system decreases. If not properly controlled, this can lead to a wider molecular weight distribution of nylon 10 in the reactor, affecting product performance. More seriously, it may cause uneven material viscosity, or even lead to sticking to the reactor walls, nodules, and coking.

[0009] In addition, invention patent CN 103709399 B discloses a process for preparing nylon 11 by atmospheric pressure melt polymerization of 11-aminoundecanoic acid. The process involves mixing 11-aminoundecanoic acid with a flux, wherein the flux is one or more organic solvents with boiling points of 185–220°C in any proportion; under atmospheric pressure, the material is heated to melt, and then further heated to 230–270°C to evaporate the flux and the water generated in the reaction; after the atmospheric pressure melt reaction is completed, the temperature is maintained at 230–270°C, and then a vacuum is drawn for a vacuum reaction; after the vacuum reaction is completed, the vacuum is stopped, atmospheric pressure is restored, and nylon 11 is obtained by discharging the material.

[0010] This method uses organic solvents as co-solvents, which brings many problems in actual industrial production. Large amounts of organic solvents need to be recycled, and there are certain safety risks. Residual organic solvents in the product will also affect the product's performance and use. Summary of the Invention

[0011] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a method for preparing nylon 10 from 10-aminodecanoic acid. This method can effectively control the molecular weight growth rate of nylon 10 during the reaction process, resulting in nylon 10 with a uniform molecular weight distribution and good normality.

[0012] To achieve the above technical objectives, the technical solution adopted in this embodiment of the invention is: a method for preparing nylon 10 from 10-aminodecanoic acid, comprising the following steps: (1) Add 10-aminodecanoic acid, molecular weight regulator, catalyst, antioxidant and deionized water to the reactor, replace the gas in the reactor repeatedly with inert gas, raise the temperature to 180-210℃ and the pressure to 1.0-2.0MPa, and at the same time start the reactor to stir and continuously discharge water vapor to maintain the pressure of 1.0-2.0MPa. Under constant pressure, react for 2-5 hours. (2) Increase the exhaust volume appropriately, reduce the pressure of the reactor to 0.5-0.7MPa, and at the same time raise the reactor temperature to 210-230℃, and control the exhaust time to 2-4 hours; (3) Stop venting, introduce inert gas into the reactor to raise the reactor pressure to 1.0-1.2 MPa, then vent the gas to reduce the reactor pressure to 0.4-0.5 MPa, while maintaining the reactor temperature at 220-230℃, and control the venting time to 1-3 hours; (4) Stop venting, introduce inert gas into the reactor to raise the reactor pressure to 0.8-1.0 MPa, then vent, and reduce the reactor pressure to 0.2-0.3 MPa within 2-3 hours, while raising the reactor temperature to 225-235℃; depending on the product viscosity requirements, this process can be repeated 1-2 times. (5) Continue to introduce inert gas into the reactor to maintain the reactor pressure at 0.05-0.1MPa and the temperature at 230-235℃. Continue the reaction and monitor the change of the reactor stirring current. When the current reaches or approaches the set value, the reaction ends. After extrusion, stripping, cooling and pelletizing, nylon 10 resin particles are obtained.

[0013] Specifically, a ribbon agitator is installed inside the reactor in step (1), and the edge of the ribbon agitator is 2-5 mm away from the reactor wall. Because 10-aminodecanoic acid monomer is easy to polymerize and reacts quickly, the requirements for heat and mass transfer in the reactor are very high, so a specially designed agitator is used.

[0014] Specifically, the ribbon stirrer in step (1) is equipped with a current load display instrument, which is used to indirectly detect the molecular weight of the polymer, especially in the later stage of polymerization, where it can intuitively reflect the viscosity change.

[0015] Specifically, in step (1), the formula, by mass fraction, is: 100 parts of 10-aminodecanoic acid, 0.1-10 parts of molecular weight regulator, 0.01-0.1 parts of catalyst, 0.02-0.2 parts of antioxidant and 100-500 parts of deionized water.

[0016] Specifically, in step (1), the molecular weight regulator is a dicarboxylic acid including adipic acid, sebacic acid, and dodecanoic acid.

[0017] Specifically, in step (1), the catalyst is a phosphorus-based compound, using one or more of phosphoric acid, phosphorous acid, sodium phosphite, sodium hypophosphite, and pyrophosphite.

[0018] Sodium hypophosphite is preferred because it not only has a catalytic effect but also excellent anti-discoloration properties. The addition amount is 0.01-0.1 parts, preferably 0.02-0.08 parts by mass. This is because a catalyst can both accelerate the reaction and, under certain conditions, promote molecular hydrolysis.

[0019] Specifically, in step (1), the antioxidant is one or more of antioxidants 1010, 1070, 1076, 1098, 2246, 245 and 330, preferably one or more of antioxidants 1098, 2246 and 330; the amount of antioxidant added is 0.02-0.2 parts by mass, preferably 0.04-0.1 parts, because hindered phenolic antioxidants and antioxidants with different molecular structures have different temperature resistance and antioxidant effects.

[0020] Specifically, in step (1), the amount of deionized water added is 100-500 parts by mass, preferably 200-400 parts; because water not only acts as a solvent, but also plays a role in heat conduction and mass transfer enhancement. Only by maintaining an appropriate water content can the stirring operate normally (the polymerization system in the early stage is a slurry) and achieve the best effect; more importantly, the water content (in the later stage of polymerization) plays a balancing and inhibiting role on the size of polymer molecules, and the residual amount of water in the reactor corresponds to the molecular weight balance range of the polymer.

[0021] Specifically, in step (2), the pressure of the reactor is reduced to 0.5-0.7 MPa, while the reactor temperature is increased to 210-230℃. This step is the first stage of the depressurization reaction, with a large exhaust volume and an exhaust time of 2-4 hours, preferably 2-3 hours. At this time, the viscosity of Nylon 10 molecules is low, heat and mass transfer is good, the system has good fluidity, and it is approximately a homogeneous system.

[0022] Specifically, in step (3), the venting is interrupted, and inert gas is introduced into the reactor, raising the pressure to 1.0-1.2 MPa. Then, the pressure is reduced to 0.4-0.5 MPa, and the reactor temperature is maintained at 220-230℃. This step is the second stage of the depressurization reaction. At this time, the drainage rate must be controlled to prevent the molecular weight from increasing too quickly. Nitrogen is introduced to increase the pressure, and then the gas is slowly vented. The venting time is 1-3 hours. The advantage of introducing inert gas is that it reduces the partial pressure of water vapor in the reactor. The higher pressure is because, under the corresponding temperature conditions, the evaporation of water in the reactor is inhibited, and the homogenization and consistency of molecules are guaranteed.

[0023] Specifically, in step (4), the venting is interrupted, and inert gas is introduced into the reactor to raise the reactor pressure to 0.8-1.0 MPa. Then, the venting is stopped, and the pressure drops to 0.2-0.3 MPa within 2-3 hours. At the same time, the reactor temperature rises to 230-235℃. This step is the first stage of molecular homogenization. By using inert gas to increase the pressure, only a small amount of moisture is removed, allowing the polymer molecules to be fully balanced and uniform, and to remain for a relatively long time. If there are special requirements for the product viscosity, this process can be repeated 1-2 times.

[0024] Specifically, in step (5), inert gas is continuously introduced into the reactor to maintain the reactor pressure at 0.05-0.1 MPa and the temperature at 230-235 °C, and the reaction continues. This step is the second stage of molecular homogenization. The system is still under positive pressure to prevent oxygen depletion and ensure the appearance of the resin. On the other hand, it prevents a small amount of water from evaporating in a short period of time and ensures that the molecular weight grows in a balanced manner until the end of the reaction. At this time, the change of the stirring current of the reactor should be monitored. When the current reaches or approaches the set value, the reaction ends.

[0025] Compared with the prior art, the beneficial effects of the technical solution provided by the embodiments of the present invention are as follows: 1) Adding a large amount of water to the reaction system improves the heat and mass transfer conditions in the early stage of the reaction and inhibits the reaction in the middle and late stages, preventing material coking, decomposition, nodulation, and agglomeration.

[0026] 2) The reactor is stirred using a ribbon agitator. The ribbon can scrape the wall to prevent material from sticking to the heat transfer surface and ensure the uniformity of the resin molecular weight.

[0027] 3) During the depressurization stage in the later stage of the reaction, as water is discharged, the molecular weight of Nylon 10 increases rapidly. By repeatedly introducing inert gas into the reactor and then depressurizing, the pressure of the inert gas is used to suppress the evaporation of water in the system material, control the growth rate of Nylon 10 molecular weight, and avoid the problem of excessively rapid molecular weight growth leading to deterioration of heat and mass transfer conditions in the reaction system and poor uniformity of materials in the reactor.

[0028] 4) Add phosphorus compounds as catalysts to the reaction, preferably sodium hypophosphite: because it not only has catalytic activity, but also excellent anti-color change effect; at the same time, because the catalyst can both accelerate the reaction and promote molecular hydrolysis, it can effectively promote the balanced growth of polymer molecules as long as moisture is present.

[0029] 5) This invention uses water as a solvent, which is both safe and environmentally friendly. The vapor can be recycled after condensation. Compared with preparation processes that require a large amount of organic solvents, the preparation method of this invention is a more modern and green production process.

[0030] 6) This invention uses a positive pressure reaction process, resulting in uniform and well-normal molecular distribution; the entire process is protected by inert gas, and the resulting nylon 10 resin chips are transparent and have a good appearance.

[0031] 7) This invention produces Nylon 10 resin from 10-aminodecanoic acid, which is the first of its kind in China and enriches the new varieties of the nylon family.

[0032] 8) The process method adopted in this invention can be used for both large-scale production and small-batch production, and is flexible and convenient to operate. Attached Figure Description

[0033] Figure 1 This is a molecular weight distribution diagram of nylon 10 obtained in Example 1 of the present invention.

[0034] Figure 2 This is a molecular weight distribution diagram of nylon 10 obtained in Example 2 of the present invention.

[0035] Figure 3 This is a molecular weight distribution diagram of nylon 10 prepared in Comparative Example 1 of this invention.

[0036] Figure 4 This is a molecular weight distribution diagram of nylon 10 prepared in Comparative Example 2 of this invention.

[0037] in Figure 1-4 The vertical axis of the molecular weight distribution graph represents the signal intensity of the GPC concentration detector, in Mv; the horizontal axis represents the time it takes for nylon 10 resin molecules to flow through the chromatographic column, in min. Detailed Implementation

[0038] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0039] The evaluation method used in the examples is as follows: 1) Relative viscosity Accurately weigh 0.25 g of sample and add it to 25 mL of m-cresol. Stir and dissolve at 20-30 °C. After complete dissolution, place the solution in an Ubbelohde viscometer and incubate at 25 °C for 10 minutes. Measure the descent rate (t). Also measure the descent rate (t0) of m-cresol in the same manner. Calculate the relative viscosity from t and t0 using the following formula: Relative viscosity = t / t0.

[0040] 2) The weight-average molecular weight and distribution curve of the resin were determined using gel permeation chromatography (GPC). A standard elution curve was prepared using methyl methacrylate (PMMA) as a standard sample, and the molecular weight distribution of the polymer was characterized by GPC using hexafluoroisopropanol containing 0.01 mol / L sodium trifluoroacetate as a solvent.

[0041] 3) Tensile strength Melted in an injection molding machine at 230°C, with an injection pressure of 600 kgf / cm². 2Injection-molded sheets were obtained under the conditions of 1.0 second injection time and 40℃ mold temperature. The obtained injection-molded sheets were annealed at 25℃ for 24 hours and then tested under absolutely dry conditions. Tensile strength and elongation at break were determined according to GB / T 1040.1-2018 Determination of tensile properties of plastics.

[0042] 4) b value A certain amount of Nylon 10 particles were taken, and the b-value of the particles was measured using a CR-400 / 410 colorimeter.

[0043] Example 1 A method for preparing nylon 10 from 10-aminodecanoic acid includes the following steps: (1) Add 2000 kg of 10-aminodecanoic acid, 10.8 kg of sebacic acid, 4500 kg of deionized water, 0.6 kg of phosphorous acid catalyst, and 1.2 kg of antioxidant 1098 to the reactor in sequence. Under nitrogen protection, start stirring and heat to 200℃. After the reactor pressure reaches 1.5 MPa, open the exhaust valve and continuously discharge water vapor to maintain the reactor pressure at 1.5 MPa. React for 4 hours. (2) Increase the exhaust volume appropriately, reduce the pressure of the reactor to 0.6 MPa within 3 hours, and raise the temperature of the reactor to 225°C; (3) Stop venting, introduce nitrogen into the reactor to make the reactor pressure reach 1.0 MPa, then open the vent valve and reduce the reactor pressure to 0.5 MPa within 2 hours, while maintaining the reactor temperature at 230℃. (4) Stop venting, introduce nitrogen into the reactor to make the reactor pressure reach 0.8MPa, then open the vent valve and reduce the reactor pressure to 0.25MPa within 2.5 hours, while raising the reactor temperature to 235℃; (5) Continue to introduce nitrogen into the reactor to maintain the reactor pressure at 0.1 MPa and the reactor temperature at 235°C. Continuously monitor the stirring current. After the reaction continues for 3 hours, the stirring current reaches 101A (set current 95-100A). The reaction ends. After extrusion, stripping, cooling and pelletizing, nylon 10 resin particles are obtained.

[0044] Example 2 A method for preparing nylon 10 from 10-aminodecanoic acid includes the following steps: (1) Add 2000 kg of 10-aminodecanoic acid, 19.4 kg of sebacic acid, 5000 kg of deionized water, 0.6 kg of phosphorous acid catalyst, and 1.2 kg of antioxidant 1098 to the reactor in sequence. Under nitrogen protection, start stirring and heat to 205℃. After the reactor pressure reaches 1.7 MPa, open the exhaust valve and continuously discharge water vapor to maintain the reactor pressure at 1.8 MPa. React for 3 hours. (2) Increase the exhaust volume appropriately, reduce the pressure of the reactor to 0.5 MPa within 2.5 hours, and raise the temperature of the reactor to 228°C; (3) Stop venting, introduce nitrogen into the reactor to make the reactor pressure reach 1.1 MPa, then open the vent valve and reduce the reactor pressure to 0.4 MPa in 2 hours, while maintaining the reactor temperature at 230℃; (4) Stop venting, introduce nitrogen into the reactor to make the reactor pressure reach 0.9MPa, then open the vent valve and reduce the reactor pressure to 0.2MPa in 2 hours, while raising the reactor temperature to 235℃. (5) Continue to introduce nitrogen into the reactor to maintain the reactor pressure at 0.1 MPa and the reactor temperature at 235°C. Continuously monitor the stirring current. After the reaction continues for 3 hours, the stirring current reaches 96A (set current 95-100A). The reaction ends. After extrusion, stripping, cooling and pelletizing, nylon 10 resin particles are obtained.

[0045] Comparative Example 1 A method for preparing nylon 10 from 10-aminodecanoic acid includes the following steps: (1) Add 2000 kg of 10-aminodecanoic acid, 10.8 kg of sebacic acid, 4000 kg of deionized water, 0.6 kg of phosphorous acid catalyst, and 1.2 kg of antioxidant 1098 to the reactor in sequence. Under nitrogen protection, start stirring and heat to 200℃. After the reactor pressure reaches 1.5 MPa, open the exhaust valve and continuously discharge water vapor to maintain the reactor pressure at 1.5 MPa. React for 4 hours. (2) Increase the opening of the exhaust valve and increase the exhaust volume. Adjust the exhaust volume to reduce the pressure of the reactor to atmospheric pressure within 7 hours. During the pressure reduction process, continuously monitor the stirring current. When the pressure drops to 0.1 MPa, the stirring current has reached 99A (set current 95-100A). End the reaction. After extrusion, stripping, cooling and pelletizing, nylon 10 resin particles are obtained.

[0046] Comparative Example 2 A method for preparing nylon 10 from 10-aminodecanoic acid includes the following steps: (1) Add 2000 kg of 10-aminodecanoic acid, 19.4 kg of sebacic acid, 4000 kg of deionized water, 0.6 kg of phosphorous acid catalyst and 1.2 kg of antioxidant 1098 to the reactor in sequence. Under nitrogen protection, start stirring and heat to 200℃. After the reactor pressure reaches 1.5 MPa, open the exhaust valve and continuously discharge water vapor to maintain the reactor pressure at 1.5 MPa. React for 4 hours. (2) Increase the opening of the exhaust valve and increase the exhaust volume. Adjust the exhaust volume to reduce the pressure of the reactor to atmospheric pressure within 7 hours. During the pressure reduction process, continuously monitor the stirring current. When the pressure drops to atmospheric pressure, the stirring current reaches 70A. Continue the reaction for 2 hours until the stirring current reaches 95A (set current 95-100A). End the reaction. After extrusion, strip drawing, cooling and pelletizing, nylon 10 resin particles are obtained.

[0047] In step (1) of Examples 1-2 and Comparative Examples 1-2, a ribbon agitator is installed inside the reactor, and the distance between the edge of the ribbon agitator and the reactor wall is 2-5 mm. The ribbon agitator is equipped with a current load display instrument, which can indirectly detect the molecular weight of the polymer, especially in the later stage of polymerization, it can intuitively reflect the viscosity change.

[0048] The performance parameters of the nylon 10 resin particles prepared in Examples 1-2 and Comparative Examples 1-2 are listed in Table 1.

[0049] Table 1. Performance parameters of nylon 10 resin particles in Examples 1-2 and Comparative Examples 1-2

[0050] The nylon 10 resins obtained in Examples 1-2 have good viscosity consistency, and the molecular weight distribution of nylon 10 with different viscosities is basically the same. The normal distribution of molecular weight is narrower, and the mechanical properties and b-value are better than those of Comparative Examples 1-2.

[0051] 1) In Comparative Example 1, the reaction rate during polymerization was too fast, resulting in poor viscosity consistency and a wide molecular weight distribution, which affected the mechanical properties of the product.

[0052] 2) By increasing the amount of molecular weight regulator, the target molecular weight of nylon 10 is reduced. The viscosity consistency of the nylon 10 product obtained by polymerization in Comparative Example 2 is better than that in Comparative Example 1, but there is still a large gap compared with Examples 1-2.

[0053] Finally, it should be noted that the above specific embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A method for preparing nylon 10 from 10-aminodecanoic acid, characterized in that, Includes the following steps: (1) Add 10-aminodecanoic acid, molecular weight regulator, catalyst, antioxidant and deionized water to the reactor, replace the gas in the reactor repeatedly with inert gas, raise the temperature to 180-210℃ and the pressure to 1.0-2.0MPa, and at the same time start the reactor to stir and continuously discharge water vapor to maintain the pressure of 1.0-2.0MPa. Under constant pressure, react for 2-5 hours. (2) Increase the exhaust volume appropriately, reduce the pressure of the reactor to 0.5-0.7MPa, and at the same time raise the reactor temperature to 210-230℃, and control the exhaust time to 2-4 hours; (3) Stop venting, introduce inert gas into the reactor to raise the reactor pressure to 1.0-1.2 MPa, then vent the gas to reduce the reactor pressure to 0.4-0.5 MPa, while maintaining the reactor temperature at 220-230℃, and control the venting time to 1-3 hours; (4) Stop venting, introduce inert gas into the reactor to raise the reactor pressure to 0.8-1.0 MPa, then vent, and reduce the reactor pressure to 0.2-0.3 MPa within 2-3 hours, while raising the reactor temperature to 225-235℃; (5) Continue to introduce inert gas into the reactor to maintain the reactor pressure at 0.05-0.1MPa and the temperature at 230-235℃, continue the reaction, monitor the change of the reactor stirring current, and when the current reaches or approaches the set value, end the reaction. After extrusion, stripping, cooling and pelletizing, nylon 10 resin particles are obtained. In step (1), a ribbon agitator is installed inside the reactor, and the edge of the ribbon agitator is 2-5 mm away from the reactor wall.

2. The method for preparing nylon 10 from 10-aminodecanoic acid according to claim 1, characterized in that, The ribbon agitator described in step (1) is equipped with a current load display instrument.

3. The method for preparing nylon 10 from 10-aminodecanoic acid according to claim 1, characterized in that, In step (1), the formula is as follows by mass: 100 parts of 10-aminodecanoic acid, 0.1-10 parts of molecular weight regulator, 0.01-0.1 parts of catalyst, 0.02-0.2 parts of antioxidant and 100-500 parts of deionized water.

4. The method for preparing nylon 10 from 10-aminodecanoic acid according to claim 1, characterized in that, In step (1), the molecular weight regulator is a dicarboxylic acid including adipic acid, sebacic acid, and dodecanoic acid.

5. The method for preparing nylon 10 from 10-aminodecanoic acid according to claim 1, characterized in that, In step (1), the catalyst is a phosphorus-based compound, and one or more of phosphoric acid, phosphorous acid, sodium phosphite, sodium hypophosphite and pyrophosphite are used.

6. The method for preparing nylon 10 from 10-aminodecanoic acid according to claim 1, characterized in that, In step (1), the antioxidant is one or more of antioxidants 1010, 1070, 1076, 1098, 2246, 245 and 330.

7. The method for preparing nylon 10 from 10-aminodecanoic acid according to claim 1, characterized in that, In step (1), the antioxidant is one or more of antioxidants 1098, 2246 and 330, and the amount added is 0.04-0.1 parts by mass.

Citation Information

Patent Citations

  • A process for preparing nylon 11 by atmospheric pressure melt polymerization of 11-aminoundecanoic acid

    CN103709399B

  • Process method for preparing nylon12 by taking long-chain amino acid as monomer

    CN107312170A

  • Polyamide-10 having excellent mechanical and thermal characteristics and method for preparing same